Electrochemical device and electronic device including the same

By using the fluorophosphazene compound in the electrochemical device and the element A in the positive active material, the synergistic effect is solved, the problems of insufficient cycle performance and safety performance are solved, the stability of the negative and positive electrodes is improved, and the use of the electrochemical device is extended. life.

CN114122519BActive Publication Date: 2024-10-18DONGGUAN AMPEREX TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111397032.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-10-18
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing electrochemical devices have shortcomings in cycle performance and safety performance, especially stability and safety issues at high temperatures and long-term use.

Method used

By adding a fluorophosphazene compound to the electrolyte and the element A (such as Al, Mg, Zr or Ti) contained in the positive electrode active material, the mass percentage content ratio is adjusted to form a synergistic effect and improve the film formation stability on the negative electrode surface. and positive electrode structural stability, thereby improving the cycle performance and safety performance of electrochemical devices.

Benefits of technology

It effectively improves the cycle performance and safety performance of the electrochemical device, including the film formation stability on the negative electrode surface and the structural stability of the positive electrode piece, reducing thermal stability problems and extending the service life of the electrochemical device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003370687210000011
    Figure BDA0003370687210000011
  • Figure BDA0003370687210000021
    Figure BDA0003370687210000021
  • Figure BDA0003370687210000022
    Figure BDA0003370687210000022
Patent Text Reader

Abstract

The present application provides an electrochemical device and an electronic device, which include a positive electrode and an electrolyte, wherein the electrolyte includes a fluorinated phosphazene compound; the positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes an element A, wherein the element A is selected from at least one of Al, Mg, Zr or Ti. Based on the mass of the electrolyte, the mass percentage of the fluorinated phosphazene compound represented by the general formula (I) is W I Based on the mass of the positive electrode active material, the mass percentage of element A is W A ; W I With W A Satisfy the relationship: 0.01≤W I / W A ≤15, which can effectively improve the film formation stability on the negative electrode surface, stabilize the positive electrode structure and improve the thermal stability of the electrochemical device, thereby effectively improving the cycle performance and safety performance of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device comprising the electrochemical device. Background Art

[0002] Electrochemical devices, such as lithium-ion batteries, are widely used in wearable devices, smart phones, drones, laptops and other fields due to their advantages such as high operating voltage, high energy density, environmental friendliness, stable cycle and safety. With the development of modern information technology and the expansion of the application of electrochemical devices, the requirements for the cycle performance and safety performance of electrochemical devices are becoming increasingly higher. Summary of the invention

[0003] The purpose of this application is to provide an electrochemical device and an electronic device including the electrochemical device to improve the cycle performance and safety performance of the electrochemical device. The specific technical solution is as follows:

[0004] In a first aspect, the present application provides an electrochemical device, which comprises a positive electrode and an electrolyte; the electrolyte comprises a fluorophosphazene compound represented by general formula (I):

[0005]

[0006] wherein R1 is selected from C1 to C4 alkyl, C6 to C 12 Aromatic or C6 to C 12 wherein R2 and R3 are each independently selected from hydrogen, a halogen atom, a C1 to C4 alkyl group, a C1 to C4 alkoxy group, a C1 to C4 halogenated alkyl group or a C1 to C4 halogenated alkoxy group; the positive electrode comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer comprises a positive electrode active material, the positive electrode active material comprises an element A, and the element A comprises at least one of Al, Mg, Zr or Ti; based on the mass of the electrolyte, the mass percentage of the fluorophosphazene compound is W I Based on the mass of the positive electrode active material, wherein the mass percentage of the element A is W A ; said W I With the W A Satisfy the relationship: 0.01≤W I / W A ≤15. By adjusting the electrolyte to contain a fluorinated phosphazene compound and the positive electrode active material to contain element A, W I / W A The value of within the above range can effectively improve the film formation stability on the negative electrode surface, the structural stability of the positive electrode sheet, and the thermal stability of the electrochemical device, thereby effectively improving the cycle performance and safety performance of the electrochemical device.

[0007] In some embodiments of the first aspect of the present application, the fluorophosphazene compound includes at least one of the compounds of formula (I-1) to formula (I-3):

[0008]

[0009] In some embodiments of the first aspect of the present application, at least one of the following conditions is met: (a) the W I The range is: 0.01% ≤ W I ≤5%; (b) W A The range is: 0.001% ≤ W A ≤1%.

[0010] In some embodiments of the first aspect of the present application, based on the mass of the positive electrode active material, at least one of the following conditions (a) to (f) is satisfied: (a) the mass percentage of Al is W Al , 0.001%≤W Al ≤0.4%; (b) the mass percentage of Mg is W Mg , 0.001%≤W Mg ≤0.4%; (c) the mass percentage of Zr is W Zr , 0.001%≤W Zr ≤0.2%; (d) the mass percentage of Ti is W Ti , 0.001%≤W Ti ≤0.2%; (e) the mass percentage of the Al is greater than the mass percentage of the Mg; (f) the mass percentage of the Zr is greater than the mass percentage of the Ti.

