Vapor phase epitaxial growth method and method for preparing substrate with epitaxial layer

By utilizing the temperature gradient and Si vapor pressure of the SiC container in the TaC container, the rapid and uniform growth of the high-purity SiC epitaxial layer is achieved, and the problems of slow growth rate and non-uniformity in the prior art are solved, and the SiC epitaxial layer is improved. Quality and productivity.

CN114293247BActive Publication Date: 2024-11-05KWANSEI GAKUIN EDUCTIONAL FOUND +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111338480.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-04-28
Filing Date
2017-04-27
Publication Date
2024-11-05
Estimated Expiration
2037-04-27

AI Technical Summary

Technical Problem

Existing SiC epitaxial layer growth methods, such as CVD and seed crystal additive sublimation techniques, have slow growth rates and are not suitable for large-scale production, and may lead to difficulties in forming non-uniformity and high-purity epitaxial layers.

Method used

Using the gas phase epitaxial growth method, the temperature gradient of the SiC container is heated in the TaC container, and the C atoms on the inner surface of the SiC container are bonded to Si atoms to form a high-purity SiC epitaxial layer, and the growth is controlled by the Si vapor pressure of the TaC container. condition.

Benefits of technology

The formation of a SiC epitaxial layer with high purity and uniformity in a short time is achieved, which simplifies the control of the heating device, reduces the manufacturing cost, and improves the quality and growth efficiency of the epitaxial layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114293247B_ABST
    Figure CN114293247B_ABST
Patent Text Reader

Abstract

A SiC container (3) composed of a material containing polycrystalline SiC is contained in a TaC container (2) composed of a material containing TaC, and a base substrate (40) is contained in the SiC container (3), and the TaC container (2) is heated in an environment in which a Si vapor pressure is generated in the TaC container (2) and a temperature gradient is generated. As a result, a single crystal 3C-SiC epitaxial layer (41) is grown on the base substrate (40) by bonding between C atoms sublimated by etching the inner surface of the SiC container (3) and Si atoms in the environment.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is filed on April 27, 2017 、Application No. 201780026022.7(PCT / JP2017 / 016738) 、The name of the invention is Vapor phase epitaxial growth method and method for preparing substrate with epitaxial layer A divisional application for a patent application. Technical Field

[0002] The invention mainly relates to a method for vapor phase growing an epitaxial layer of single crystal SiC on a substrate. Background Art

[0003] In recent years, silicon carbide (SiC) has attracted much attention as a material for semiconductor chips. SiCSiC has excellent mechanical strength and radiation resistance. In addition, SiC has the following characteristics: the valence electrons of electrons and holes can be easily controlled by adding impurities, and it has a wide bandgap (for example, 2.2 eV for 3C-type single crystal SiC), a high breakdown electric field, and a saturated drift rate of electrons. Due to these factors, SiC is expected to become a material for the next generation of power devices, which can achieve high temperature, high frequency, voltage resistance and environmental resistance that cannot be achieved in the existing semiconductor materials. In addition, it has also attracted attention as a substrate for LEDs (light emitting diodes).

[0004] Conventionally, in a method for manufacturing a semiconductor chip using SiC, a method for forming an epitaxial layer is known. Patent Documents 1 and 2 disclose a method for forming an epitaxial layer of SiC.

[0005] In Patent Document 1, a SiC epitaxial layer is formed by a CVD (Chemical Vapor Deposition) method. In the process of growing the epitaxial layer, a defect generation suppression layer whose growth rate is controlled to be less than 1 μm / h is introduced, so that an epitaxial layer with fewer defects can be formed.

[0006] In addition, as another technique for growing an epitaxial layer, the following method is known. That is, the method for forming the epitaxial layer includes a process of growing a bulk crystal of SiC using a seed crystal addition sublimation technique, and a process of liquid phase growing an epitaxial layer on the surface of the bulk crystal. In the process of growing the epitaxial layer, by performing liquid phase growth, micropipe defects propagating from the seed crystal to the bulk crystal substrate can be blocked, thereby forming an epitaxial layer of SiC with fewer micropipe defects.

