Manufacturing method of FRP products
By precuring the anisotropic prepreg during the manufacturing process of FRP products and curing it with chopped fiber prepregs, the problem of strength reduction caused by the disordered fiber arrangement is solved, and the strength improvement of FRP products is achieved.
Patent Information
- Application Number
- CN202080057639.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-06
- Filing Date
- 2020-08-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-08-20
AI Technical Summary
During the manufacturing process of FRP products, the fiber arrangement is disordered in a specific direction, resulting in a problem of reduced strength. Especially when one-way prepreg, cross prepreg and chopped fiber prepreg are solidified in one piece, it is difficult to suppress the fiber arrangement chaos. Impacts the strength of the product.
By prefabricating the anisotropic prepreg in the prefabricating process and solidifying the chopped fiber prepreg in the prefabricating process, the anisotropic prepreg is first prefabricated before the compression molding process to reach more than 6%. The degree of curing is to suppress the confusion of fiber arrangement and to use appropriate heating and pressure conditions in the compression molding process to ensure the neat arrangement of the fibers.
It effectively suppresses the confusion of fiber arrangement, improves the strength of FRP products, and achieves the expected performance.
Smart Images

Figure BDA0003505113470000101 
Figure BDA0003505113470000131 
Figure BDA0003505113470000161
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a FRP product.
[0002] This application claims priority based on Japanese Patent Application No. 2019-151942 filed in Japan on August 22, 2019 and Japanese Patent Application No. 2020-039300 filed in Japan on March 6, 2020, and the contents of which are incorporated herein by reference. Background Art
[0003] FRP (fiber reinforced plastic) products are widely used, ranging from sporting goods and leisure products to components of transportation equipment and industrial equipment.
[0004] In the manufacture of FRP products, prepreg is often used as an intermediate material. Prepreg is a composite material formed by fibers and a matrix resin composition. It includes materials such as unidirectional prepreg, cross prepreg, and tow prepreg in which fibers are arranged in a specific direction, and materials such as sheet molding compound (SMC) in which chopped fiber bundles are oriented in all directions within the plane.
[0005] It is known that for FPR products manufactured using prepregs in which fibers are arranged in a specific direction, if the fiber arrangement is disordered, the strength will be greatly reduced.
[0006] It is known that an FRP product having excellent strength can be produced by integrally curing a unidirectional prepreg or a cross prepreg with an SMC (for example, see Patent Document 1).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2018 / 101245 Summary of the invention
[0010] Problems to be solved by the invention
[0011] An object of the present invention is to provide a manufacturing method for suppressing the disorder of fiber arrangement in the portion formed by curing an anisotropic prepreg such as a unidirectional prepreg, a cross prepreg, or a tow prepreg in which fibers are arranged in a specific direction, and a chopped fiber prepreg such as a sheet molding compound, in an FRP product obtained by integrally curing the anisotropic prepreg such as a unidirectional prepreg, a cross prepreg, or a tow prepreg, thereby exhibiting the expected strength.
[0012] Solution to the problem
[0013] The embodiments of the present invention include the following aspects.
[0014] [1] A method for manufacturing a FRP product, the method comprising:
[0015] (i) a prefabrication process for prefabricating anisotropic prepreg; and
[0016] (ii) a compression molding step of curing the anisotropic prepreg prefabricated in the prefabrication step in a press mold together with the chopped fiber prepreg to obtain a molded product having a boundary between the aligned fiber reinforcement portion derived from the anisotropic prepreg and the chopped fiber reinforcement portion derived from the chopped fiber prepreg,
[0017] The anisotropic prepreg is pre-cured before the compression molding step, thereby suppressing the disorder of the fiber arrangement of the aligned fiber-reinforced portion of the molded product obtained in the compression molding step.
[0018] [2] The manufacturing method according to [1], wherein
[0019] When the degree of curing of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is 6% or more immediately before the compression molding step.
[0020] [3] A method for manufacturing a FRP product, the method comprising:
[0021] (i) a prefabrication process, prefabrication of anisotropic prepreg;
[0022] (ii) a compression molding step of curing the anisotropic prepreg prefabricated in the prefabrication step in a press mold together with the chopped fiber prepreg to obtain a molded product having a boundary between the aligned fiber reinforcement portion derived from the anisotropic prepreg and the chopped fiber reinforcement portion derived from the chopped fiber prepreg,
[0023] Here, when the degree of curing of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is 6% or more immediately before the compression molding step.
[0024] [4] The production method according to any one of [1] to [3], wherein
[0025] When the degree of curing of the anisotropic prepreg immediately before the compression molding step is set to 0%, the degree of curing of the anisotropic prepreg immediately before the compression molding step may be 18% or more, or 36% or more.
[0026] [5] The production method according to any one of [1] to [4], wherein
[0027] When the curing degree of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the curing degree of the anisotropic prepreg immediately before the compression molding step may be 94% or less, 60% or less, 50% or less, or 40% or less.
[0028] [6] The production method according to any one of [1] to [5], wherein
[0029] When the curing degree of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the curing degree of the anisotropic prepreg immediately before the compression molding step is 60% or less, or may be 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less.
[0030] [7] The production method according to any one of [1] to [6], wherein
[0031] The prefabrication step includes cutting the anisotropic prepreg.
[0032] [8] The production method according to any one of [1] to [7], wherein
[0033] The prefabrication process includes correcting the anisotropic prepreg.
[0034] [9] The production method according to any one of [1] to [8], wherein
[0035] The prefabrication step includes forming a preform having a three-dimensional shape from the anisotropic prepreg.
[0036]
[10] The manufacturing method according to [9], wherein
[0037] In the prefabrication step, the anisotropic prepreg is multi-wound on a shaping mold or a shaping jig.