[0011] In some embodiments of the first aspect of the present application, the W Al With the W I Satisfy the relationship: 1≤W I / W Al ≤50.

[0012] In some embodiments of the first aspect of the present application, the electrolyte further comprises a dinitrile compound represented by general formula (II):

[0013]

[0014] wherein R is selected from C1 to C 10 Alkylene, unsubstituted or fluorine-substituted C2 to C 10 unsubstituted or fluorinated C6 to C 10 arylene, unsubstituted or fluorine-substituted C6 to C 10Based on the mass of the electrolyte, the mass percentage of the dinitrile compound is W II , 0.5% ≤ W II ≤10%. By adjusting the mass percentage of the dinitrile compound within the above range, the cycle performance and safety performance of the electrochemical device can be effectively improved.

[0015] In some embodiments of the first aspect of the present application, the dinitrile compound includes at least one of adiponitrile, succinonitrile or 1,4-dicyano-2-butene.

[0016] In some embodiments of the first aspect of the present application, the W I With the W II Satisfy the relationship: 0.5≤W II / W I ≤12.

[0017] In some embodiments of the first aspect of the present application, the electrolyte further comprises a compound having a sulfur-oxygen double bond; based on the mass of the electrolyte, the mass percentage of the compound having a sulfur-oxygen double bond is W III , the W III The range is: 0.5% ≤ W III ≤5%. By adjusting the content of the sulfur-oxygen double bond compound within the above range, it is beneficial to improve the cycle performance of the electrochemical device.

[0018] In some embodiments of the first aspect of the present application, the compound having a sulfur-oxygen double bond includes at least one of vinyl sulfate, 1,3-propane sultone or 2,4-butane sultone.

[0019] In some embodiments of the first aspect of the present application, the W III With the W I Satisfy the relationship: 0.1≤W III / W I ≤10.

[0020] In some embodiments of the first aspect of the present application, the W III With the W Zr Satisfy the relationship: 5≤W III / W Zr ≤50.

[0021] A second aspect of the present application provides an electronic device, which includes the electrochemical device provided in the first aspect of the present application.

[0022] The present application arranges the fluorophosphazene compound in the electrolyte and the element A in the positive electrode active material so that the two produce a synergistic effect, which can not only effectively improve the film formation stability on the negative electrode surface, but also stabilize the positive electrode structure and improve the thermal stability of the electrochemical device, thereby effectively improving the cycle performance and safety performance of the electrochemical device.

[0023] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field based on the present application belong to the scope of protection of the present application.

[0025] It should be noted that in the invention content of this application, lithium-ion batteries are used as an example of electrochemical devices to explain this application, but the electrochemical devices of this application are not limited to lithium-ion batteries. Those skilled in the art should understand that the following description is only for illustrative purposes and does not limit the scope of protection of this application.

[0026] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0027] In a first aspect, the present application provides an electrochemical device comprising a positive electrode and an electrolyte;

[0028] The electrolyte includes a fluorophosphazene compound represented by the general formula (I):

[0029]

[0030] wherein R1 is selected from C1 to C4 alkyl, C6 to C 12 Aromatic or C6 to C 12 The positive electrode comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises element A, wherein the element A comprises at least one of Al, Mg, Zr or Ti. Based on the mass of the electrolyte, the mass percentage of the fluorophosphazene compound is W IBased on the mass of the positive electrode active material, wherein the mass percentage of the element A is W A , the W I With the W A Satisfy the relationship: 0.01≤W I / W A ≤15. For example, W I / W A The value of can be 0.01, 0.1, 1, 3, 5, 7, 9, 11, 13, 15, or any range therebetween.

[0031] Without being limited to any theory, the inventors of the present application have found through research that the fluorophosphazene compound can not only decompose and reduce at the negative electrode to form a good solid electrolyte interface (SEI) film, but also help to assist element A in stabilizing the positive electrode distortion. Further, element A can occupy the lithium position after the positive electrode is delithiated, stabilize the positive electrode structure, and alleviate the positive electrode structure distortion during the lithium ion battery cycle. After element A occupies the lithium position, the bond strength between element A and the oxygen element in the positive electrode is stronger than the bond strength between cobalt and the oxygen element in the positive electrode, which can alleviate the deoxygenation, prevent the dissolution of cobalt, and stabilize the positive electrode structure. By adjusting the electrolyte to contain the fluorophosphazene compound and the positive electrode active material to contain element A, W is controlled. I / W A The value of within the above range can effectively improve the film formation stability on the negative electrode surface, the structural stability of the positive electrode sheet, and the thermal stability of the electrochemical device, thereby effectively improving the cycle performance and safety performance of the electrochemical device.