[0007] [Prior art literature]

[0008] [Patent Document]

[0009] Patent Document 1: Japanese Patent Application Publication No. 2007-284298 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] However, since the growth rate of the CVD method of Patent Document 1 is slow, the processing time will be increased, especially when a relatively thick epitaxial layer is formed. Therefore, not only the manufacturing cost is increased, but also it is not suitable for large-scale production. In addition, when the CVD method is used, since the supply amount of the raw material gas varies depending on the height and location of the substrate, it may cause uneven growth rate in some cases.

[0012] In addition, in the method using the seed crystal addition sublimation technique, since an element for improving the solubility of the molten SiC melt is mixed into the silicon melt in the process of growing the epitaxial layer, there is a concern that the element may be accidentally mixed into the epitaxial crystal, and that heterogeneous polymorphs may be mixed due to the high solvent (carbon) concentration in the silicon melt. Therefore, there is a possibility that a high-purity epitaxial layer cannot be formed.

[0013] The present invention has been accomplished in view of the above circumstances, and its main object is to provide a method for forming an epitaxial layer of high-purity SiC in a short time.

[0014] The technical solutions and effects used to solve the problem

[0015] The problem to be solved by the present invention is as described above, and the means for solving this problem and their effects are described below.

[0016] According to a first aspect of the present invention, the following vapor phase epitaxial growth method is provided. That is, a SiC container composed of a material containing polycrystalline SiC is housed inside a TaC container composed of a material containing TaC, and a base substrate is housed inside the SiC container, and the TaC container is heated in such a manner that the pressure inside the TaC container becomes Si vapor and a temperature gradient is set. As a result, an epitaxial layer growth process of growing an epitaxial layer of single crystal SiC on the base substrate is performed by bonding C atoms sublimated by etching the inner surface of the SiC container with Si atoms in the environment.

[0017] Furthermore, since SiC has excellent heat resistance, the processing temperature can be heated to about 2000°C, so a high-purity SiC epitaxial layer can be formed in a short time. In addition, since the raw material of the epitaxial layer is a SiC container, the epitaxial layer can be grown more uniformly compared to CVD, which introduces raw material gas.

[0018] In the vapor phase epitaxial growth method, it is preferred that the material of the base substrate is an Al compound or a N compound.

[0019] Therefore, by utilizing the method of the present invention, the base substrate is not limited to SiC, and thus a highly versatile epitaxial growth method can be realized.

[0020] In the vapor phase epitaxial growth method, the material of the base substrate may be SiC, and the off angle relative to the <11-20> direction or the <1-100> direction may be 1° or less.

[0021] Thus, when the base substrate is SiC and the off angle is small, the terrace becomes wider, and a high-quality SiC epitaxial layer can be easily formed regardless of the polycrystalline phenomenon of the base substrate.

[0022] In the vapor phase epitaxial growth method, preferably, in the epitaxial layer growth process, the temperature gradient is 2° C. / mm or less.

[0023] Thus, by using the method of the present invention, the pressure of C atoms in the SiC container increases, so that the epitaxial layer can be sufficiently grown even at a low temperature gradient as described above. Therefore, the heating device or heating control can be simplified.

[0024] In the vapor phase epitaxial growth method, preferably, in the epitaxial layer growth process, a plurality of the base substrates are arranged in the SiC container, and the epitaxial layer is grown on each of the plurality of the base substrates.

[0025] Thus, since epitaxial layers can be formed on a plurality of substrates at the same time, the process can be made more efficient. In particular, by using the method of the present invention, epitaxial layers can be formed uniformly regardless of the position in the SiC container, so that the quality will not be reduced.

[0026] In the vapor phase epitaxial growth method, the inner surface of the TaC container is preferably made of Si or a Si compound, and Si atoms are sublimated from the inner surface of the TaC container by heating during the growth of the epitaxial layer, thereby setting the inside of the TaC container to a Si vapor pressure.