[0038]
[11] The production method according to any one of [1] to
[10] , wherein
[0039] In the above-mentioned prefabrication step, the above-mentioned anisotropic prepreg is integrated with other anisotropic prepregs.
[0040]
[12] The production method according to any one of [1] to
[11] , wherein
[0041] In the prefabrication step, the anisotropic prepreg is at least partially pre-cured.
[0042]
[13] The manufacturing method according to
[12] , wherein:
[0043] When the degree of curing of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is at least 6% or more at the end of the prefabrication step.
[0044]
[14] The production method according to any one of [1] to
[13] , wherein
[0045] The anisotropic prepreg is a uniaxial prepreg.
[0046]
[15] The production method according to any one of [1] to
[13] , wherein
[0047] The anisotropic prepreg is a multiaxial prepreg.
[0048]
[16] The production method according to any one of [1] to
[15] , wherein
[0049] The anisotropic prepreg contains carbon fibers.
[0050]
[17] The production method according to any one of [1] to
[16] , wherein
[0051] The chopped fiber prepreg contains carbon fibers.
[0052]
[18] The production method according to any one of [1] to
[17] , wherein
[0053] The anisotropic prepreg contains an epoxy resin.
[0054]
[19] The production method according to any one of [1] to
[18] , wherein
[0055] The chopped strand prepreg contains at least one selected from vinyl ester resins and unsaturated polyester resins.
[0056]
[20] The production method according to any one of [1] to
[18] , wherein
[0057] The chopped fiber prepreg contains epoxy resin.
[0058]
[21] The production method according to any one of [1] to
[20] , wherein
[0059] The above-mentioned chopped fiber prepreg is a sheet molding compound.
[0060]
[22] The production method according to any one of [1] to
[21] , wherein
[0061] The aligned fiber reinforcement portion is arranged on a portion of the surface of the molded article such that fibers included in the aligned fiber reinforcement portion are parallel to the surface of the molded article obtained in the compression molding step.
[0062]
[23] The production method according to any one of [1] to
[22] , wherein
[0063] The molded product obtained in the compression molding step has ridges on the surface, and the neatly arranged fiber reinforcement portion in which fibers are oriented in one direction is arranged along all or part of the ridges in such a manner that the direction of the fibers in the neatly arranged fiber reinforcement portion in which fibers are oriented in one direction is parallel to the ridges.
[0064] Effects of the Invention
[0065] According to the present invention, a manufacturing method can be provided, which is used to suppress the disorder of fiber arrangement in the part formed by curing an anisotropic prepreg such as a unidirectional prepreg, a cross prepreg, and a tow prepreg in which fibers are arranged in a specific direction, and a short-cut fiber prepreg such as a sheet molding compound in an FRP product obtained by integrally curing the anisotropic prepreg such as a unidirectional prepreg, a cross prepreg, and a tow prepreg, thereby exhibiting the expected strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 This is a perspective view illustrating the structure of a shaping jig that can be used in the prefabrication process.
[0067] Figure 2 The prepreg tape (or tow prepreg) is wound on Figure 1 A three-dimensional view of the surrounding area of the three support rods of the shaping fixture shown.
[0068] Figure 3 is an example of using Figure 1 A three-dimensional view of a preform that can be formed using the shaping fixture shown.
[0069] Figure 4 It is a cross-sectional view illustrating the step of integrally curing the anisotropic prepreg and the chopped fiber prepreg.
[0070] Figure 5 It is a cross-sectional view illustrating the step of integrally curing the anisotropic prepreg and the chopped fiber prepreg.
[0071] Figure 6 It is a cross-sectional view illustrating the step of integrally curing the anisotropic prepreg and the chopped fiber prepreg.
[0072] Figure 7 This is a perspective view showing an example of an FRP product that can be produced by the production method according to the embodiment of the present invention.
[0073] Figure 8The figure shows a state where a prepreg tape and SMC are arranged in a press mold (lower mold), (a) is a plan view, and (b) is a cross-sectional view along the AA line of (a).
[0074] Fig. 9 The compression molded product is shown, (a) is a top view, and (b) is a cross-sectional view along the BB line of (a).
[0075] Fig.10 This is a cross-sectional view showing the steps of preparing the test piece used in Experiment 6.
[0076] Explanation of symbols
[0077] 10 Shaping fixture
[0078] 11 Board
[0079] 12 Support rods
[0080] 20 Prepreg tape (or tow prepreg)
[0081] 30 Prefabs
[0082] 41 Lower mold
[0083] 42 Upper mold
[0084] 51 Short-cut fiber prepreg
[0085] 52 Anisotropic prepreg
[0086] 61 Shaping fixture
[0087] 71 Anisotropic prepreg
[0088] 81 Core
[0089] 91 Chopped Fiber Prepreg
[0090] 95 Secondary Preform
[0091] 100 FRP products
[0092] 101 Chopped fiber reinforcement
[0093] 102 Neatly arranged fiber reinforcement
[0094] 201 SMC
[0095] 202 Prepreg Tape
[0096] 300 Pressing die (lower die)
[0097] 301 Cavity
[0098] 400 Compression molding
[0099] 401 Chopped fiber reinforcement
[0100] 402 Neatly arranged fiber reinforcement
[0101] 501 Thick Strip
[0102] 502 Heat-resistant belt
[0103] 503 SMC
[0104] 600 test pieces
[0105] 601 Neatly arranged fiber reinforcement
[0106] 603 Chopped Fiber Reinforcement DETAILED DESCRIPTION
[0107] Hereinafter, embodiments of the present invention will be described in detail.
[0108] In the method for producing the FRP product of the embodiment, a prepreg is used.
