Non-aqueous electrolyte secondary battery and method for manufacturing non-aqueous electrolyte secondary battery

By adjusting the binder content ratio in the electrode mixture layer of the non-aqueous electrolyte secondary battery, the problem of cracks and peeling of the electrode mixture layer is solved, the internal resistance is reduced, and the battery performance is improved.

CN114270592BActive Publication Date: 2024-10-11PANASONIC ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080059098.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-28
Filing Date
2020-08-18
Publication Date
2024-10-11
Estimated Expiration
2040-08-18

AI Technical Summary

Technical Problem

Existing technology cannot effectively suppress cracks and peeling of the positive and negative electrode mixture layers in non-aqueous electrolyte secondary batteries, and increasing the binder content will cause internal resistance to rise, affecting battery characteristics.

Method used

By changing the binder content ratio from the beginning to the end in the mixture layer of the positive and negative electrodes, a variety of mixture slurries are formed and applied to ensure that the binder content at the beginning is higher than that at the end, reducing cracks and peeling of the mixture layer, and suppresses the increase in internal resistance.

Benefits of technology

It effectively suppresses cracks and peeling of the battery mixture layer, reduces internal resistance, and improves battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114270592B_ABST
    Figure CN114270592B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a non-aqueous electrolyte secondary battery which suppresses the internal resistance of the battery caused by the binder contained in the mixture layer and suppresses the cracking and peeling of the mixture layer. The non-aqueous electrolyte secondary battery of one embodiment of the present invention comprises a wound electrode body formed by winding a strip-shaped positive electrode (11) and a strip-shaped negative electrode (12) with a separator in between, and an outer packaging body for accommodating the electrode body. The positive electrode (11) comprises a positive electrode collector (30) and a positive electrode mixture layer (32) formed on the positive electrode collector (30) and comprising at least a positive electrode active material and a binder, and the negative electrode (12) comprises a negative electrode collector (40) and a negative electrode mixture layer (42) formed on the negative electrode collector (40) and comprising at least a negative electrode active material and a binder. The content of the binder at the starting end portion (42a) of at least one of the positive electrode mixture layer (32) and the negative electrode mixture layer (42) is higher than the content of the binder at the terminal portion (42b).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nonaqueous electrolyte secondary battery and a method for manufacturing the nonaqueous electrolyte secondary battery. Background Art

[0002] A non-aqueous electrolyte secondary battery in which a wound electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator and contained in an outer package has been widely used. The electrodes (positive and negative electrodes) of the electrode body have a composite layer containing an active material and a binder on both sides of each metal collector. Sometimes cracks are generated in the composite layer due to the winding of the electrode, or the composite layer is peeled off from the collector. Patent document 1 discloses a method for suppressing the peeling of the composite layer on the inner circumference of the collector by increasing the content of the binder (adhesive) contained in the composite layer on the inner circumference of the collector.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 8-17472 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] However, the technology disclosed in Patent Document 1 cannot fully suppress cracking and peeling of the mixture layer at the beginning of the winding start side of the electrode body in which the positive electrode and the negative electrode are wound with a small curvature radius. If the content of the binder is increased to suppress cracking and peeling of the mixture layer, there is a problem that the internal resistance of the battery increases and the battery characteristics decrease.

[0008] An object of the present invention is to provide a nonaqueous electrolyte secondary battery in which an increase in the internal resistance of the battery due to a binder contained in a material mixture layer is suppressed, and cracking and peeling of the material mixture layer are suppressed.

[0009] Means used to solve problems

[0010] A nonaqueous electrolyte secondary battery as one embodiment of the present invention is a nonaqueous electrolyte secondary battery having a wound electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween, and an outer packaging body for accommodating the electrode body. The battery is characterized in that the positive electrode has a positive electrode collector and a positive electrode mixture layer formed on the positive electrode collector and containing at least a positive electrode active material and a binder, and the negative electrode has a negative electrode collector and a negative electrode mixture layer formed on the negative electrode collector and containing at least a negative electrode active material and a binder, and the content of the binder at the beginning of at least one of the positive electrode mixture layer and the negative electrode mixture layer is higher than the content of the binder at the end.