[0032] In some embodiments of the present application, the fluorinated phosphazene compound includes at least one of the compounds of formula (I-1) to formula (I-3):

[0033]

[0034] In some embodiments of the present application, at least one of the following conditions is met:

[0035] (a) W I The range is: 0.01% ≤ W I ≤5%; for example, the W I The value of can be 0.01%, 0.1%, 1%, 2%, 3%, 4%, 5% or any range therebetween; it can suppress excessive impedance of the electrode interface and improve the cycle performance of the electrochemical device;

[0036] (b) W A The range is: 0.001% ≤ W A ≤1%. For example, the W AThe value of can be 0.001%, 0.01%, 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1% or any range therebetween; it can inhibit lattice distortion, stabilize the positive electrode structure, and improve the cycle performance of the electrochemical device.

[0037] In some embodiments of the present application, based on the mass of the positive electrode active material, at least one of the following conditions (a) to (f) is satisfied:

[0038] (a) The mass percentage of Al is W Al , the W Al The range is: 0.001% ≤ W Al ≤0.4%; for example, the W Al It can be 0.001%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4% or any range therebetween. Without being limited to any theory, the inventors of the present application have found that by adjusting the mass percentage of Al W Al Within the above range, the element Al occupies the lattice gap, and after the positive electrode is delithiated, the chemical bond formed by the element Al and the oxygen element is stronger than the chemical bond formed by the element Co and the oxygen element, thereby slowing down the deoxygenation, preventing the dissolution of the element Co, stabilizing the positive electrode structure, and improving the cycle performance of the electrochemical device;

[0039] (b) The mass percentage of Mg is W Mg , the W Mg The range is: 0.001% ≤ W Mg ≤0.4%; for example, the W Mg It can be 0.001%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4% or any range therebetween; not limited to any theory, the inventors of the present application have found that by adjusting the mass percentage content of Mg W Mg Within the above range, the element Mg occupies the lattice gap, and after the positive electrode is delithiated, the chemical bond formed by the element Mg and the oxygen element is stronger than the chemical bond formed by the element Co and the oxygen element, thereby slowing down the deoxygenation, preventing the dissolution of the element Co, stabilizing the positive electrode structure, and improving the cycle performance of the electrochemical device;

[0040] (c) The mass percentage of Zr is W Zr , the W Zr The range is: 0.001% ≤ W Zr ≤0.2%; for example, the W Zr It can be 0.001%, 0.01%, 0.02%, 0.04%, 0.08%, 0.12%, 0.16%, 0.2% or any range therebetween; not limited to any theory, the inventors of the present application have found that by adjusting the mass percentage content of Zr WZr Within the above range, the Zr element occupies the lattice gap, and after the positive electrode is delithiated, the chemical bond formed by the Zr element and the oxygen element is stronger than the chemical bond formed by the Co element and the oxygen element, thereby slowing down the deoxygenation, preventing the dissolution of the Co element, stabilizing the positive electrode structure, and improving the cycle performance of the electrochemical device;

[0041] (d) The mass percentage of Ti is W Ti , the W Ti The range is: 0.001% ≤ W Ti ≤0.2%; for example, the W Ti It can be 0.001%, 0.01%, 0.02%, 0.04%, 0.08%, 0.12%, 0.16%, 0.2% or any range therebetween; not limited to any theory, the inventors of the present application have found that by adjusting the mass percentage of Ti W Ti Within the above range, the Ti element occupies the lattice gap, and after the positive electrode is delithiated, the chemical bond formed by the element Ti and the oxygen element is stronger than the chemical bond formed by the element Co and the oxygen element, thereby slowing down the deoxygenation, preventing the dissolution of the element Co, stabilizing the positive electrode structure, and improving the cycle performance of the electrochemical device;

[0042] (e) the mass percentage of Al is greater than the mass percentage of Mg; without being limited to any theory, the inventors of the present application have found that by setting W Al >W Mg , which can make the positive electrode have better structural stability and improve the cycle performance of the electrochemical device;

[0043] (f) the mass percentage of Zr is greater than the mass percentage of Ti; without being limited to any theory, the inventors of the present application have found that by setting W Zr >W Ti , which can make the positive electrode have better structural stability and improve the cycle performance of the electrochemical device.

[0044] Without being limited to any theory, the inventors of the present application have found that the cycle performance of the electrochemical device can be further improved by controlling the electrochemical device to satisfy at least one of the above conditions.

[0045] In some embodiments of the present application, the W Al With the W I Satisfy the relationship: 1≤W I / W Al ≤50. For example, W I / W Al The value of can be 1, 10, 20, 30, 40, 50 or any range therebetween. Without being limited to any theory, the inventors of the present application have found that by regulating W I / W Al When the value of is within the above range, the element Al and the fluorophosphazene compound produce a synergistic effect, which can effectively improve the cycle performance and safety performance of the electrochemical device.