[0027] Thus, compared with the method of putting solid Si etc. into the TaC container, the burden on the operator can be reduced. In addition, by forming Si etc. over a wide area on the inner surface of TaC, a uniform Si environment can be achieved.

[0028] In the vapor phase epitaxial growth method, it is preferred that the polycrystalline form of the epitaxial layer is 3C-SiC.

[0029] Alternatively, in the vapor phase epitaxial growth method, the polycrystalline form of the epitaxial layer may also be 4H-SiC or 6H-SiC.

[0030] Thereby, epitaxial layers of various polycrystalline forms can be grown while exerting the effects of the present invention.

[0031] According to a second aspect of the present invention, there is provided a method for producing a substrate with an epitaxial layer, in which the vapor phase epitaxial growth method is used.

[0032] In this way, a substrate with a high-purity epitaxial layer can be prepared efficiently.

[0033] In the method for preparing the substrate with the epitaxial layer, the following method is preferred. That is, the material of the base substrate is SiC. Furthermore, the base substrate is accommodated in the TaC container without penetrating the SiC container, and the base substrate is heated under Si vapor pressure to etch the base substrate.

[0034] Thus, the TaC container can be used not only when forming an epitaxial layer but also when etching. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a schematic diagram showing a high temperature vacuum furnace used in a heating process;

[0036] Figure 2 It is a cross-sectional structural diagram specifically showing a main heating chamber and a preheating chamber of a high-temperature vacuum furnace;

[0037] Figure 3 is a schematic cross-sectional view showing a process of growing an epitaxial layer using a TaC container and a SiC container;

[0038] Figure 4 It is a cross-sectional schematic diagram for explaining the atomic arrangement and stacking period of 3C-SiC single crystal and 4H-SiC single crystal;

[0039] Figure 5 is a diagram illustrating the off-angle of the SiC substrate;

[0040] Figure 6 1 is a diagram showing a state in which an epitaxial layer is grown by configuring SiC containers inside and outside a TaC container;

[0041] Figure 7 1 is a microscope photograph showing the Si surface and the C surface of the epitaxial layer after the SiC container is arranged inside and outside the TaC container;

[0042] Figure 8 Schematic cross-sectional views showing four cases of heat treatment with different treatment conditions (particularly, the distance from the base substrate to the raw material);

[0043] Fig. 9 is a graph showing the relationship between the position of the substrate and the growth rate;

[0044] Fig.10 is a schematic cross-sectional view showing a process of etching using TaC; and

[0045] Fig.11 It is a schematic cross-sectional view showing a state where 3C-SiC epitaxial layers are simultaneously formed on a plurality of substrate substrates. DETAILED DESCRIPTION

[0046] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0047] First, refer to Figures 1 to 3 , illustrating the high-temperature vacuum furnace 11, TaC container 2 and SiC container 3 used in the heat treatment. Figure 1 1 is a schematic diagram showing a high-temperature vacuum furnace 11 used for the heat treatment. Figure 2 It is a cross-sectional view specifically showing the main heating chamber and the preheating chamber of the high-temperature vacuum furnace 11 . Figure 3 1 is a schematic cross-sectional view showing a process of growing an epitaxial layer using the TaC container 2 and the SiC container 3 .

[0048] like Figure 1 and Figure 2 As shown, the high temperature vacuum furnace 11 includes: a main heating chamber 21, which can heat the processed object (substrate substrate, etc.) to a temperature of 1000°C or more and 2300°C or less; and a preheating chamber 22, which can preheat the processed object to a temperature of 500°C or more. The preheating chamber 22 is arranged below the main heating chamber 21 and is adjacent to the main heating chamber 21 in the vertical direction. In addition, the high temperature vacuum furnace 11 has an insulating chamber 23 arranged below the preheating chamber 22. The insulating chamber 23 is adjacent to the preheating chamber 22 in the vertical direction.