[0011] A method for manufacturing a nonaqueous electrolyte secondary battery as one embodiment of the present invention is a method for manufacturing a nonaqueous electrolyte secondary battery having a wound electrode body formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween, and an outer package body for accommodating the electrode body. The method is characterized in that it includes: a positive electrode mixture layer forming step of forming a positive electrode mixture layer containing at least a positive electrode active material and a binder on a positive electrode current collector of a positive electrode; and a negative electrode mixture layer forming step of forming a negative electrode mixture layer containing at least a negative electrode active material and a binder on a negative electrode current collector of a negative electrode, and in at least one of the positive electrode mixture layer forming step and the negative electrode mixture layer forming step, the coating amount ratio of a plurality of mixture slurries having different binder contents is changed from one side of a starting end portion side to the other side of a terminal portion side, and the plurality of mixture slurries are coated.

[0012] Effects of the Invention

[0013] According to the nonaqueous electrolyte secondary battery of the present invention, it is possible to suppress an increase in the internal resistance of the battery due to the binder contained in the material mixture layer, and to suppress cracking and peeling of the material mixture layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is an axial cross-sectional view of a cylindrical secondary battery as an example of an embodiment.

[0015] Figure 2 yes Figure 1 The illustrated secondary battery is a perspective view of a wound electrode assembly.

[0016] Figure 3 It is a front view showing a positive electrode and a negative electrode constituting an electrode body as an example of an embodiment in a developed state.

[0017] Figure 4 (a)~ Figure 4 (d) means Figure 3 A graph showing changes in the content of the binder contained in the negative electrode mixture layer in the longitudinal direction.

[0018] Figure 5 This is a radial cross-sectional view of a negative electrode in the vicinity of a winding axis of an electrode assembly as an example of an embodiment. DETAILED DESCRIPTION

[0019] Hereinafter, an example of an embodiment of a cylindrical secondary battery according to the present invention will be described in detail with reference to the accompanying drawings. In the following description, specific shapes, materials, numerical values, directions, etc. are provided for easy understanding of the present invention and can be appropriately changed according to the specifications of the cylindrical secondary battery. In addition, in the following description, when multiple embodiments and variations are included, it is initially envisioned that their characteristic parts can be appropriately combined and used.

[0020] Figure 1 It is an axial cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1 In the secondary battery 10 shown, the electrode body 14 and the non-aqueous electrolyte (not shown) are contained in the outer packaging body 15. The electrode body 14 has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound with the separator 13 in between. As a non-aqueous solvent (organic solvent) of the non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and these solvents can be mixed and used in two or more kinds. In the case of mixing and using two or more solvents, it is preferred to use a mixed solvent containing cyclic carbonates and chain carbonates. For example, as cyclic carbonates, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used, and as chain carbonates, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), etc. can be used. As the electrolyte salt of the non-aqueous electrolyte, LiPF can be used. 6 , LiBF 4 、LiCF 3 SO 3 The amount of the electrolyte salt dissolved in the non-aqueous solvent may be, for example, 0.5 to 2.0 mol / L. In the following, for convenience of description, the sealing body 16 side is referred to as "upper" and the bottom side of the outer package 15 is referred to as "lower".

[0021] The interior of the secondary battery 10 is sealed by blocking the open end of the outer package 15 with a sealing body 16. Insulating plates 17 and 18 are provided above and below the electrode body 14, respectively. The positive lead 19 extends upward through the through hole of the insulating plate 17 and is welded to the bottom plate of the sealing body 16, that is, the lower surface of the filter plate 22. In the secondary battery 10, the top plate of the sealing body 16, that is, the cap 26, which is electrically connected to the filter plate 22, becomes the positive terminal. On the other hand, the negative lead 20 passes through the through hole of the insulating plate 18, extends to the bottom side of the outer package 15, and is welded to the bottom inner surface of the outer package 15. In the secondary battery 10, the outer package 15 becomes the negative terminal. It should be noted that when the negative lead 20 is provided at the terminal portion, the negative lead 20 passes through the outside of the insulating plate 18, extends to the bottom side of the outer package 15, and is welded to the bottom inner surface of the outer package 15.

