A method for compensating the deviation of rolling center line of hot-rolled medium and thick plates

By measuring and calculating the centerline offset of the steel plate, combined with rolling force and stiffness, and adjusting the roll gap value in real time, the accuracy problem of centerline offset compensation during the rolling process of medium and thick plates is solved, and production stability and product quality are improved. .

CN114160586BActive Publication Date: 2024-10-08MINGJIAN (LIAONING) HIGH-TECH IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111459001.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-02
Publication Date
2024-10-08
Estimated Expiration
2041-12-02

AI Technical Summary

Technical Problem

The existing technology cannot effectively apply high-precision compensation for the centerline offset of the steel plate during the rolling process of medium and thick plates online, resulting in sickle bend defects and production stability problems.

Method used

By measuring the centerline offset of the slab after the first pass of rolling, the comprehensive centerline offset is calculated, and combined with the rolling force and stiffness, the bounce value and roll gap leveling compensation amount on both sides of the rolling mill are calculated in real time. Adjust the roll gap value in the second pass of rolling to alleviate the centerline offset.

Benefits of technology

It improves the centerline offset compensation accuracy during the rolling process, reduces sickle bend defects, and improves production stability and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114160586B_ABST
    Figure CN114160586B_ABST
Patent Text Reader

Abstract

The present invention provides a method for compensating the centerline deviation of hot-rolled medium and thick plates, and belongs to the technical field of hot-rolled plate and strip steel production. The present invention obtains the deformation characteristics of the rolled piece and the equipment characteristics of the rolling mill to a certain extent through the measured centerline deviation of the slab after the first rolling. The calculation method fully considers the actual stiffness on both sides of the rolling mill, and improves the calculation accuracy of the bounce value; the calculation method is simple and practical, and it is relatively easy to embed into the control system, so as to achieve the purpose of alleviating the sickle bend defect of the steel plate and improving the rolling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hot-rolled plate and strip steel production, and in particular to a method for compensating for rolling centerline deviation of hot-rolled medium and thick plates. Background Art

[0002] Hot-rolled medium and thick plates are widely used in industrial fields such as construction engineering, container manufacturing, bridge construction and shipbuilding. They can also be used as the base material (intermediate billet) for hot-rolled thin plates.

[0003] In the production of hot-rolled medium and thick plates (intermediate billets), the quality of the steel plates and the load on the equipment are very large. In addition, the uneven temperature of the slabs makes it easy for the centerline of the steel plates to deviate during the rolling process. The deviation of the centerline of the steel plate will cause the inconsistency between the bounce value and the roll gap value on both sides of the rolling mill, which will cause defects such as sickle bending and side bending of the steel plate, seriously affecting the product dimensional accuracy and production stability. Using the asynchronous action of the hydraulic cylinders on both sides of the rolling mill to level the roll gap can effectively alleviate the side bending defects caused by the deviation of the centerline of the steel plate and improve product quality.

[0004] For example, Chinese patent 202110718963.5 discloses "a method for centering the side guide of a medium and thick plate rolling mill", which increases the clamping deviation control on the middle and tail of the rolled piece to avoid the centerline deviation during the rolling process. It corrects the steel plate through the clamping device outside the rolling mill, and does not consider the influence of the temperature and dimensional deviation of the rolled piece itself on the centerline deviation. At the same time, as production progresses, the accuracy of the clamping device will inevitably decrease gradually, and the correction effect is difficult to guarantee.

[0005] Chinese patent 202110000908.2 discloses "a control method for sickle bending of medium and thick plates", which determines the bounce value deviation by the stiffness on both sides of the rolling mill, and then determines the roll gap leveling value. The compensation value of the centerline offset is determined by the bounce deviation value on both sides of the rolling mill. When there is a stiffness difference on both sides of the rolling mill due to equipment failure, it will greatly interfere with the calculation of the roll gap leveling value.

[0006] Chinese patent 201710588265.1 discloses "a method for eliminating the camber of medium and thick plate rolling by setting the roll swing tilt". This method determines the leveling direction of the mill by judging the camber value before and after rolling, so as to alleviate the camber. It is necessary to compare the size of the camber of the steel plate before and after rolling, and then determine the centerline offset compensation value of the next pass, which has serious hysteresis. Failure to adjust the roll gap in time may cause equipment damage and is not suitable for online application.