[0046] In some embodiments of the present application, the electrolyte further comprises a dinitrile compound represented by general formula (II):

[0047]

[0048] wherein R is selected from C1 to C 10 Alkylene, unsubstituted or fluorine-substituted C2 to C 10 unsubstituted or fluorinated C6 to C 10 arylene, unsubstituted or fluorine-substituted C6 to C 10 Based on the mass of the electrolyte, the mass percentage of the dinitrile compound is W II , 0.5% ≤ W II ≤10%. Without being limited to any theory, the inventors of the present application have found that by regulating the dinitrile compound within the above range, the easily oxidizable components in the electrolyte can be separated from the positive electrode surface, and when the electrochemical device is charged, the oxidation effect of the electrochemical device on the electrolyte is reduced, thereby effectively improving the cycle performance and safety performance of the electrochemical device.

[0049] In some embodiments of the present application, the dinitrile compound includes at least one of adiponitrile (AND), succinonitrile (SN) or 1,4-dicyano-2-butene (HEDN).

[0050] In some embodiments of the present application, the W I With the W II Satisfy the relationship: 0.5≤W II / W I ≤12. For example, the W II / W I The value of can be 0.5, 1, 2, 3, 4, 5, 6, 12 or any range therebetween. Without being limited to any theory, the inventors of the present application have found that when the mass percentage content of the dinitrile compound W II The mass percentage of fluorophosphazene compound W I When the ratio is too low, for example, less than 0.5, the cycle performance of the electrochemical device is not significantly improved; when the mass percentage of the dinitrile compound is W II The mass percentage of fluorophosphazene compound W I When the ratio is too high, for example, higher than 12, the effect of improving the cycle performance of the electrochemical device is weak; by adjusting the mass percentage content W of the dinitrile compound II The mass percentage of fluorophosphazene compound WI When the ratio is within the above range, the positive electrode structure is stabilized and the negative electrode interface is improved simultaneously, thereby effectively improving the cycle performance of the electrochemical device.

[0051] In some embodiments of the present application, the electrolyte further comprises a compound having a sulfur-oxygen double bond; based on the mass of the electrolyte, the mass percentage of the compound having a sulfur-oxygen double bond is W III , the W III The range is: 0.5% ≤ W III ≤5%. Without being limited to any theory, the inventors of the present application have found that when the content of the compound containing the sulfur-oxygen double bond is too low, for example, less than 0.5%, the cycle performance of the electrochemical device is not significantly improved; when the content of the compound containing the sulfur-oxygen double bond is too high, for example, higher than 5%, the impedance of the SEI film is too large, the polarization of the cycle process is large, and the cycle performance of the electrochemical device is deteriorated; by adjusting the mass percentage content W of the compound containing the sulfur-oxygen double bond III In the above range, the compound containing sulfur-oxygen double bonds can form a film at the positive electrode and the negative electrode, improve the stability of the SEI film, and help improve the cycle performance of the electrochemical device.

[0052] In some embodiments of the present application, the compound having a sulfur-oxygen double bond includes at least one of dithiothreitol sulfate (DTD), 1,3-propane sultone (PS) or 2,4-butane sultone.

[0053] In some embodiments of the present application, the W III With the W I Satisfy the relationship: 0.1≤W III / W I ≤10. For example, W III / W I The value of can be 0.1, 1, 3, 5, 7, 9, 10 or any range therebetween. Without being limited to any theory, the inventors of the present application have found that by regulating the mass percentage content W of the compound having a sulfur-oxygen double bond III The mass percentage of fluorophosphazene compound W I When the ratio is within the above range, the compound having a sulfur-oxygen double bond and the fluorophosphazene compound produce a synergistic effect, which is beneficial to further improve the cycle performance and safety performance of the electrochemical device.

[0054] In some embodiments of the present application, the W III With the W Zr Satisfy the relationship: 5≤W III / W Zr ≤50. For example, W III / W ZrThe value of can be 5, 10, 20, 30, 40, 50 or any range therebetween. Without being limited to any theory, the inventors of the present application have found that by regulating the mass percentage content W of the compound having a sulfur-oxygen double bond III The mass percentage of Zr Zr Within the above range, the compound having a sulfur-oxygen double bond and the element Zr produce a synergistic effect, which is beneficial to further improve the cycle performance and safety performance of the electrochemical device.