[0109] Examples of the fibers contained in the prepreg include carbon fibers, glass fibers, aramid fibers, boron fibers, silicon carbide fibers, high-strength polyethylene, polyparaphenylene benzophenone, and polyisocyanate. Polyolefin (PBO) fiber, nylon fiber, stainless steel fiber. Among them, carbon fiber having high strength despite low specific gravity is preferred.
[0110] The matrix resin composition contained in the prepreg contains a thermosetting resin such as epoxy resin, vinyl ester resin, unsaturated polyester resin, polyimide resin, maleimide resin, phenolic resin as a main component. In particular, the thermosetting resins with excellent adhesion to carbon fibers are epoxy resin and vinyl ester resin. The matrix resin composition may contain two or more thermosetting resins.
[0111] The matrix resin composition may contain various additives such as a low shrinkage agent, a filler, and a flame retardant as needed.
[0112] The matrix resin composition may also contain a thermoplastic resin. The preferred amount of the thermoplastic resin is 1% to 30% by mass of the total matrix resin composition, and may be 15% or less by mass. The thermoplastic resin that may be contained in the matrix resin composition includes, for example, polyolefins such as polyethylene and polypropylene, polyamides such as nylon 6 and nylon 66, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyether ketones, polyether sulfones, and aromatic polyamides.
[0113] [1. Method for manufacturing FRP products]
[0114] The method for producing an FRP product according to the embodiment includes at least (i) a prefabrication step and (ii) a compression molding step.
[0115] In the method for producing an FRP product according to the embodiment, the anisotropic prepreg is pre-cured before the compression molding step to suppress the disorder of the fiber arrangement in the aligned fiber reinforcement portion of the molded product obtained in the compression molding step.
[0116] According to the findings obtained by the inventors through experiments, when the anisotropic prepreg is pre-cured in such a way that the degree of cure of the anisotropic prepreg, which is 0% immediately before the prefabrication step, reaches 6% or more immediately before the compression molding step, the disorder of the fiber arrangement in the aligned fiber reinforcement portion of the molded product obtained in the compression molding step is suppressed.
[0117] Hereinafter, the prefabrication step, the compression molding step, and the pre-curing in the method for producing the FRP product according to the embodiment will be described in detail.
[0118] [1.1. Prefabrication process]
[0119] The prefabrication process is a process for prefabricating anisotropic prepreg.
[0120] Anisotropic prepreg is a general term for uniaxial prepreg and multiaxial prepreg.
[0121] In uniaxial prepreg, the fiber bundle is oriented in a single direction. Examples of uniaxial prepreg include: a unidirectional prepreg sheet in which a plurality of fiber bundles are paralleled in one direction and arranged in a single plane and impregnated with a matrix resin composition; a unidirectional prepreg tape in which a unidirectional prepreg sheet is cut along the fiber direction; and a tow prepreg (also called pre-impregnated tow) in which a single fiber bundle is impregnated with a matrix resin composition.
[0122] A prepreg obtained by impregnating a uniaxial non-crimped woven fabric formed by sewing fiber bundles paralleled in one direction into a matrix resin composition is also a type of uniaxial prepreg.
[0123] A typical example of a multiaxial prepreg is a cross prepreg obtained by impregnating a woven fabric composed of warp and weft yarns formed of fiber bundles with a matrix resin composition. In such a cross prepreg, fibers are oriented in two directions that are orthogonal to each other.
[0124] Cross prepreg using a triaxial fabric woven from fiber bundles is a multiaxial prepreg in which fibers are oriented in three directions.
[0125] A prepreg obtained by impregnating a laminate of a plurality of uniaxial non-crimped woven fabrics stacked and shifted in the axial direction with a matrix resin composition is a type of multiaxial prepreg.
[0126] In this specification and the present invention, the cutting process of the anisotropic prepreg is regarded as a kind of prefabrication operation. At the stage of providing the prefabrication process, the anisotropic prepreg may have a degree of softness that allows it to be cut by a small pair of scissors or a cutter having a metal blade.
[0127] An example of the cutting process performed on the anisotropic prepreg (anisotropic prepreg sheet) formed into a sheet shape in the prefabrication step is trimming to make the planar shape and size of the anisotropic prepreg sheet suitable for the purpose.
[0128] In the prefabrication process, a slit may be formed in the anisotropic prepreg sheet. A cutter may be used to form the slit. The slit formation may be accompanied by an operation of cutting a portion of the fiber bundle, for example, to prevent the fiber orientation from being disordered when a preform having a three-dimensional shape is formed from the anisotropic prepreg sheet.
[0129] The prefabrication of the anisotropic prepreg sheet in the prefabrication step may include straightening, that is, removing curls and flattening. The straightening of the anisotropic prepreg sheet may be performed by sandwiching the anisotropic prepreg sheet between two flat plates.
[0130] The prefabrication of the anisotropic prepreg sheet in the prefabrication step may include deforming the anisotropic prepreg sheet to form a preform in a three-dimensional shape.
[0131] When forming a preform of a three-dimensional shape, it is preferred to deform the anisotropic prepreg sheet by pressing it against a shaping mold. The preform can also be formed by winding the anisotropic prepreg sheet around a shaping mold of various shapes. The winding can be performed multiple times.
[0132] In the prefabrication process, the prefabrication of the elongated anisotropic prepreg such as the prepreg tape or the tow prepreg may include straightening, that is, removing curls to make the elongated anisotropic prepreg straight. The straightening of the elongated anisotropic prepreg may be performed by applying tension to the elongated anisotropic prepreg.
[0133] The prefabrication of an elongated anisotropic prepreg such as a prepreg tape or a tow prepreg in the prefabrication step may include winding the anisotropic prepreg around a shaping die to form a preform having a three-dimensional shape.