[0049] The high temperature vacuum furnace 11 has a vacuum chamber 19, and the main heating chamber 21 and the preheating chamber 22 are arranged inside the vacuum chamber 19. A turbomolecular pump 34 as a vacuum forming device is connected to the vacuum chamber 19, and a vacuum pressure of, for example, 10 -2 Pa or less, preferably 10 -7 A gate valve 25 is provided between the turbomolecular pump 34 and the vacuum chamber 19. In addition, the turbomolecular pump 34 is connected to a rotary pump 26 for auxiliary use.

[0050] The high temperature vacuum furnace 11 has a moving mechanism 27, which can move the object to be processed between the preheating chamber 22 and the main heating chamber 21 in the vertical direction. The moving mechanism 27 includes a support body 28 that can support the object to be processed, and a cylinder part 29 that can move the support body 28 up and down. The cylinder part 29 has a cylinder rod 30, one end of which is connected to the support body 28. In addition, the high temperature vacuum furnace 11 is provided with a vacuum gauge 31 for measuring the vacuum degree and a mass spectrometer 32 for performing mass spectrometry.

[0051] The vacuum chamber 19 is connected to a storage room (not shown) for storing the processed object in advance via a conveying path 65. The conveying path 65 can be opened and closed by a gate valve 66.

[0052] The main heating chamber 21 is formed into an equilateral hexagon in a planar cross-sectional view and is disposed at the upper portion of the inner space of the vacuum chamber 19. Figure 2 As shown, a mesh heater 33 as a heater is provided inside the main heating chamber 21. In addition, a first multi-layer heat-reflecting metal plate 71 is fixed to the side wall or the top plate of the main heating chamber 21, and the heat of the mesh heater 33 is reflected toward the center of the main heating chamber 21 through the first multi-layer heat-reflecting metal plate 71.

[0053] Thus, the following layout is realized in the main heating chamber 21: the mesh heater 33 is arranged in a manner to surround the object to be treated as the heat treatment object, and a multi-layer heat-reflecting metal plate 71 is arranged outside the mesh heater 33. In addition, the mesh heater 33 is configured in a manner that increases in width as it goes up, or the power supplied can be increased as it goes up. Thus, a temperature gradient can be set in the main heating chamber 21. Furthermore, the main heating chamber 21 can be heated to a temperature of, for example, 1000° C. or more and 2300° C. or less.

[0054] The top plate side of the main heating chamber 21 is closed by the first multi-layer heat-reflecting metal plate 71, and on the other hand, a through hole 55 is formed in the first multi-layer heat-reflecting metal plate 71 on the bottom surface. The processed object can move between the main heating chamber 21 and the preheating chamber 22 adjacent to the lower side of the main heating chamber 21 through the through hole 55.

[0055] A part of the support body 28 of the moving mechanism 27 is inserted into the through hole 55. The support body 28 is configured as follows: the second multi-layer heat reflecting metal plate 72, the third multi-layer heat reflecting metal plate 73 and the fourth multi-layer heat reflecting metal plate 74 are arranged in order from the top and spaced from each other.

[0056] The three multi-layer heat-reflecting metal plates 72 to 74 are all arranged horizontally and connected to each other by a column 35 arranged in a vertical direction. In addition, a support platform 36 is arranged in the space between the second multi-layer heat-reflecting metal plate 72 and the third multi-layer heat-reflecting metal plate 73, and a TaC container 2 containing a processed object can be placed on the support platform 36. In the present embodiment, the support platform 36 is made of tantalum carbide.

[0057] A flange is formed at the end of the cylinder rod 30 of the cylinder portion 29, and the flange is fixed to the bottom of the fourth multi-layer heat reflecting metal plate 74. According to this structure, by extending and retracting the cylinder portion 29, the object to be processed on the support table 36 can be moved up and down together with the three multi-layer heat reflecting metal plates 72 to 74.