[0055] The electrolyte of the present application also includes lithium salts. The present application does not particularly limit the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiB(C2O4)2, LiBOB), lithium difluorooxalatoborate (LiBF2(C2O4), LiDFOB), lithium hexafluoroantimonate (LiSbF6), lithium hexafluoroarsenate (LiAsF6), lithium perfluorobutylsulfonate (LiC4F9SO3), lithium perchlorate (LiClO4), lithium aluminate (LiAlO2), lithium tetrachloroaluminate (LiAlCl4), lithium bis(C2O4)2 (LiB(C2O4)2, LiBOB), lithium di(C2O4)2 (LiDFOB), lithium hexafluoroantimonate (LiSbF6), lithium hexafluoroarsenate (LiAsF6), lithium perfluorobutylsulfonate (LiC4F9SO3), lithium perchlorate (LiClO4), lithium aluminate (LiAlO2), lithium tetrachloroaluminate (LiAlCl4), lithium bis(C2O4)2 (LiB(C2O4)2, LiBOB), lithium bis(C2O4)2 (LiDFOB), lithium bis(C2O4)2 (LiB(C2O4)2, LiDFOB), lithium bis(C2O4)2 (LiSbF6), lithium bis(C2O4)2 (LiAsF6), lithium bis(C2O4)2 (LiDFOB), lithium bis(C2O4)2 (LiB(C2O4)2, LiDFOB), lithium bis(C2O4)2 (LiSbF6), lithium bis(C2O4)2 (LiDFOB), lithium bis(C2O4)2 (LiDFOB), lithium bis(C2O4)2 (LiDFOB), lithium bis(C2O x F 2x+1 SO2)(C y F 2y+1 SO2), wherein x and y are natural numbers), at least one of lithium chloride (LiCl) or lithium fluoride (LiF). The lithium salt of the present application may also include at least one of fluorine, boron or phosphorus. Preferably, the lithium salt may include LiPF6, because LiPF6 can give high ionic conductivity and improve the cycle performance of lithium ion batteries.

[0056] The electrolyte of the present application also includes a non-aqueous solvent. The present application has no particular restrictions on the non-aqueous solvent, as long as the purpose of the present application can be achieved. For example, the non-aqueous solvent may include at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compound may be a chain carbonate compound. Examples of the above-mentioned chain carbonate compounds are at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or ethyl methyl carbonate (EMC). Examples of the above-mentioned carboxylate compounds are at least one of ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate or propyl propionate. Examples of the above-mentioned ether compounds are at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. Examples of the above-mentioned other organic solvents are at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate or phosphoric acid ester. The content of the non-aqueous solvent is not particularly limited as long as the purpose of the present application can be achieved.

[0057] In the present application, the electrolyte may further include other additives. There is no particular limitation on other additives in the present application as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of lithium tetrafluoroborate (LiBF4), vinylene carbonate (VC) or lithium dioxalate borate (LiBOB).

[0058] The present application has no particular restrictions on the positive electrode current collector, which can be any positive electrode current collector known in the art, such as copper foil, aluminum foil, aluminum alloy foil, and composite current collector, etc. The present application has no particular restrictions on the positive electrode active material, which can be any positive electrode active material in the prior art, for example, it can include at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, or lithium iron manganese phosphate.

[0059] In the present application, the thickness of the positive electrode current collector and the positive electrode active material layer is not particularly limited as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 8 μm to 12 μm, and the thickness of the positive electrode active material layer is 30 μm to 120 μm.

[0060] In the present application, the positive electrode active material layer may also include a conductive agent. The present application has no particular restrictions on the conductive agent, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of conductive carbon black, carbon nanotubes, carbon fibers, flake graphite, Ketjen black, graphene, metal materials or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers. Specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole.

[0061] In the present application, the positive electrode active material layer may also include a binder. There is no particular limitation on the binder as long as the purpose of the present application can be achieved. For example, it may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin, nylon, etc.

[0062] Optionally, the positive electrode may further include a conductive layer, which is located between the positive electrode current collector and the positive electrode active material layer. The present application has no particular limitation on the composition of the conductive layer, which may be a commonly used conductive layer in the art, for example, including but not limited to the above conductive agent and the above binder.

[0063] There is no special restriction on the negative electrode sheet in the present application, as long as the purpose of the present application can be achieved. For example, the negative electrode sheet usually includes a negative electrode current collector and a negative electrode active material layer. In the present application, the negative electrode active material layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector, or it can be a partial area of ​​the negative electrode current collector. There is no special restriction in the present application, as long as the purpose of the present application can be achieved.

[0064] In the present application, the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode active material is not particularly limited, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithiated TiO2-Li4Ti5O 12 Or at least one of Li-Al alloy.

[0065] There is no particular restriction on the negative electrode current collector in the present application, as long as the purpose of the present application can be achieved, and materials such as metal foil or porous metal plate can be used, such as foil or porous plate of metals such as copper, nickel, titanium or iron or their alloys, such as copper foil. In the present application, there is no particular restriction on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness is 4μm to 12μm.

[0066] In the present application, the negative electrode active material layer may further include a conductive agent, and the present application has no particular limitation on the conductive agent, as long as the purpose of the present application can be achieved.

[0067] In the present application, the negative electrode active material layer may also include a binder. The present application has no particular limitation on the binder as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of styrene-butadiene rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl butyral, aqueous acrylic resin or carboxymethyl cellulose.