[0134] The prefabrication of the elongated anisotropic prepreg in the prefabrication step may include winding the prepreg around a shaping jig having a plurality of relatively fixedly arranged struts to form a preform having a three-dimensional shape. Figure 1 The shaping fixture 10 shown is an example thereof, and comprises a plate 11 and three support rods 12 vertically arranged on one surface thereof. Figure 2 As shown, the prepreg tape (or tow prepreg) 20 can be formed by applying tension to the prepreg tape (or tow prepreg) 20 and winding it around the three support rods 12 of the shaping jig 10. Figure 3 The preform 30 is shown.
[0135] By changing Figure 1 By changing the number and arrangement of the support rods 12 of the shaping jig 10 and the winding method of the prepreg tape (or tow prepreg) 20, preforms of various shapes can be formed.
[0136] When the elongated anisotropic prepreg is wound around a shaping mold or a shaping jig, the prepreg may be wound multiple times.
[0137] When a preform having a three-dimensional shape is formed from a curled anisotropic prepreg, the anisotropic prepreg may be corrected before being deformed into the three-dimensional shape.
[0138] In the prefabrication process, when the anisotropic prepreg is corrected or when a preform having a three-dimensional shape is formed from the anisotropic prepreg, the anisotropic prepreg can be integrated with other anisotropic prepregs.
[0139] In the prefabrication process, the anisotropic prepreg can be heated as needed to make the anisotropic prepreg easy to plastically deform. The heating of the anisotropic prepreg can be direct or indirect, and the method is not particularly limited. That is, the anisotropic prepreg can be directly heated by hot air or infrared rays, or the anisotropic prepreg can be indirectly heated by heating the shaping mold or the shaping fixture.
[0140] [1.2. Compression molding process]
[0141] The compression molding process is a process of solidifying the anisotropic prepreg prefabricated in the prefabrication process together with the chopped fiber prepreg in a press mold to obtain a molded product having a boundary between the regularly arranged fiber reinforcement part from the anisotropic prepreg and the chopped fiber reinforcement part from the chopped fiber prepreg.
[0142] The chopped fiber prepreg is a prepreg formed by impregnating a matrix resin composition into a chopped fiber bundle (also called a chopped fiber bundle) obtained by cutting the fiber bundle into a length of generally 100 mm or less, typically about 50 mm (about 2 inches) or about 25 mm (about 1 inch). Representative examples of chopped fiber prepreg are sheet molding compound (SMC) and bulk molding compound (BMC).
[0143] Compared with anisotropic prepreg, chopped fiber prepreg has excellent fluidity during molding.
[0144] In the compression molding process, for example, Figure 4 Steps shown.
[0145] Figure 4 (a) is a cross-sectional view showing a lower die 41 of a pressing die.
[0146] Figure 4 (b) shows a state where the chopped strand prepreg (SMC) 51 is placed in the lower mold 41 .
[0147] Figure 4 (c) shows a state where anisotropic prepreg 52 is further arranged in the lower mold 41 and overlapped on a part of the chopped strand prepreg (SMC) 51 .
[0148] Figure 4 (d) shows a state where the upper mold 42 is lowered to heat and compress the chopped strand prepreg (SMC) 51 and the anisotropic prepreg 52 .
[0149] In another example, during the compression molding process, Figure 5 and Figure 6 Steps shown.
[0150] Figure 5 (a) is a cross-sectional view of a shaping mold (or shaping jig) 61 .
[0151] Figure 5 (b) shows a state where anisotropic prepreg 71 is preformed by winding it around a shaping mold (or shaping jig) 61. The boundaries 72 between the prepreg ends of the preformed anisotropic prepreg 71 are not particularly limited, but the prepreg ends may overlap each other.
[0152] Figure 5 (c) shows a state where the preformed anisotropic prepreg 71 is separated from the shaping mold (or shaping jig) 61 .
[0153] Figure 6 (a) is a cross-sectional view of a core mold 81 used in the compression molding step.
[0154] Figure 6 (b) shows a state where chopped fiber prepreg (SMC) 91 is prefabricated by winding it around a core 81. Although there is no particular limitation on the boundaries 92 between the prepreg ends of the prefabricated chopped fiber prepreg (SMC) 91, the prepreg ends may be connected to each other.
[0155] Figure 6 (c) shows a state where the preformed anisotropic prepreg 71 is fitted into the preformed chopped strand prepreg (SMC) 91 to form a secondary preform 95. In the compression molding step, the secondary preform 95 is placed in a press mold together with the core 81 to be heated and compressed.
[0156] The compression molding conditions can refer to the conditions used in the compression molding of FRP products in the past, and although not particularly limited, the molding temperature is, for example, 100°C to 200°C, the molding pressure is, for example, 1 MPa to 10 MPa, and the molding time is, for example, 1 minute to 20 minutes.
[0157] [1.3. Pre-curing of anisotropic prepreg]
[0158] The purpose of pre-curing the anisotropic prepreg before the compression molding process is to suppress the flow of the anisotropic prepreg in the compression molding process by allowing the curing reaction (gelation) to proceed in advance, thereby suppressing the disorder of the fiber arrangement in the aligned fiber reinforcement part of the obtained compression molded product. If the anisotropic prepreg is not pre-cured, when the chopped fiber prepreg loaded together with the anisotropic prepreg in the press mold flows, the anisotropic prepreg will also flow, causing the orientation of the fibers constituting the anisotropic prepreg to become disordered.
[0159] Precuring can be performed by heating the anisotropic prepreg.
[0160] When setting the conditions for pre-curing, the degree of curing defined by the following formula (1) is useful as an index.
[0161] [Mathematical formula 1]
[0162]
[0163] In the above formula (1), the total heat release and the residual heat release are the heat release values when the sample is heated from room temperature (25°C) to 300°C at 10°C / min in a nitrogen atmosphere in differential scanning calorimetry (DSC).