[0007] Chinese patent 201510654519.6 discloses a "Method and system for detecting sickle bend of medium and thick plate rolling mill". The sickle bend of steel plate is softly measured by judging the difference in rolling force on both sides of the rolling mill. The roll gap leveling value is calculated by judging the difference in rolling force on both sides of the rolling mill. The uniformity of the temperature and size of the rolled piece, the surface condition of the rolled piece and other factors will affect the rolling force on both sides, and the accuracy of the roll gap leveling value calculated from this may be low. At the same time, this patent only provides a measurement method, but does not provide improvement measures.

[0008] It can be seen that the technical solutions of the above patents are not suitable for the high-precision compensation method of the center line deviation of medium and thick plate rolling applied online. Summary of the invention

[0009] In view of this, the present invention provides a method for compensating the rolling centerline deviation of hot-rolled medium and thick plates, so as to alleviate the sickle bend defect of the steel plate and improve the rolling stability.

[0010] The method for compensating the rolling center line deviation of hot-rolled medium and thick plates of the present invention comprises the following steps:

[0011] (1) Use a width gauge to measure the centerline offset ΔB of the slab head after the first rolling pass H , Central centerline offset ΔB B and the tail centerline offset ΔB T ;

[0012] (2) Using the measured ΔB H , ΔB B and ΔB T , calculate the slab comprehensive centerline offset ΔB C for:

[0013] ΔB C =(ΔB H +ΔB T ) / 2-ΔB B

[0014] (3) The total rolling force P of the second pass is read in the control system. The rolling force deviation ΔP on both sides caused by the center line offset is:

[0015]

[0016] In the formula, B S is the slab width;

[0017] (4) According to the rolling force deviation ΔP and the total rolling force P, the rolling force P on the transmission side is calculated respectively. DS and the operating side rolling force P OS ,for:

[0018]

[0019] (5) According to the rolling force on both sides and the measured stiffness on both sides, calculate the bounce value on both sides of the rolling mill:

[0020]

[0021] In the formula, ΔS DS is the transmission side bounce value; ΔS OS is the operating side bounce value; M DS M is the transmission side stiffness; OS is the operating side stiffness;

[0022] (6) Calculate the roll gap leveling compensation value Δ S according to the bounce values ​​on both sides of the rolling mill calculated in step (5) T for:

[0023] ΔS T =ΔS DS -ΔS OS

[0024] (7) According to the roll gap leveling compensation amount calculated in step (6), the roll gap value on the operating side is adjusted in the second rolling pass to alleviate the sickle bend defect of the steel plate.

[0025] Preferably, the hot-rolled medium and thick plate rolling process is to use a hot-rolled medium and thick plate unit or a rough rolling unit of a finishing rolling line to roll the ingot into a steel plate with a thickness of 30 to 60 mm.

[0026] Preferably, the thickness of the ingot is 230-250 mm, and the width is 1500-2100 mm.

[0027] Preferably, the width gauge in step (1) is arranged at the first pass exit;

[0028] Preferably, in step (1), the center line of the slab is negative when it is biased toward the operating side, and is positive when it is biased toward the transmission side.

[0029] Preferably, the total rolling force P in step (3) is 15000 to 22000 kN.

[0030] Preferably, when the roll gap leveling compensation amount in step (7) is a negative value, the roll gap value on the operating side is reduced during the second rolling pass; when the roll gap leveling compensation amount is a positive value, the roll gap value on the operating side is increased during the second rolling pass.

[0031] Compared with the prior art, the present invention has the following beneficial effects: the present invention obtains the deformation characteristics of the rolled piece and the equipment characteristics of the rolling mill to a certain extent through the measured centerline offset of the slab after the first rolling pass; the calculation method fully considers the actual stiffness on both sides of the rolling mill, and improves the calculation accuracy of the bounce value; the calculation method is simple and practical, and is relatively easy to embed into the control system; the roll gap leveling value calculated by the present invention can better compensate for the centerline offset of the steel plate during the rolling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It represents the process flow chart of medium and thick plate production. DETAILED DESCRIPTION

[0033] The present invention provides a method for compensating for the rolling centerline deviation of hot-rolled medium and thick plates. In the embodiments, the hot-rolled medium and thick plates are prepared by a hot-rolled medium and thick plate unit or a rough rolling unit of a finishing rolling line. The equipment parameters of the hot-rolled medium and thick plate unit or the rough rolling unit of a finishing rolling line are shown in Table 1.

[0034] Table 1

[0035]

[0036] The present invention will be further described below in conjunction with the embodiments.