[0068] In the present application, the negative electrode active material layer may further include a thickener. The present application has no particular limitation on the thickener, as long as the purpose of the present application can be achieved. For example, the thickener may be sodium carboxymethyl cellulose.

[0069] Optionally, the negative electrode may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode active material layer. The present application has no particular limitation on the composition of the conductive layer, which may be a conductive layer commonly used in the art.

[0070] There is no particular limitation on the isolation membrane in the present application, as long as the purpose of the present application can be achieved. The isolation membrane may include a substrate layer and a surface treatment layer. The present application has no particular limitation on the substrate layer, for example, it may include but is not limited to polyethylene (PE), polypropylene (PP), polytetrafluoroethylene-based polyolefin (PO)-based diaphragms, polyester films (such as polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex, aramid films, woven films, non-woven films (non-woven fabrics), microporous films, composite films, diaphragm paper, rolled films or spinning films. At least one of them is preferably PP. The isolation membrane of the present application may have a porous structure, and the size of the pore size is not particularly limited, as long as the purpose of the present application can be achieved. For example, the size of the pore size can be 0.01μm to 1μm. In the present application, the thickness of the isolation membrane is not particularly limited, as long as the purpose of the present application can be achieved. For example, the thickness can be 5μm to 500μm.

[0071] In the present application, a surface treatment layer may also be provided on at least one surface of the substrate layer. The present application has no particular restrictions on the surface treatment layer, which may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer may include, but is not limited to, inorganic particles and an inorganic layer binder. The present application has no particular restrictions on inorganic particles, for example, may include but is not limited to at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on the inorganic layer binder, for example, may include but is not limited to at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The polymer layer contains polymers, and the polymer material may include but is not limited to at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene).

[0072] The electrochemical device of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In some embodiments, the electrochemical device may include, but is not limited to, a lithium-ion battery.

[0073] The preparation process of the electrochemical device is well known to those skilled in the art, and the present application has no particular limitation. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a wound structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device; or stacking the positive electrode, the separator and the negative electrode in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0074] The second aspect of the present application provides an electronic device, comprising the electrochemical device in any of the aforementioned embodiments of the present application. The electrochemical device provided by the present application has good cycle performance and safety performance, so that the electronic device provided by the present application has a long service life and good performance.

[0075] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. For example, the display device includes but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0076] Test methods and equipment:

[0077] High temperature cycle test:

[0078] The battery was placed in a 45°C constant temperature box, charged to 4.4V at a constant current of 1.5C, charged to 0.05C at a constant voltage of 4.4V, and then discharged to 3.0V at a constant current of 1.0C. This was a charge and discharge cycle. The charge and discharge test was performed 500 times in the above manner to monitor the capacity retention rate. The 45°C cycle capacity retention rate = (discharge capacity of the 500th cycle / initial discharge capacity) × 100%.

[0079] Safety Testing:

[0080] The battery was charged to 4.4V at a constant current of 0.5C at 25°C, and then charged to 0.05C at a constant voltage of 4.4V and then rested for 60 minutes (min). The battery was transferred to a high and low temperature box for testing. The high and low temperature box was heated to 130°C at a constant rate of 3°C / min and maintained for 60 minutes. The pass rate of the battery during the test was recorded (the pass standard was that the battery did not catch fire, burn, or explode). To ensure the reliability of the test, at least 5 batteries were used for parallel testing.

[0081] Element A content test:

[0082] (1) The lithium-ion battery is disassembled after being discharged, and the positive electrode active material in the positive electrode active material layer is taken for inductively coupled plasma emission spectroscopy (ICP) testing.

[0083] (2) The lithium-ion battery is disassembled after being discharged, and the positive electrode active material in the positive electrode active material layer is taken for surface X-ray energy dispersive spectroscopy (EDS) test.

[0084] The content value of element A is the larger value between the content value of element A obtained by ICP test and the content value of element A obtained by EDS test.

[0085] Test of component content in electrolyte:

[0086] The lithium-ion battery is discharged and centrifuged, and the liquid obtained after centrifugation is subjected to GC-MS testing; the percentage of each component (EC, PC, DEC, additives) is detected.

[0087] Example 1

[0088] (1) Preparation of negative electrode sheet: Mix the negative electrode active materials artificial graphite, styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) in a mass ratio of 97.4:1.2:1.4, then add deionized water as a solvent, prepare a slurry with a solid content of 70wt%, and stir evenly. The slurry is evenly coated on one surface of a copper foil with a thickness of 8μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a negative electrode active material layer coated on one side with a thickness of 150μm, and a negative electrode sheet with a negative electrode active material layer coated on one side is obtained. Cut the negative electrode sheet into a specification of (74mm×867mm) and weld the tabs for standby use.