[0022] The outer package 15 is, for example, a metal outer package can in a cylindrical shape with a bottom. A sealing gasket 27 is provided between the outer package 15 and the sealing body 16 to ensure the airtightness of the interior of the secondary battery 10. The outer package 15 has a groove portion 21 formed by, for example, pressing the side portion from the outside to support the sealing body 16. The groove portion 21 is preferably formed in an annular shape along the circumference of the outer package 15, and supports the sealing body 16 on its upper surface.

[0023] The sealing body 16 has a filter plate 22, a lower valve body 23, an insulating component 24, an upper valve body 25 and a cap 26 stacked in sequence starting from the electrode body 14 side. The various components constituting the sealing body 16 have, for example, a disc shape or a ring shape, and the various components except the insulating component 24 are electrically connected to each other. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective central portions, and the insulating component 24 is interposed between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat, for example, the lower valve body 23 breaks, whereby the upper valve body 25 expands toward the cap 26 side and separates from the lower valve body 23, thereby blocking the electrical connection between the two. If the internal pressure rises further, the upper valve body 25 breaks, and gas is discharged from the opening 26a of the cap 26.

[0024] Next, refer to Figure 2 , while explaining the electrode body 14. Figure 2 It is a three-dimensional diagram of the electrode body 14. As described above, the electrode body 14 has a winding structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 between them. The positive electrode 11, the negative electrode 12, and the separator 13 are all formed into a strip shape, and are spirally wound around the winding core arranged along the winding axis 28 so as to be alternately stacked along the radial direction of the electrode body 14. In the radial direction, the side of the winding axis 28 is called the inner peripheral side, and the opposite side is called the outer peripheral side. In the electrode body 14, the length direction of the positive electrode 11 and the negative electrode 12 becomes the winding direction, and the belt width direction of the positive electrode 11 and the negative electrode 12 becomes the axial direction. At the upper end of the electrode body 14, the positive lead 19 extends axially from the approximate center of the radial direction between the center and the outermost periphery. In addition, at the lower end of the electrode body 14, the negative lead 20 extends axially from near the winding axis 28.

[0025] For the separator 13, a porous sheet having ion permeability and insulation can be used. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the separator 13, olefin resins such as polyethylene and polypropylene are preferred. The thickness of the separator 13 is, for example, 10 μm to 50 μm. With the increase in capacity and output of the battery, the separator 13 tends to be thinner. The separator 13 has a melting point of, for example, about 130° C. to 180° C.

[0026] Next, refer to Figure 3 to Figure 5 , an embodiment in which the content of the binder in the negative electrode mixture layer 42 in the longitudinal direction is non-uniform will be described. Figure 3 It is a front view of the positive electrode 11 and the negative electrode 12 constituting the electrode body 14 . Figure 3 In the figure, the positive electrode 11 and the negative electrode 12 are shown in an unfolded state. Figure 3For example, in the electrode body 14, in order to prevent the precipitation of lithium in the negative electrode 12, the negative electrode 12 is formed larger than the positive electrode 11. Specifically, the length of the negative electrode 12 in the belt width direction (axial direction) is greater than the length of the positive electrode 11 in the belt width direction. In addition, the length of the negative electrode 12 in the longitudinal direction is greater than the length of the positive electrode 11 in the longitudinal direction. Therefore, when the electrode body 14 is wound, at least the portion of the positive electrode 11 where the positive electrode mixture layer 32 is formed is arranged opposite to the portion of the negative electrode 12 where the negative electrode mixture layer 42 is formed, through the separator 13.

[0027] The positive electrode 11 has a strip-shaped positive electrode collector 30 and a positive electrode mixture layer 32 formed on the positive electrode collector 30. The positive electrode mixture layer 32 is formed on at least one of the inner circumference and the outer circumference of the positive electrode collector 30. For the positive electrode collector 30, a foil of a metal such as aluminum, a film in which the metal is arranged on the surface, etc. can be used. A suitable positive electrode collector 30 is an aluminum foil or an alloy foil with aluminum as the main component. The thickness of the positive electrode collector 30 is, for example, 10 μm to 30 μm.