[0058] The preheating chamber 22 is formed by surrounding the space below the main heating chamber 21 with a plurality of heat-reflecting metal plates 76. The preheating chamber 22 is formed into a circular shape in a planar cross-sectional view. In addition, the preheating chamber 22 does not include a heating mechanism such as the mesh heater 33.

[0059] like Figure 2 As shown, a through hole 56 is formed on the bottom surface of the preheating chamber 22 and on the multi-layer heat-reflecting metal plate 76. In addition, a passage hole 50 is formed on the multi-layer heat-reflecting metal plate 76 forming the side wall of the preheating chamber 22 and at a portion opposite to the conveying path 65. In addition, the high-temperature vacuum furnace 11 has an opening and closing member 51 capable of closing the passage hole 50.

[0060] The heat insulating chamber 23 adjacent to the lower side of the preheating chamber 22 is divided at its upper side by the multi-layer heat reflecting metal plate 76, and at its lower side and side by the multi-layer heat reflecting metal plate 77. The multi-layer heat reflecting metal plate 77 covering the lower side of the heat insulating chamber 23 is provided with a through hole 57 through which the cylinder rod 30 can be inserted.

[0061] A storage recess 58 is formed in the multi-layer heat reflecting metal plate 77 at a position corresponding to the upper end of the through hole 57. The storage recess 58 can store the fourth multi-layer heat reflecting metal plate 74 of the support body 28.

[0062] The multilayer heat reflecting metal plates 71 to 74, 76, and 77 are all made of metal plates (made of tungsten) stacked at predetermined intervals. The portion of the opening and closing member 51 that closes the passage hole 50 also uses a multilayer heat reflecting metal plate of the same structure.

[0063] The material of the multilayer heat-reflecting metal plates 71-74, 76, 77 can be any material as long as it has sufficient heating characteristics for the heat radiation of the mesh heater 33 and has a melting point higher than the ambient temperature. For example, as the multilayer heat-reflecting metal plates 71-74, 76, 77, in addition to the above-mentioned tungsten, high-melting-point metal materials such as tantalum, niobium, and molybdenum can also be selected. In addition, carbides such as tungsten carbide, zirconium carbide, tantalum carbide, hafnium carbide, and molybdenum carbide can also be selected as the multilayer heat-reflecting metal plates 71-74, 76, 77. Moreover, an infrared reflection film composed of gold or tungsten carbide can be further formed on the reflection surface.

[0064] The multi-layer heat reflective metal plates 72 to 74 provided on the support body 28 have a structure in which tungsten plates having a punched metal structure and having a plurality of small through holes are stacked at predetermined intervals while shifting the positions of the through holes.

[0065] Furthermore, the number of stacked layers of the second multi-layer heat reflecting metal plate 72 disposed on the uppermost layer of the support body 28 is smaller than the number of stacked layers of the first multi-layer heat reflecting metal plate 71 of the main heating chamber 21 .

[0066] In this state, the object to be processed is introduced into the interior of the vacuum chamber 19 from the conveying path 65 and placed on the support table 36 in the preheating chamber 22. When the mesh heater 33 is driven in this state, the main heating chamber 21 is heated to a predetermined temperature of 1000°C or more and 2300°C or less (e.g., about 1900°C). At this time, the pressure in the vacuum chamber 19 is adjusted to 10 by driving the turbomolecular pump 34. -3 Pa or less, preferably 10 -5 Below Pa.

[0067] As described above, the number of laminated sheets of the second multi-layer heat-reflecting metal plate 72 of the support body 28 is less than the number of laminated sheets of the first multi-layer heat-reflecting metal plate 71. Therefore, a part of the heat generated by the mesh heater 33 is appropriately supplied (distributed) to the preheating chamber 22 via the second multi-layer heat-reflecting metal plate 72, so that the processed object in the preheating chamber 22 can be preheated to a predetermined temperature of 500° C. or more (e.g., 800° C.). In other words, preheating can be achieved even without providing a heater in the preheating chamber 22, so that a simple structure of the preheating chamber 22 can be achieved.