[0164] The total heat release is the heat release of the anisotropic prepreg immediately before the prefabrication process begins. It is equivalent to the heat released by the anisotropic prepreg immediately before the prefabrication process begins until it is completely cured.
[0165] The residual heat release is the heat release exhibited by the anisotropic prepreg at a certain point in time after the start of the prefabrication process, and is equivalent to the heat released by the anisotropic prepreg from that point in time until complete curing.
[0166] In short, the degree of curing in this specification indicates to what extent the curing of the anisotropic prepreg has progressed, when the state immediately before the prefabrication step is 0% and the state after complete curing is 100%.
[0167] As shown in the experimental results described below, when the anisotropic prepreg and the chopped fiber prepreg, which had a curing degree of 6% by heat treatment before the compression molding process, were integrally cured in a press mold, it was confirmed that the fiber arrangement disorder in the regularly arranged fiber reinforcement part was suppressed in the obtained compression molded product.
[0168] In this experiment, heating at 80°C for 2.5 hours was required to make the curing degree of the anisotropic prepreg 6%, which indicates that the heating for the purpose of softening the matrix resin in the B stage when prefabricating the anisotropic prepreg in the prior art does not serve as pre-curing. In the above heating, the heating time is usually kept below 1 minute so as not to make the surface temperature exceed 80°C, and therefore, the curing degree of the anisotropic prepreg does not substantially change.
[0169] The cutting process that can be performed in the prefabrication process usually does not have a substantial effect on the degree of curing of the anisotropic prepreg. Therefore, for example, when the first process performed on the anisotropic prepreg in the prefabrication process is the cutting process, the heat release of the anisotropic prepreg measured immediately after the cutting process can be treated as the total heat release.
[0170] The heat treatment as the preliminary curing is preferably performed so that the degree of cure of the anisotropic prepreg immediately before the compression molding step becomes 6% or more.
[0171] If the composition of the matrix resin is different, the degree of curing of the anisotropic prepreg achieved by the same heat treatment may be different, and as a tendency, the higher the temperature of the heat treatment and the longer the time, the higher the degree of curing of the prepreg. Therefore, by changing the conditions of the heat treatment, conducting multiple trials, and feeding back the results, it is possible to easily set the precuring conditions that allow the anisotropic prepreg to achieve the desired degree of curing.
[0172] According to the experiments conducted by the inventors, the curing degree of the anisotropic prepreg immediately before the compression molding process is more preferably 18% or more, and more preferably 36% or more. The pre-curing of the anisotropic prepreg has little effect on the bonding strength between the aligned fiber reinforcement part and the chopped fiber reinforcement part in the compression molded product. As shown in the experimental results described later, when the curing degree of the anisotropic prepreg immediately before the compression molding process is 94%, the anisotropic prepreg and the chopped fiber prepreg can be preferably integrally molded.
[0173] The pre-curing can be performed simultaneously, for example, when the anisotropic prepreg is corrected in the pre-fabrication step or when a preform having a three-dimensional shape is formed from the anisotropic prepreg in the pre-fabrication step.
[0174] For example, by appropriately setting the temperature and holding time of the plates when correcting a curled anisotropic prepreg sheet held between two plates, the degree of cure of the corrected anisotropic prepreg sheet can be set to any value of 6% or more.
[0175] Alternatively, in order to correct a curled unidirectional prepreg tape or tow prepreg, it can be heated using hot air or infrared rays while tension is applied. By appropriately setting the temperature and time at this time, the degree of curing of the corrected unidirectional prepreg tape or tow prepreg can reach any value above 6%.
[0176] In other examples, when an anisotropic prepreg is deformed to form a preform having a three-dimensional shape by pressing it against a shaping mold and holding it, or by winding it around a shaping mold or a shaping fixture and holding it, the degree of curing of the anisotropic prepreg can be made to reach any value above 6% by placing the anisotropic prepreg together with the shaping mold or the shaping fixture into a hot air oven and appropriately setting the holding temperature and holding time.
[0177] The heating treatment for pre-curing can be performed after the prefabrication process is completed. For example, after the curling is corrected, the anisotropic prepreg removed from the correction fixture can be subjected to the heating treatment for pre-curing. Alternatively, after the preform is formed into a three-dimensional shape using a shaping mold or a shaping fixture, the preform can be removed from the fixture and subjected to the heating treatment for pre-curing.
[0178] Of course, the processing performed on the anisotropic prepreg in the prefabrication step may be only the cutting process.
[0179] The heating treatment for pre-curing may be performed in several steps. For example, additional heating treatment of the anisotropic prepreg that has been heat-treated in the pre-fabrication step may be performed after the pre-fabrication step is completed.
[0180] The present inventors have experimentally found that the effect of suppressing the disorder of the fiber arrangement in the aligned fiber reinforcement portion of the molded product due to the pre-curing of the anisotropic prepreg has a tendency to reach saturation when the curing degree of the anisotropic prepreg exceeds about 36% immediately before the compression molding process. In addition, the results of studying the change over time of the curing degree when the anisotropic prepreg is subjected to a heat treatment have shown that the curing degree has the following tendency: after initially increasing slowly, it rises sharply when it reaches 5 to 6%, and then turns to slowly increase again after exceeding 60%.
[0181] Therefore, from the perspective of production efficiency, the degree of curing of the anisotropic prepreg immediately before the compression molding process begins is preferably 60% or less. For the molded product to be manufactured, in order to obtain sufficient and necessary results, it can be 50% or less, further 40% or less, further 30% or less, further 20% or less, and further 10% or less.
[0182] The lower limit and upper limit of the curing degree of the anisotropic prepreg immediately before the compression molding process described above can be arbitrarily combined. For example, the curing degree of the anisotropic prepreg immediately before the compression molding process is 6 to 94%, 6 to 60%, 6 to 50%, 6 to 40%, 6 to 30%, 6 to 20%, 6 to 10%, 18 to 94%, 18 to 60%, 18 to 50%, 18 to 40%, 18 to 30%, 18 to 20%, 36 to 94%, 36 to 60%, 36 to 50%, 36 to 40%.