[0028] On both sides of the positive electrode collector 30, the positive electrode mixture layer 32 is preferably formed in the entire area except for the positive electrode exposed portion 34 described later. The positive electrode mixture layer 32 preferably contains a positive electrode active material, a conductive agent, and a binder. The positive electrode mixture layer 32 is formed by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, a binder, and a solvent such as N-methyl-2-pyrrolidone (NMP) on both sides of the positive electrode collector 30 and drying it (positive electrode mixture layer formation step). Thereafter, the positive electrode mixture layer 32 is compressed.

[0029] Examples of the positive electrode active material include lithium-containing transition metal oxides containing transition metal elements such as Co, Mn, and Ni. The lithium-containing transition metal oxide is not particularly limited, but is preferably a material having the general formula Li 1+x MO 2 (wherein, -0.2<x≤0.2, M contains at least one of Ni, Co, Mn and Al).

[0030] The conductive agent contained in the positive electrode mixture layer 32 may preferably be a carbon material such as carbon black (CB), acetylene black (AB), Ketjen black, or graphite.

[0031] Examples of binders included in the positive electrode mixture layer 32 include fluorine resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide (PI), acrylic resins, polyolefin resins, and the like. When the positive electrode mixture slurry is prepared using an aqueous solvent, styrene butadiene rubber (SBR), nitrile rubber (NBR), CMC or its salt, polyacrylic acid or its salt, polyvinyl alcohol, and the like can be used. As a binder, from the perspective of the flexibility of the positive electrode 11, rubber resins having a molecular structure with repeated double bonds and single bonds, such as SBR and NBR, are preferred. These can be used alone or in combination of two or more. The content of the binder in the positive electrode mixture layer 32 is 0.5% to 10% by mass, preferably 1% to 5% by mass.

[0032] The positive electrode 11 is provided with a positive electrode exposure portion 34 where the surface of the positive electrode current collector 30 is exposed. The positive electrode exposure portion 34 is a portion to which the positive electrode lead 19 is connected, and is a portion of the surface of the positive electrode current collector 30 that is not covered by the positive electrode mixture layer 32. The positive electrode exposure portion 34 is formed wider than the positive electrode lead 19 in the length direction. It is suitable to provide the positive electrode exposure portion 34 on both sides of the positive electrode 11 in a manner overlapping in the thickness direction of the positive electrode 11. The positive electrode lead 19 is joined to the positive electrode exposure portion 34 by, for example, ultrasonic welding.

[0033] Figure 3 In the example shown, a positive electrode exposure portion 34 is provided in the central portion in the longitudinal direction of the positive electrode 11 over the entire length in the belt width direction. The positive electrode exposure portion 34 may also be formed at the starting end or the terminal end of the positive electrode 11, but from the viewpoint of current collection, it is preferably provided at a position approximately equidistant from the starting end and the terminal end. By connecting the positive electrode exposure portion 34 provided at such a position to the positive electrode lead 19, when the electrode body 14 is wound, the positive electrode lead 19 is arranged to protrude upward from the end surface in the belt width direction at the middle position in the radial direction of the electrode body 14. The positive electrode exposure portion 34 is provided by, for example, intermittent coating without coating a portion of the positive electrode current collector 30 with the positive electrode mixture slurry.

[0034] The negative electrode 12 includes a strip-shaped negative electrode collector 40 and negative electrode mixture layers 42 formed on both surfaces of the negative electrode collector 40. For example, a metal foil such as copper or a film having a metal such as copper disposed on the surface layer can be used for the negative electrode collector 40. The thickness of the negative electrode collector 40 is, for example, 5 μm to 30 μm.

[0035] It is suitable that the negative electrode mixture layer 42 is formed on both sides of the negative electrode current collector 40 in the entire region except for the negative electrode exposed portion 44 described later. The negative electrode mixture layer 42 preferably contains a negative electrode active material and a binder. The negative electrode mixture layer 42 is formed by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, and a solvent such as water to both sides of the negative electrode current collector 40 and drying it (negative electrode mixture layer forming step). Thereafter, the negative electrode mixture layer 42 is compressed.