[0068] After the preheating treatment is performed for a predetermined time, the cylinder 29 is driven to raise the support 28. As a result, the object to be treated moves from the lower side through the through hole 55 into the main heating chamber 21. Thus, the main heating treatment is immediately started, so that the object to be treated in the main heating chamber 21 can be quickly raised to a predetermined temperature (about 1900°C).

[0069] like Figure 3 As shown, the TaC container 2 is a fitting container including an upper container 2a and a lower container 2b, and the upper container 2a and the lower container 2b can fit each other. With this structure, although the internal space of the TaC container 2 is sealed, a small amount of gas atoms can still move from the inside of the TaC container 2 to the outside (and vice versa). In addition, the TaC container 2 is constructed in a manner that can perform the C atom adsorption ion pump function described later when high-temperature treatment is performed under vacuum, and specifically, it is composed of tantalum metal and the tantalum carbide layer is exposed in the internal space.

[0070] More specifically, in the TaC container 2, a TaC layer is formed on a portion of the innermost layer (the layer closest to the object to be processed), and a TaC layer is formed on the outer side of the TaC layer. 2C layer, and tantalum metal as a substrate is formed on the outside thereof. Therefore, as long as the high-temperature treatment is continued under vacuum as described above, the TaC container 2 has the function of continuously adsorbing and capturing carbon atoms from the surface of the tantalum carbide layer. In this sense, the TaC container 2 of this embodiment has a C atom adsorption ion pump function (ion getter function). In addition, Si is supplied to the TaC layer of the innermost layer. As a result, the Si sublimates during the heat treatment to generate Si vapor. In addition, the Si vapor contained in the environment in the TaC container 2 and the C vapor in the C vapor are selectively adsorbed in the TaC container 2, so that the TaC container 2 can be maintained as a high-purity Si environment.

[0071] Furthermore, the supply source of Si is not limited to the structure of supplying Si to the inner wall of the TaC container 2. For example, it can also be supplied from TaC. x Si y (For example, TaSi 2 or 5 Si 3 ) constitutes the inner wall of the TaC container 2, or may be composed of other Si compounds. In addition, solid Si (Si particles) may be arranged inside the TaC container 2.

[0072] The SiC container 3 includes polycrystalline SiC such as 3C-SiC. In the present embodiment, the SiC container 3 is entirely made of SiC. However, as long as the SiC container 3 is structured so that Si vapor and C vapor are generated in the internal space during the heating process, a portion of the SiC container 3 (e.g., the inner surface) may also be made of polycrystalline SiC.

[0073] Similar to the TaC container 2, the SiC container 3 is also a hybrid container including an upper container 3a and a lower container 3b, and the upper container 3a and the lower container 3b can be hybridized with each other. With this structure, although the internal space of the SiC container 3 is sealed, a small amount of gas atoms can still move from the inside of the SiC container 3 to the outside (and vice versa). As a result, the Si vapor generated inside the TaC container 2 moves from the outside of the SiC container 3 to the inside, thereby supplying Si vapor to the internal space of the SiC container 3. In addition, as Figure 3 As shown, since the SiC container 3 is disposed inside the TaC container 2, it is smaller than the TaC container 2. In addition, at least one base substrate 40 is accommodated in the SiC container 3.

[0074] The base substrate 40 is a substrate for forming a bottom layer or a substrate of the epitaxial layer 41. The base substrate 40 may be a SiC substrate or a substrate composed of a material other than SiC (e.g., an Al compound or a N compound). In the case of a SiC substrate, the polycrystalline form may be arbitrary, for example, it may be composed of 3C-SiC, 4H-SiC, or 6H-SiC. Furthermore, in the case of a SiC substrate, the off-angle (refer to Figure 5 ) can be less than 1° or greater than 1°. In addition, the epitaxial layer 41 can be formed on either the Si surface or the C surface of the base substrate 40.