[0183] [2. Shape of FRP products]
[0184] The method for producing an FRP product according to the embodiment can be preferably used for producing an FRP product having a three-dimensional shape.
[0185] In a preferred example of the FRP product manufactured by the method for manufacturing an FRP product of the embodiment, the aligned fiber reinforcement part is arranged on a part of the product surface so that the fibers contained in the aligned fiber reinforcement part are parallel to the product surface. In particular, in an FRP product having a ridgeline on the surface, the aligned fiber reinforcement part in which the fibers are oriented in one direction is preferably arranged along all or part of the ridgeline so that the orientation direction of the fibers is parallel to the ridgeline.
[0186] Figure 7 This is a perspective view showing an example of an FRP product manufactured by the method for manufacturing an FRP product according to the embodiment. Figure 7 The FRP product 100 shown is a rectangular parallelepiped, and has chopped fiber reinforcements 101 constituting each face (six faces) of the rectangular parallelepiped, and aligned fiber reinforcements 102 arranged along the ridges of the rectangular parallelepiped. In the aligned fiber reinforcements 102, the direction of the fibers is parallel to the ridges.
[0187] [3. Experimental results]
[0188] The results of experiments conducted by the present inventors are described below.
[0189] The prepregs used in the experiment are shown in Table 1 below.
[0190] [Table 1]
[0191]
[0192] The tow prepreg can be produced by developing (opening) a carbon fiber tow with 50,000 filaments (PYROFIL (registered trademark) TRW40 50L manufactured by Mitsubishi Chemical Corporation) and then impregnating the tow prepreg with epoxy resin by a melt method. The tow prepreg produced has a width of 12.7 mm, a maximum thickness of 0.3 mm, and a resin content of 38%.
[0193] In all the experiments, a differential scanning calorimeter (DSC) device Q-1000 manufactured by TA INSTRUMENTS was used to measure the heat release amount in order to determine the degree of cure of the anisotropic prepreg.
[0194] In DSC, 5 mg to 10 mg of a sample was heated from room temperature (25° C.) to 300° C. at 10° C. / min in a nitrogen atmosphere.
[0195] DSC samples were collected at three locations near one end of the prepreg tape or tow prepreg, and the heat release values measured for the samples were averaged to obtain the heat release value of the prepreg tape or tow prepreg.
[0196] [Experiment 1]
[0197] A prepreg tape having a length of 285 mm, a width of 25 mm, and a thickness of 0.2 mm with the fiber direction as the longitudinal direction was cut from a unidirectional prepreg sheet having a resin content of 30% (PYROFIL (registered trademark) TR361E250S manufactured by Mitsubishi Chemical Corporation), and placed in a hot air oven and maintained at 80° C. for 4 hours. The degree of cure of the prepreg tape after the heat treatment was 19%.
[0198] The heat-treated prepreg tape was loaded into the cavity of a press mold (lower mold) together with SMC cut into 295 mm squares and 2 mm in thickness.
[0199] like Figure 8 As shown in (a) (top view) and (b) (cross-sectional view), SMC201 is placed flat on the bottom surface of the cavity 301 of the pressing mold 300, and the prepreg tape 202 is arranged on the upper surface of SMC201 in a manner that the length direction is parallel to the opposite sides of SMC201.
[0200] The cavity bottom surface of the press mold 300 is 300 mm square, so the SMC filling rate obtained by dividing the area of the SMC by the bottom area of the cavity is 93%.
[0201] The SMC 201 and the prepreg tape 202 were integrally cured under the conditions of a pressure of 4 MPa, a temperature of 140° C., and a curing time of 5 minutes to obtain Fig. 9The compression molded product 400 shown in (a) (top view) and (b) (cross-sectional view) has the surface of the chopped fiber reinforcement part 401 and the surface of the aligned fiber reinforcement part 402 on the same plane, and the compression molded product 400 is a plate of 300 mm square and 2 mm thickness.
[0202] In the obtained compression molded product 400, at the midpoint in the width direction of one end of the connected aligned fiber reinforcement portion 402 ( Fig. 9 (a) and the midpoint in the width direction of the other end ( Fig. 9 When the direction of the line segment PQ from the point Q) shown in (a) is taken as the reference direction, a portion where the direction of the fibers deviates from the reference direction can be visually recognized in the aligned fiber reinforced portion 402. The deviation angle of the fibers in such a portion (the angle between the fibers and the reference direction) is 6° at most in the aligned fiber reinforced portion 402.
[0203] [Experiment 2]
[0204] A compression molded article was produced in the same manner as in Experiment 1 except that the heating time (80° C. holding time) in the heat treatment of the prepreg tape was 5 hours. The degree of cure of the prepreg tape after the heat treatment was 48%.
[0205] In the aligned fiber-reinforced portion of the compression molded product, no portion where the fiber direction deviated from the reference direction was confirmed. That is, in the aligned fiber-reinforced portion, the deviation angle of the fiber was 0°.
[0206] [Experiment 3]
[0207] A compression molded article was produced in the same manner as in Experiment 1 except that a tow prepreg cut to a length of 285 mm was used instead of the prepreg tape and the heating time (80° C. holding time) in the heat treatment of the tow prepreg was set to 2.5 hours. The degree of cure of the tow prepreg after the heat treatment was 6%.
[0208] In the aligned fiber reinforcement portion of the compression molded product, a portion where the fiber direction deviated from the reference direction was confirmed. In the aligned fiber reinforcement portion, the maximum value of the deviation angle of the fibers was 6°.