[0089] (2) Preparation of electrolyte: In an argon atmosphere glove box with a water content of <10 ppm, organic solvents ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) were mixed uniformly at a mass ratio of 1:1:3, and fully dried lithium salt LiPF6 was dissolved in the above non-aqueous solvent to obtain an electrolyte, wherein the mass percentage of lithium salt LiPF6 was 12.5%. Add an additive fluorophosphazene compound to the electrolyte in an amount of 0.01% by mass.

[0090] (3) Preparation of positive electrode sheet: The positive electrode active material, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) is added as a solvent. The system is stirred under the action of a vacuum mixer until the system becomes a uniform positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on one side of a positive electrode current collector aluminum foil with a thickness of 12μm, dried at 85°C, and cold pressed to obtain a positive electrode sheet with a positive electrode active material layer thickness of 100μm, and a positive electrode sheet with a positive electrode active material layer coated on one side is obtained. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use. Among them, the positive electrode active material includes lithium cobalt oxide, elemental Mg and elemental Ti, wherein, based on the mass of the positive electrode active material, the mass percentage of Mg is 0.3%, the mass percentage of Ti is 0.2%, and the balance is lithium cobalt oxide.

[0091] (4) Isolation membrane: PE porous polymer film is used as the isolation membrane.

[0092] (5) Preparation of lithium-ion batteries: stack the positive electrode sheet, separator, and negative electrode sheet in order, with the separator placed between the positive and negative electrodes to serve as an isolation, and then wind them to obtain a bare cell; place the bare cell in an outer packaging foil, inject the prepared electrolyte into the dried cell, and complete the preparation of the lithium-ion battery after vacuum packaging, standing, forming, shaping, and other processes.

[0093] Example 2 to Example 32

[0094] Except for changing the relevant parameters as shown in Table 1, the rest is the same as Example 1.

[0095] Example 33 to Example 36

[0096] In addition to adjusting the content of element Al, the content of the fluorophosphazene compound, and the ratio of the mass percentage of the fluorophosphazene compound to the mass percentage of Al as shown in Table 2, I / W Al Other than that, the rest is the same as Example 3.

[0097] Example 37 to Example 45

[0098] The dinitrile compound is then added to the electrolyte, and the content of the dinitrile compound, the content of the fluorophosphazene compound and the mass percentage of the dinitrile compound are adjusted as shown in Table 3. II The mass percentage of fluorophosphazene compound W I The ratio W II / W I Other than that, the rest is the same as Example 3.

[0099] Example 46 to Example 54

[0100] A compound having a sulfur-oxygen double bond is further added to the electrolyte, and the content of the compound having a sulfur-oxygen double bond, the content of the fluorophosphazene compound and the mass percentage of the compound having a sulfur-oxygen double bond are adjusted as shown in Table 4. III The mass percentage of fluorophosphazene compound W I The ratio W III / W I Other than that, the rest is the same as Example 3.

[0101] Example 55 to Example 63

[0102] In addition to adjusting the content of element Zr, the content of the compound having a sulfur-oxygen double bond, and the mass percentage content ratio of the compound having a sulfur-oxygen double bond to the mass percentage content of Zr as shown in Table 5, III / W Zr , the rest is the same as Example 22.

[0103] Comparative Examples 1 to 4

[0104] Except for changing the relevant parameters as shown in Table 1, the rest is the same as Example 1.

[0105] Table 1

[0106]

[0107]

[0108] In Table 1, “ / ” indicates that there is no corresponding preparation parameter.

[0109] Table 2

[0110]

[0111]

[0112] Table 3

[0113]

[0114] Table 4

[0115]

[0116] Table 5

[0117]

[0118]

[0119] It can be seen from Examples 1 to 7, Examples 14 to 22 and Comparative Example 4 that W I / W A When the value of W is within the range of this application, the cycle performance and safety performance are better. I / W A When W is too small, the cycle performance is affected. I / W A When it is too high, the cycle performance is affected.

[0120] It can be seen from Examples 1 to 22, Comparative Examples 1 and 3 that, compared with those without fluorinated phosphazene compounds, the cycle performance and safety performance are better after adding fluorinated phosphazene compounds. When the content of fluorinated phosphazene compounds is high, the cycle performance is affected.

[0121] It can be seen from Examples 14 to 32, Comparative Examples 1 and 2 that after the addition of element A, the cycle performance and safety performance of the electrochemical device are better.

[0122] It can be seen from Example 15, Example 3 to Example 7 and Example 33 to Example 36 that when W I / W Al When the value of W is within the range of this application, the cycle performance and safety performance are better. I / W Al If W is too small, the cycle performance and safety performance will be affected. I / W Al When it is too high, the cycle performance and safety performance will be affected.

[0123] It can be seen from Example 3 and Example 37 to Example 45 that, compared with the case where no dinitrile compound is present, the cycle performance and safety performance are better after the dinitrile compound is added.