[0036] Figure 3 In the example shown, a negative electrode exposed portion 44 is provided at the beginning of the length direction of the negative electrode 12 over the entire length of the current collector in the width direction. The negative electrode exposed portion 44 is a portion to which the negative electrode lead 20 is connected, and is a portion of the surface of the negative electrode current collector 40 that is not covered by the negative electrode mixture layer 42. The negative electrode exposed portion 44 is formed wider in the length direction than the width of the negative electrode lead 20. It is suitable to provide the negative electrode exposed portion 44 on both sides of the negative electrode 12 in a manner that overlaps in the thickness direction of the negative electrode 12.

[0037] In this embodiment, the negative electrode lead 20 is joined to the inner peripheral surface of the negative electrode current collector 40 by, for example, ultrasonic welding. One end of the negative electrode lead 20 is disposed on the negative electrode exposed portion 44, and the other end extends downward from the lower end of the negative electrode exposed portion 44.

[0038] The negative electrode lead 20 is not limited to the Figure 3 In the example shown, the negative electrode lead 20 may be provided only at the terminal portion of the negative electrode 12. Alternatively, the negative electrode lead 20 may be provided at the beginning and the terminal portion of the negative electrode 12. In this case, the current collection performance is improved. By making the negative electrode exposed portion 44 at the terminal portion of the negative electrode 12 and the outer packaging body 15 (see Figure 1 ), the terminal end of the negative electrode 12 can be electrically connected to the outer package 15 without using the negative electrode lead 20. The negative electrode exposed portion 44 is provided by, for example, intermittent coating of the negative electrode mixture slurry without coating a portion of the negative electrode current collector 40.

[0039] The negative electrode active material is not particularly limited as long as it can reversibly store and release lithium ions. For example, carbon materials such as natural graphite and artificial graphite, metals such as Si and Sn that alloy with lithium, or alloys and oxides containing these materials can be used.

[0040] Examples of binders included in the negative electrode mixture layer 42 include fluorine-based resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide (PI), acrylic resins, polyolefin resins, and the like. When the negative electrode mixture slurry is prepared using an aqueous solvent, styrene butadiene rubber (SBR), nitrile rubber (NBR), CMC or its salt, polyacrylic acid or its salt, polyvinyl alcohol, and the like can be used. As a binder, from the perspective of the flexibility of the negative electrode 12, rubber-based resins such as SBR and NBR having a molecular structure with repeated double bonds and single bonds are preferred. These can be used alone or in combination of two or more. The content of the binder in the negative electrode mixture layer 42 is 0.5% to 10% by mass, preferably 1% to 5% by mass.

[0041] Figure 3 In the figure, the starting end 42a of the negative electrode mixture layer 42 is adjacent to the negative electrode exposed portion 44. On the other hand, the ending end 42b of the negative electrode mixture layer 42 is the same as the ending end of the negative electrode 12. The negative electrode mixture layer 42 exists continuously from the starting end 42a to the ending end 42b.

[0042] Next, refer to Figure 4 (a)~ Figure 4 (d) Yes Figure 3 A change in the content of the binder contained in the negative electrode mixture layer 42 in the longitudinal direction of the negative electrode mixture layer 42 will be described. Figure 4 In (a), the content of the binder decreases at a fixed ratio from the starting end to the terminal end. That is, the content of the binder is high at the starting end 42a of the negative electrode mixture layer 42, where cracks and peeling are prone to occur, and the content of the binder is low at the terminal end 42b, where the winding radius becomes larger than the starting end 42a and cracks and peeling are not prone to occur. As a result, the increase in the internal resistance of the battery caused by the binder contained in the negative electrode mixture layer 42 can be suppressed, and cracks and peeling of the negative electrode mixture layer 42 can be suppressed.

[0043] In addition, if Figure 4 (b) The slope indicating the reduction rate of the adhesive content from the starting end portion 42a to the terminal end portion 42b may not be constant, and the slope may change in the middle. Figure 4 In (c), the content of the adhesive agent decreases from the starting end portion 42a to the terminal end portion 42b, and the content of the adhesive agent is constant between the starting end portion 42a and the terminal end portion 42b. Figure 4 In (d), the content of the adhesive decreases from the starting end 42a to the terminal end 42b, and the content of the adhesive is constant near the starting end 42a. Similarly, if the content of the adhesive decreases from the starting end 42a to the terminal end 42b, the content of the adhesive near the terminal end 42b can be constant. Figure 4 (c) and Figure 4As shown in (d), at least a portion of the negative electrode mixture layer 42 is provided with a region where the content of the binder decreases continuously from the starting end portion 42a side to the terminal portion 42b side. In this region, the content of the binder is preferably reduced linearly, or it may be reduced non-linearly. Thus, the content of the binder at the starting end portion 42a of the negative electrode mixture layer 42 can be higher than the content of the binder at the terminal portion 42b. It should be noted that in the negative electrode mixture layer 42, the binder whose content changes is preferably a rubber-based resin.