[0209] [Experiment 4]
[0210] A compression molded article was produced in the same manner as in Experiment 1, except that a tow prepreg cut to a length of 285 mm was used instead of the prepreg tape cut from the unidirectional prepreg sheet and the heating time (80° C. holding time) in the heat treatment of the tow prepreg was set to 3 hours. The degree of cure of the tow prepreg after the heat treatment was 18%.
[0211] In the aligned fiber reinforced portion of the compression molded product, a portion where the fiber direction deviated from the reference direction was confirmed. In the aligned fiber reinforced portion, the maximum value of the deviation angle of the fibers was 5°.
[0212] [Experiment 5]
[0213] A compression molded article was produced in the same manner as in Experiment 3 except that the heating time (80° C. holding time) in the heat treatment of the tow prepreg was 3.5 hours. The degree of cure of the tow prepreg after the heat treatment was 36%.
[0214] In the aligned fiber-reinforced portion of the compression molded product, no portion where the fiber direction deviated from the reference direction was confirmed. That is, in the aligned fiber-reinforced portion, the deviation angle of the fiber was 0°.
[0215] [Comparative Experiment 1]
[0216] A compression molded article was produced in the same manner as in Experiment 1 except that the prepreg tape was not subjected to heat treatment.
[0217] In the aligned fiber reinforcement portion of the compression molded product, a portion where the fiber direction deviated from the reference direction was confirmed. In the aligned fiber reinforcement portion, the maximum value of the deviation angle of the fibers was 12°.
[0218] [Comparative Experiment 2]
[0219] A compression molded article was produced in the same manner as in Experiment 3 except that the tow prepreg was not subjected to heat treatment.
[0220] In the aligned fiber reinforcement portion of the compression molded product, a portion where the fiber direction deviated from the reference direction was confirmed. In the aligned fiber reinforcement portion, the maximum value of the deviation angle of the fibers was 9°.
[0221] The results of Experiments 1 to 5 and Comparative Experiments 1 and 2 are shown in Tables 2 and 3.
[0222] [Table 2]
[0223]
[0224] [Table 3]
[0225]
[0226] [Experiment 6]
[0227] An experiment was conducted to evaluate the bonding strength at the interface between an aligned fiber reinforcement portion and a chopped fiber reinforcement portion in a compression molded product obtained by integrally curing a precured anisotropic prepreg and a chopped fiber prepreg.
[0228] First, 10 strips of 75 mm in length, 25 mm in width, and 0.2 mm in thickness cut from a prepreg sheet were stacked and made to adhere to each other by vacuum compaction. The stack was placed in a hot air oven at 80°C for 8 hours to obtain a thick strip formed by integrating the 10 strips. The curing degree of the thick strip was 94%.
[0229] Then, if Fig.10 As shown in the cross-sectional view of (a), the heat-resistant belt 502 is wound around a portion of the thick strip 501, and only one end 501A of the thick strip 501 is exposed in a predetermined area.
[0230] In addition, if Fig.10 As shown in the cross-sectional view of (b), the end portion 501A of the thick strip 501 is sandwiched between two SMC503 sheets cut to 2 mm thick, 70 mm long and 28 mm wide, and then pressed at 140°C to 150°C for 5 minutes to produce a Fig.10 (c) shows a test piece 600 having an aligned fiber reinforcement portion 601 and a chopped fiber reinforcement portion 603 .
[0231] The aligned fiber reinforcement part 601 is a part formed by solidifying the thick strip 501 , and the chopped fiber reinforcement part 603 is a part formed by solidifying the SMC 503 .
[0232] The tensile test was performed using a universal testing machine 4482 manufactured by Instron, and the strength of the interface between the neatly arranged fiber reinforcement 601 and the short fiber reinforcement 603 in the test piece 600 was evaluated. A load cell with a load capacity of 100 kN was used in the tensile test, and the tensile speed was set to 0.5 mm / min. The test piece was destroyed at the interface between the neatly arranged fiber reinforcement 601 and the short fiber reinforcement 603. The shear strength of the interface obtained based on the load at the time of destruction and the contact area between the neatly arranged fiber reinforcement and the short fiber reinforcement was 17 (N / mm 2 ).
[0233] [Comparative Experiment 3]
[0234] A comparative test piece was produced in the same manner as the test piece produced in Experiment 6 except that a tape obtained by winding an unheat-treated prepreg tape around a SUS304 metal tape was used instead of the thick tape formed of the heat-treated prepreg.
[0235] The prepreg tape was cut from the prepreg sheet with the fiber direction as the length direction and had a width of 25 mm. The metal strip had a length of 75 mm, a width of 28 mm, and a thickness of 2 mm.
[0236] The prepreg tape is wound so that its fiber direction is parallel to the length direction of the metal strip.
[0237] When the heat-resistant belt was wound, the area of the interface between the aligned fiber reinforcement portion and the chopped fiber reinforcement portion in the comparative test piece was made the same as that of the test piece in Experiment 6.
[0238] The tensile test was carried out in the same manner as in Experiment 6. The result showed that in the comparative test piece, the interface between the aligned fiber reinforcement and the chopped fiber reinforcement also failed. The shear strength of the interface obtained from the load at failure and the contact area between the aligned fiber reinforcement and the chopped fiber reinforcement was 16.7 (N / mm 2 ), which is basically the same as the test piece in Experiment 6.
[0239] This result indicates that even when the curing degree of the anisotropic prepreg is increased to 94% by precuring, the strength of the interface between the aligned fiber reinforcement portion and the chopped fiber reinforcement portion can be sufficiently ensured in the compression molded product obtained by integrally curing the anisotropic prepreg and the chopped fiber prepreg.