[0124] It can be seen from Examples 37 to 45 that when W II / W I When the value of W is within the range of this application, the cycle performance and safety performance are better. II / W I If the W is too small, the cycle performance and safety performance will be affected. II / W I When it is too high, the cycle performance is affected.

[0125] It can be seen from Examples 46 to 54 that after the addition of the compound having a sulfur-oxygen double bond, the cycle performance and safety performance of the electrochemical device are improved; when W III / W I When the value of W is within the range of this application, the cycle performance and safety performance are better. III / W I When the value of W is too low, the cycle performance and safety performance are affected. III / W I When the value is too high, the cycle performance and safety performance are affected.

[0126] It can be seen from Examples 55 to 63 that when W III / W Zr When the value of W is within the range of this application, the cycle performance and safety performance are better. II / W I If the W is too small, the cycle performance and safety performance will be affected. II / W I When it is too high, the cycle performance and safety performance will be affected.

[0127] The above description is only a preferred embodiment of the present application and is not intended to limit the protection scope of the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application are included in the protection scope of the present application.

Claims

1. An electrochemical device comprising a positive electrode and an electrolyte; The electrolyte includes a fluorophosphazene compound represented by the general formula (I): in, R1 is selected from C1 to C4 alkyl, C6 to C 12 Aromatic or C6 to C 12 R2 and R3 are each independently selected from hydrogen, a halogen atom, a C1 to C4 alkyl group, a C1 to C4 alkoxy group, a C1 to C4 haloalkyl group or a C1 to C4 haloalkoxy group; The positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, the positive electrode active material includes element A, and the element A includes at least one of Al, Mg, Zr or Ti; Based on the mass of the electrolyte, the mass percentage of the fluorophosphazene compound is W I ; Based on the mass of the positive electrode active material, the mass percentage of the element A is W A , 0.001%≤W A ≤1%; The W I With the W A Satisfy the relationship: 0.1≤W I / W A ≤15.

2. The electrochemical device according to claim 1, wherein: The fluorinated phosphazene compound includes at least one of the compounds of formula (I-1) to formula (I-3):

3. The electrochemical device according to claim 1, wherein The W I The range is: 0.01% ≤ W I ≤5%.

4. The electrochemical device according to claim 1, wherein Based on the mass of the positive electrode active material, at least one of the following conditions (a) to (f) is satisfied: (a) The mass percentage of Al is W Al , 0.001%≤W Al ≤0.4%; (b) The mass percentage of Mg is W Mg , 0.001%≤W Mg ≤0.4%; (c) The mass percentage of Zr is W Zr , 0.001%≤W Zr ≤0.2%; (d) The mass percentage of Ti is W Ti , 0.001%≤W Ti ≤0.2%; (e) the mass percentage of the Al is greater than the mass percentage of the Mg; (f) The mass percentage of the Zr is greater than the mass percentage of the Ti.

5. The electrochemical device according to claim 1, wherein Based on the mass of the positive electrode active material, the mass percentage of Al is W Al , the W Al With the W I Satisfy the relationship: 1≤W I / W Al ≤50.

6. The electrochemical device according to claim 1, wherein The electrolyte further comprises a dinitrile compound represented by general formula (II): wherein R is selected from C1 to C 10 Alkylene, unsubstituted or fluorine-substituted C2 to C 10 unsubstituted or fluorinated C6 to C 10 arylene, unsubstituted or fluorine-substituted C6 to C 10 alicyclic groups; Based on the mass of the electrolyte, the mass percentage of the dinitrile compound is W II , 0.5% ≤ W II ≤10%.

7. The electrochemical device according to claim 6, wherein: The dinitrile compound includes at least one of adiponitrile, succinonitrile or 1,4-dicyano-2-butene.

8. The electrochemical device according to claim 6, wherein: The W I With the W II Satisfy the relationship: 0.5≤W II / W I ≤12.

9. The electrochemical device according to claim 4, wherein: The electrolyte further comprises a compound having a sulfur-oxygen double bond; Based on the mass of the electrolyte, the mass percentage of the compound having a sulfur-oxygen double bond is W III , the W III The range is: 0.5% ≤ W III ≤5%.

10. The electrochemical device according to claim 9, wherein: The compound having a sulfur-oxygen double bond includes at least one of vinyl sulfate, 1,3-propane sultone or 2,4-butane sultone.

11. The electrochemical device according to claim 9, wherein The W III With the W I Satisfy the relationship: 0.1≤W III / W I ≤10.

12. The electrochemical device according to claim 9, wherein: Based on the mass of the positive electrode active material, the mass percentage of Zr is W Zr , the W III With the W Zr Satisfy the relationship: 5≤W III / W Zr ≤50.

13. An electronic device comprising the electrochemical device according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Battery

    CN109428078A

  • Non-aqueous electrolyte secondary battery

    JP2020021631A

  • Lithium ion secondary battery

    US20090081548A1