[0044] Here, a method for forming a negative electrode mixture layer 42 in which the content of a binder changes from one side of the starting end portion 42a side and the terminal portion 42b side to the other side is described. In order to form such a negative electrode mixture layer 42, it is preferred to use a multilayer die coater. By using a multilayer die coater, it is possible to adjust the coating amount ratio of a plurality of negative electrode mixture slurries with different contents of the binder and apply them to the negative electrode collector 40 at the same time. When the negative electrode mixture slurry is applied to the negative electrode collector 40, the negative electrode collector 40 moves relative to the multilayer die coater. Therefore, by applying a plurality of negative electrode mixture slurries with different contents of the binder to the negative electrode collector 40 while changing their coating amount ratio at a specified time, it is possible to form a region in which the content of the binder changes from the starting end portion 42a side to the terminal portion 42b side at an arbitrary position in the negative electrode mixture layer 42. For example, a first negative electrode mixture slurry and a second negative electrode mixture slurry having a higher binder content than the first negative electrode mixture slurry are prepared. Next, the first and second negative electrode mixture slurries are applied from the starting end 42a to the terminal end 42b of the negative electrode current collector 40 using a multilayer die coater while increasing the coating amount ratio of the first negative electrode mixture slurry to the second negative electrode mixture slurry, thereby obtaining a negative electrode current collector having a Figure 4 (a) shows the negative electrode mixture layer 42 with the distribution curve shown.

[0045] In the above, the case where the content of the binder at the starting end 42a in the negative electrode mixture layer 42 is higher than the content of the binder at the terminal end 42b is described. In the positive electrode mixture layer 32, the content of the binder at the starting end may be higher than the content of the binder at the terminal end. In addition, of course, the content of the binder at the starting end may be higher than the content of the binder at the terminal end in either the positive electrode mixture layer 32 or the negative electrode mixture layer 42. It should be noted that, Figure 3 For the positive electrode 11 shown, when the composite layer is divided into two or more parts by an exposed portion, the content of the binder at the starting end portion can be higher than the content of the binder at the terminal portion. Preferably, a region in which the content of the binder decreases from the starting end portion side to the terminal portion side is formed in at least a portion of the composite layer continuous from the starting end portion.

[0046] Next, refer to Figure 5, while describing the winding radius of the negative electrode 12 near the starting end portion of the negative electrode mixture layer 42 . Figure 5 It is a radial cross-sectional view of the negative electrode 12 in the vicinity of the winding axis 28 of the electrode body 14 as an example of the embodiment. Figure 5 In the figure, the positive electrode 11 and the separator 13 are omitted.

[0047] The winding radius of the innermost circumference of the negative electrode 12 in the electrode body 14 is, for example, 1 mm to 5 mm. The innermost circumference of the negative electrode 12 is the part that goes around from the starting end of the negative electrode 12. The winding radius of the innermost circumference of the negative electrode 12 is determined by the distance R between the winding axis 28 and the negative electrode 12. In order to increase the capacity of the secondary battery 10, it is preferred that R is small, but cracks and peeling are likely to occur in the negative electrode mixture layer 42. However, according to the present invention, since cracks and peeling of the negative electrode mixture layer 42 are suppressed, R is preferably 1 mm to 5 mm. As a result, it is possible to cope with the high capacity of the secondary battery 10. The winding radius of the innermost circumference of the negative electrode 12 can be adjusted by the radius of the winding core used when winding the positive electrode 11, the negative electrode 12 and the separator 13.

[0048] Example

[0049] Hereinafter, the present invention will be further described by way of examples, but the present invention is not limited to these examples.