[0240] Industrial Usability
[0241] The method for manufacturing the FRP product of the present invention can be used for manufacturing FRP components used in transportation equipment and industrial equipment, as well as for manufacturing FRP sports goods and leisure goods. The method for manufacturing the FRP product of the present invention is particularly suitable for manufacturing FRP automobile components.
Claims
1. A method for manufacturing a FRP product, the method include: (i) a prefabrication step of prefabricating an anisotropic prepreg as a uniaxial prepreg containing an epoxy resin, the prefabrication step comprising at least one of correcting the anisotropic prepreg and forming a preform having a three-dimensional shape from the anisotropic prepreg; and (ii) a compression molding step of curing the anisotropic prepreg prefabricated in the prefabrication step integrally with the chopped fiber prepreg in a press mold to obtain a molded product having a boundary between the aligned fiber reinforcement portion derived from the anisotropic prepreg and the chopped fiber reinforcement portion derived from the chopped fiber prepreg, The anisotropic prepreg is pre-cured after the prefabrication step and before the compression molding step, thereby suppressing the disorder of the fiber arrangement of the aligned fiber reinforcement portion of the molded product obtained in the compression molding step.
2. The manufacturing method according to claim 1, in, When the degree of curing of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is 6% or more immediately before the compression molding step.
3. A method for manufacturing a FRP product, the method include: (i) a prefabrication step of prefabricating an anisotropic prepreg as a uniaxial prepreg containing an epoxy resin, the prefabrication step comprising at least one of correcting the anisotropic prepreg and forming a preform having a three-dimensional shape from the anisotropic prepreg; (ii) a compression molding step of curing the anisotropic prepreg prefabricated in the prefabrication step integrally with the chopped fiber prepreg in a press mold to obtain a molded product having a boundary between the aligned fiber reinforcement portion derived from the anisotropic prepreg and the chopped fiber reinforcement portion derived from the chopped fiber prepreg, Here, when the degree of curing of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is 6% or more immediately before the compression molding step.
4. The production method according to any one of claims 1 to 3, in, When the degree of curing of the anisotropic prepreg is assumed to be 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is 18% or more immediately before the compression molding step.
5. The manufacturing method according to claim 1 or 3, in, When the degree of curing of the anisotropic prepreg immediately before the compression molding step is assumed to be 0%, the degree of curing of the anisotropic prepreg immediately before the compression molding step is 94% or less.
6. The manufacturing method according to claim 1 or 3, in, When the degree of curing of the anisotropic prepreg immediately before the compression molding step is assumed to be 0%, the degree of curing of the anisotropic prepreg immediately before the compression molding step is 60% or less.
7. The manufacturing method according to claim 1 or 3, in, The prefabrication process includes cutting the anisotropic prepreg.
8. The manufacturing method according to claim 1, in, In the prefabrication step, the anisotropic prepreg is multi-wound on a forming mold or a forming jig.
9. The manufacturing method according to claim 1 or 3, in, In the prefabrication process, the anisotropic prepreg is formed into one body with other anisotropic prepregs.
10. The manufacturing method according to claim 1 or 3, in, In the prefabrication process, pre-curing of the anisotropic prepreg is at least partially performed.
11. The manufacturing method according to claim 10, in, When the degree of curing of the anisotropic prepreg is set to 0% immediately before the prefabrication step, the degree of curing of the anisotropic prepreg is 6% or more at the end of the prefabrication step.
12. The manufacturing method according to claim 1 or 3, in, The anisotropic prepreg contains carbon fibers.
13. The manufacturing method according to claim 1 or 3, in, The chopped fiber prepreg contains carbon fibers.
14. The manufacturing method according to claim 1 or 3, in, The chopped fiber prepreg contains at least one selected from vinyl ester resin and unsaturated polyester resin.
15. The manufacturing method according to claim 1 or 3, in, The chopped fiber prepreg contains epoxy resin.
16. The manufacturing method according to claim 1 or 3, in, The chopped fiber prepreg is a sheet molding compound.
17. The manufacturing method according to claim 1 or 3, in, The aligned fiber-reinforced portion is arranged on a portion of the surface of the molded article such that fibers included in the aligned fiber-reinforced portion are parallel to the surface of the molded article obtained in the compression molding step.
18. The manufacturing method according to claim 1 or 3, in, The molded product obtained in the compression molding step has a ridgeline on the surface, and the neatly arranged fiber reinforcement portion in which fibers are oriented in one direction is arranged along all or part of the ridgeline in such a way that the direction of the fibers of the neatly arranged fiber reinforcement portion in which fibers are oriented in one direction is parallel to the ridgeline.
19. A method for manufacturing a FRP product, the method include: (i) a prefabrication process, prefabrication of anisotropic prepreg; as well as (ii) a compression molding step of curing the anisotropic prepreg prefabricated in the prefabrication step integrally with the chopped fiber prepreg in a press mold to obtain a molded product having a boundary between the aligned fiber reinforcement portion derived from the anisotropic prepreg and the chopped fiber reinforcement portion derived from the chopped fiber prepreg, The anisotropic prepreg is pre-cured before the compression molding step, thereby suppressing the disorder of the fiber arrangement of the aligned fiber reinforcement part of the molded product obtained in the compression molding step. The surface of the chopped fiber reinforcement part is on the same plane as the surface of the neatly arranged fiber reinforcement part.
Citation Information
Patent Citations
Fiber-reinforced resin molded article and method for manufacturing fiber-reinforced resin molded article
WO2018101245A1
Manufacture of fiber reinforced plastic molded product
JP1997109167A
Method for producing fiber-reinforced resin composite material and fiber-reinforced resin composite material
JP2004338270A
Method for producing preform, method for producing fiber-reinforced thermocurable resin-molded article, and preform
JP2016017111A
Method for Producing an SMC Component Provided with a Unidirectional Fiber Reinforced
US20170136714A1