[0037] Example 1

[0038] Prepare a slab with a thickness of 250mm and a width of 1600mm, and roll it into a Q235 carbon structural steel plate with a thickness of 30mm through a hot rolling medium and thick plate unit. The calculation process of the roll gap leveling amount used to compensate for the deviation of the center line of the steel plate is as follows:

[0039] (1) The centerline deviation of the slab after the first rolling pass is measured by a width gauge and is ΔB H =-20mm, ΔB B =0mm, ΔB T =-40mm;

[0040] (2) Based on the measured ΔB H , ΔB B and ΔB T , calculate the slab comprehensive centerline offset ΔB C for:

[0041] ΔB C =((-20)+(-40)) / 2-0=-30mm

[0042] (3) The rolling force setting value of the second pass is read in the control system as P = 19500 kN. The rolling force deviation ΔP on both sides caused by the center line offset is:

[0043]

[0044] (4) According to the rolling force deviation ΔP and the total rolling force P, the rolling force P on the transmission side is calculated respectively. DS and the operating side rolling force P OS ,for:

[0045]

[0046] (5) The stiffness of the operating side and the transmission side are 5400 kN / mm and 5800 kN / mm respectively. According to the rolling force on both sides and the measured stiffness on both sides, the bounce value on both sides of the rolling mill is calculated:

[0047]

[0048] (6) Calculate the roll gap leveling compensation ΔS based on the bounce values ​​on both sides of the rolling mill calculated in step (5) T for:

[0049] ΔS T =1.617-1.873=-0.256mm

[0050] (7) In the second rolling pass, the roll gap on the operating side is reduced by 0.256 mm. After measurement, after applying the compensation method of the present invention, the comprehensive centerline offset of the steel plate in Example 1 is reduced from -30 mm to -12 mm.

[0051] Example 2

[0052] Prepare a slab with a thickness of 250mm and a width of 2100mm, and roll it into a steel plate with a thickness of 40mm through a hot rolling medium and thick plate unit. The calculation process of the roll gap leveling amount used to compensate for the deviation of the center line of the steel plate is as follows:

[0053] (1) Use a width gauge to measure the centerline deviation ΔB of the slab after the first rolling pass H , ΔB B and ΔB T They are 30mm, -10mm and 50mm respectively;

[0054] (2) Based on the measured ΔB H , ΔB B and ΔB T , calculate the slab comprehensive centerline offset ΔB C for:

[0055] ΔB C =(30+50) / 2-(-10)=50mm

[0056] (3) Read the rolling force setting value of the second pass P = 21300 kN in the control system, then the rolling force deviation ΔP on both sides caused by the center line offset is:

[0057]

[0058] (4) According to the rolling force deviation ΔP and the total rolling force P, the rolling force P on the transmission side is calculated respectively. DS and the operating side rolling force P OS ,for:

[0059]

[0060] (5) The stiffness of the operating side and the transmission side are 5500 kN / mm and 5600 kN / mm respectively. According to the rolling force on both sides and the measured stiffness on both sides, the bounce value on both sides of the rolling mill is calculated:

[0061]

[0062] (6) Calculate the roll gap leveling compensation ΔS based on the bounce values ​​on both sides of the rolling mill calculated in step (5) T for:

[0063] ΔS T =1.992-1.844=0.148mm

[0064] (7) In the second rolling, the operating side roll gap increases by 0.148 mm. After measurement, after applying the compensation method of this patent, the comprehensive centerline offset of the steel plate in Example 2 is reduced from 50 mm to 21 mm.

[0065] Example 3

[0066] Prepare a slab with a thickness of 230 mm and a width of 1500 mm, and roll it into a 700L automobile beam steel intermediate slab with a thickness of 45 mm through a rough rolling mill. The calculation process of the roll gap leveling amount used to compensate for the deviation of the center line of the steel plate is as follows:

[0067] (1) Use a width gauge to measure the centerline deviation ΔB of the slab after the first rolling pass H , ΔB B and ΔB T They are -15mm, 5mm and -20mm respectively;

[0068] (2) Based on the measured ΔB H , ΔB B and ΔB T , calculate the slab comprehensive centerline offset ΔB C for:

[0069] ΔB C=((-15)+(-20)) / 2-5=-22.5mm

[0070] (3) The rolling force setting value of the second pass is read in the control system, P = 15750 kN. The rolling force deviation ΔP on both sides caused by the center line offset is:

[0071]

[0072] (4) According to the rolling force deviation ΔP and the total rolling force P, the rolling force P on the transmission side is calculated respectively. DS and the operating side rolling force P OS ,for:

[0073]

[0074] (5) The stiffness of the operating side and the transmission side are 4600 kN / mm and 4800 kN / mm respectively. According to the rolling force on both sides and the measured stiffness on both sides, the bounce value on both sides of the rolling mill is calculated:

[0075]

[0076] (6) Calculate the roll gap leveling compensation ΔS based on the bounce values ​​on both sides of the rolling mill calculated in step (5) T for:

[0077] ΔS T =1.591-1.763=-0.172mm

[0078] (7) In the second rolling, the operating side roll gap is reduced by 0.172 mm. After measurement, after applying the compensation method of this patent, the comprehensive centerline offset of the steel plate in Example 3 is reduced from -22.5 mm to -8.5 mm.