[0050] [Production of positive electrode]

[0051] 95 parts by mass of LiNi 0.8 Co 0.15 Al 0.05 O 2 , 2.5 parts by mass of acetylene black (AB), 2.5 parts by mass of polyvinylidene fluoride (PVdF) with an average molecular weight of 1.1 million were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry with a solid content of 70% by mass. Next, the positive electrode mixture slurry was applied on both sides of a positive electrode collector in the form of a strip of aluminum foil with a thickness of 15 μm, and the coating was heated to 100°C to 150°C to dry it. After the dried coating was compressed with a roller, it was cut into a specified electrode plate size to produce a positive electrode with a positive electrode mixture layer formed on both sides of the positive electrode collector. In the approximate center of the longitudinal direction of the positive electrode, a positive electrode exposure portion where the mixture layer does not exist and the collector surface is exposed is provided, and an aluminum positive electrode lead is welded to the positive electrode exposure portion.

[0052] [Production of negative electrode]

[0053] 95 parts by mass of graphite, 5 parts by mass of SiO, 1 part by mass of carboxymethyl cellulose (CMC), and 0.8 parts by mass of styrene butadiene rubber (SBR) were mixed, and water was added in an appropriate amount to prepare the first negative electrode mixture slurry. In addition, 95 parts by mass of graphite, 5 parts by mass of SiO, 1 part by mass of carboxymethyl cellulose (CMC), and 1.2 parts by mass of styrene butadiene rubber (SBR) were mixed, and water was added in an appropriate amount to prepare the second negative electrode mixture slurry. Next, the first negative electrode mixture slurry and the second negative electrode mixture slurry were set in a multilayer die coater, and applied on both sides of a strip-shaped negative electrode collector made of copper foil with a thickness of 8 μm, similarly from the starting end to the terminal end, while the coating amount ratio of the first negative electrode mixture slurry to the second negative electrode mixture slurry was continuously changed from 0:1 to 1:0, and then the coating film was dried. The dried coating film is compressed with a roller and cut into a predetermined electrode plate size to produce a positive electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector. A negative electrode exposed portion where no mixture layer is present but the surface of the collector is exposed is provided at the beginning, and a negative electrode lead made of nickel / copper is welded to the negative electrode exposed portion.

[0054] [Preparation of electrolyte]

[0055] 5 parts by mass of vinylene carbonate (VC) were added to 100 parts by mass of a mixed solvent containing ethylene carbonate (EC) and dimethyl carbonate (DMC) (EC:DMC=1:3 by volume ratio). LiPF was dissolved in the mixed solvent to a concentration of 1 mol / L. 6 , thereby preparing the electrolyte.

[0056] [Production of electrode body]

[0057] The positive electrode and the negative electrode were wound around a winding core having a radius of 1 mm via a polyethylene separator to produce an electrode body.

[0058] [Manufacturing of cylindrical secondary batteries]

[0059] Insulating plates are arranged on the upper and lower sides of the electrode body, and the electrode body is contained in the outer packaging body. Next, the negative electrode lead is welded to the bottom of the outer packaging body, and the positive electrode lead is welded to the sealing body. After that, after the electrolyte is injected into the inner part of the outer packaging body by decompression, the opening end of the outer packaging body is riveted to the sealing body through a sealing gasket to seal the cylindrical secondary battery. The capacity of the manufactured battery is 2500mAh.

[0060] <Comparative Example 1>

[0061] An electrode body and a battery were produced in the same manner as in Example, except that only the first negative electrode mixture slurry was applied on both surfaces of the negative electrode current collector without mixing the first negative electrode mixture slurry and the second negative electrode mixture slurry.

[0062] <Comparative Example 2>

[0063] An electrode body and a battery were produced in the same manner as in Example, except that the first negative electrode mixture slurry and the second negative electrode mixture slurry were not mixed and only the second negative electrode mixture slurry was applied on both surfaces of the negative electrode current collector.

[0064] [Evaluation of the presence or absence of cracks in the negative electrode mixture layer]

[0065] The electrode bodies of Example and Comparative Examples 1 and 2 were respectively disassembled and the negative electrodes were unfolded to visually check whether cracks and peeling occurred at the starting end of the negative electrode mixture layer.