[0079] Example 4

[0080] Prepare a slab with a thickness of 230 mm and a width of 1800 mm, and roll it into a Q355PL wheel steel intermediate slab with a thickness of 57.5 mm through a rough rolling mill. The calculation process of the roll gap leveling amount used to compensate for the deviation of the center line of the steel plate is as follows:

[0081] (1) Use a width gauge to measure the centerline deviation ΔB of the slab after the first rolling pass H , ΔB B and ΔB T They are 55mm, -15mm and 35mm respectively;

[0082] (2) Based on the measured ΔB H , ΔB B and ΔB T , calculate the slab comprehensive centerline offset ΔBC for:

[0083] ΔB C =(55+35) / 2-(-15)=60mm

[0084] (3) The rolling force setting value of the second pass is read in the control system as P = 18500 kN. The rolling force deviation ΔP on both sides caused by the center line offset is:

[0085]

[0086] (4) According to the rolling force deviation ΔP and the total rolling force P, the rolling force P on the transmission side is calculated respectively. DS and the operating side rolling force P OS ,for:

[0087]

[0088] (5) The stiffness of the operating side and the transmission side are 4650 kN / mm and 4750 kN / mm respectively. According to the rolling force on both sides and the measured stiffness on both sides, the bounce value on both sides of the rolling mill is calculated:

[0089]

[0090] (6) Calculate the roll gap leveling compensation ΔS based on the bounce values ​​on both sides of the rolling mill calculated in step (5) T for:

[0091] ΔS T =2.077-1.857=0.22mm

[0092] (7) In the second rolling, the operating side roll gap increases by 0.22 mm. After measurement, after applying the compensation method of this patent, the comprehensive centerline offset of the steel plate in Example 4 is reduced from 60 mm to 25 mm.

[0093] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for compensating for the deviation of the rolling center line of hot-rolled medium and thick plates, characterized in that: The following steps are involved: (1) Use a width gauge to measure the centerline offset Δ of the slab head after the first rolling pass. B H , Central centerline offset Δ B B and the tail centerline offset Δ B T ; (2) Using the measured Δ B H , Δ B B and Δ B T , calculate the slab comprehensive centerline offset Δ B C for: ; (3) Read the total rolling force of the second pass in the control system P , then the rolling force deviation on both sides caused by the center line offset Δ P for: ; In the formula, B S is the slab width; (4) According to the rolling force deviation Δ P and total rolling force P , calculate the rolling force on the transmission side P DS and rolling force on the operating side P OS ,for: ; (5) According to the rolling force on both sides and the measured stiffness on both sides, calculate the bounce value on both sides of the rolling mill: ; In the formula, Δ S DS is the transmission side bounce value; Δ S OS is the operating side bounce value; M DS is the transmission side stiffness; M OS is the operating side stiffness; (6) According to the bounce values ​​on both sides of the rolling mill calculated in step (5), calculate the roll gap leveling compensation amount Δ S T for: ; (7) According to the roll gap leveling compensation amount calculated in step (6), the roll gap value on the operating side is adjusted in the second rolling pass to alleviate the sickle camber defect of the steel plate; The total rolling force P in step (3) is 15000-22000 kN; In step (1), the center line of the slab is negative when it is biased toward the operating side, and is positive when it is biased toward the transmission side; When the roll gap leveling compensation amount in step (7) is a negative value, the roll gap value on the operating side is reduced during the second rolling pass; when the roll gap leveling compensation amount is a positive value, the roll gap value on the operating side is increased during the second rolling pass.

2. The method for compensating the rolling centerline deviation of hot-rolled medium and thick plates according to claim 1, characterized in that: The hot-rolled medium and thick plate rolling process is to use a hot-rolled medium and thick plate unit or a rough rolling unit of a finishing rolling line to roll the ingot into a steel plate with a thickness of 30 to 60 mm.

3. The method for compensating the rolling centerline deviation of hot-rolled medium and thick plates according to claim 2, characterized in that: The thickness of the ingot is 230-250 mm, and the width is 1500-2100 mm.

4. The method for compensating the rolling centerline deviation of hot-rolled medium and thick plates according to claim 1, characterized in that: The width gauge in step (1) is arranged at the exit of the first pass.