[0066] [Measurement of internal resistance]

[0067] The cylindrical secondary batteries of Example and Comparative Examples 1 and 2 were charged at a constant current of 120 mA at a temperature of 25° C. until the battery voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 8 mA. Next, the internal resistance of each battery was measured at 1 kHz by an AC four-terminal method.

[0068] Table 1 shows the evaluation results of Examples and Comparative Examples 1 and 2.

[0069] [Table 1]

[0070] Whether there are cracks Internal resistance Example none 25mΩ Comparative Example 1 have 23mΩ Comparative Example 2 none 37mΩ

[0071] In Comparative Example 1, which used only the first negative electrode mixture slurry with a low binder content, although the internal resistance of the battery was low, cracks occurred in the electrode body. On the other hand, in Comparative Example 2, which used only the second negative electrode mixture slurry with a high binder content, although cracks did not occur in the electrode body, the internal resistance of the battery increased significantly compared to Comparative Example 1. On the other hand, in the embodiment using the first and second negative electrode mixture slurries, cracks did not occur in the electrode body, and the increase in the internal resistance of the battery was suppressed compared to Comparative Example 1. Thus, it was confirmed that by making the binder content at the starting end portion higher than the binder content at the terminal portion, the increase in the internal resistance of the battery caused by the binder used in the electrode is suppressed, and cracks and peeling of the mixture layer are suppressed.

[0072] Description of Reference Numerals

[0073] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 outer packaging body, 16 sealing body, 17, 18 insulating plate, 19 positive electrode lead, 20 negative electrode lead, 21 groove part, 22 filter plate, 23 lower valve body, 24 insulating member, 25 upper valve body, 26 cap, 26a opening, 27 sealing gasket, 28 winding shaft, 30 positive electrode collector, 32 positive electrode mixture layer, 34 positive electrode exposed part, 40 negative electrode collector, 42 negative electrode mixture layer, 44 negative electrode exposed part

Claims

1. A non-aqueous electrolyte secondary battery comprising a wound electrode body in which a strip-shaped positive electrode and a strip-shaped negative electrode are wound with a separator interposed therebetween, and an outer package for accommodating the electrode body, wherein: The positive electrode comprises a positive electrode current collector and a positive electrode mixture layer formed on the positive electrode current collector and containing at least a positive electrode active material and a binder. The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer formed on the negative electrode current collector and containing at least a negative electrode active material and a binder. At least one of the positive electrode mixture layer and the negative electrode mixture layer, in the length direction of the strip-shaped positive electrode and / or the strip-shaped negative electrode, has a higher mass content of the binder at the starting end than at the ending end, the starting end corresponds to the radial inner side of the wound strip-shaped positive electrode and / or the strip-shaped negative electrode, and the ending end corresponds to the radial outer side of the wound strip-shaped positive electrode and / or the strip-shaped negative electrode.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein At least one of the positive electrode mixture layer and the negative electrode mixture layer has a region where the content of the binder continuously decreases from a starting end portion side to a terminal end portion side.

3. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: The innermost winding radius of the negative electrode in the electrode body is 1 mm to 5 mm.

4. A method for manufacturing a nonaqueous electrolyte secondary battery according to any one of claims 1 to 3, comprising a wound electrode body in which a strip-shaped positive electrode and a strip-shaped negative electrode are wound with a separator interposed therebetween, and an outer packaging body for accommodating the electrode body, wherein: include: a positive electrode mixture layer forming step of forming a positive electrode mixture layer containing at least a positive electrode active material and a binder on a positive electrode current collector of the positive electrode; and a negative electrode mixture layer forming step of forming a negative electrode mixture layer containing at least a negative electrode active material and a binder on a negative electrode current collector of the negative electrode; In at least one of the positive electrode mixture layer forming step and the negative electrode mixture layer forming step, a plurality of mixture slurries having different mass contents of the binder are applied while changing their coating amount ratio from one side of the starting end portion to the other side of the ending end portion.

5. The method for manufacturing a non-aqueous electrolyte secondary battery according to claim 4, wherein: The coating amount ratio of the plurality of mixture slurries is changed so that a region in which the content of the binder continuously decreases from the starting end side to the ending end side is formed in at least one of the positive electrode mixture layer and the negative electrode mixture layer.