[0075] Next, the epitaxial growth process is described. In this embodiment, a single crystal 3C-SiC epitaxial layer 41 is formed on a base substrate 40 by a vapor phase epitaxial growth method. Specifically, Figure 3 As shown, the base substrate 40 is accommodated in the SiC container 3, and the SiC container 3 is accommodated in the TaC container 2. In addition, the temperature gradient is set in such a way that the upper side of the TaC container 2 (the side where the epitaxial layer 41 is formed) becomes high temperature. The temperature gradient is preferably less than 2°C / mm, and more preferably about 1°C / mm. In this state, the TaC container 2 is heated at a high temperature of 1600°C or more and 2300°C or less.

[0076] By this heating treatment, Si supplied to the inner surface of the TaC container 2 sublimates, and the interior of the TaC container 2 becomes the equilibrium vapor pressure of Si. Even when using another Si source, the interior of the TaC container 2 also becomes the equilibrium vapor pressure of Si by the sublimation of Si. Therefore, since the SiC container 3 is heated at a high temperature under the Si vapor pressure, the SiC container 3 is etched (Si vapor pressure etching). Specifically, the reaction shown below is performed. Simply explained as follows: By heating SiC under the Si vapor pressure, SiC thermally decomposes and chemically reacts with Si to become Si 2 C or SiC 2 In addition, a high C partial pressure is generated inside the SiC container 3 , and the C component is transported to the surface of the base substrate 40 with a temperature gradient of 2° C. / mm or less as a driving force, thereby crystallizing 3C-SiC.

[0077] By performing Si vapor pressure etching on the SiC container 3, the carbonization of the SiC container 3 can be prevented, and the C atoms (or C compounds) can be sublimated from the SiC container 3. As described above, since the TaC container 2 has a C atom adsorption ion pump function, the inside of the TaC container 2 and the outside of the SiC container 3 become a high-purity Si environment. On the other hand, since the inside of the SiC container 3 does not absorb C atoms, it becomes a C environment. In addition, the Si vapor generated by the Si source of the TaC container 2 also enters the inside of the SiC container 3 through the gap between the upper container 3a and the lower container 3b of the SiC container 3. Therefore, the inside of the SiC container 3 is in a Si+C environment. Therefore, by setting a temperature gradient while performing a heat treatment, an epitaxial layer 41 of a single crystal 3C-SiC can be formed on the surface of the base substrate 40 (epitaxial layer growth process). In addition, a substrate with an epitaxial layer can be prepared thereby.

[0078] Here, refer to Figure 4 , briefly explain the molecular arrangement of 4H-SiC and 3C-SiC. Figure 4 As shown in (a), 3C-SiC is composed of Si atoms and C atoms stacked in a way that the height of the monolayer composed of C and Si is 0.25nm. Figure 4 As shown in (b), although the arrangement direction of 4H-SiC is reversed every two molecular layers, the arrangement direction of 3C-SiC is not reversed and is constant.

[0079] Here, by covering the base substrate 40 with the TaC container 2 and the SiC container 3 as described above, the partial pressure of C vapor inside the SiC container 3 can be increased. Therefore, even if the temperature gradient is about 1°C / mm, the epitaxial layer 41 can be fully grown. Furthermore, in the sublimation method known in the past, in order to achieve an effective growth rate, a temperature gradient with a greater height difference is required. However, in order to increase the height difference of the temperature gradient, a precise heating device and fine control are required, which may increase the manufacturing cost. In this regard, in the present embodiment, since the temperature gradient can be less than 2°C / mm, about 1°C / mm, or less than 1°C / mm, the manufacturing cost can be reduced.

[0080] In addition, by growing the epitaxial layer 41 using the method of this embodiment, even if the substrate substrate 40 is not SiC, the epitaxial layer 41 of single crystal 3C-SiC can be formed. In addition, even if the substrate substrate 40 is not 3C-SiC, the epitaxial layer 41 of single crystal 3C-SiC can be formed. SiC can also be grown on 4H-SiC by performing the MBE method (molecular beam epitaxy) and the CVD method (chemical vapor deposition method). However, since the MBE method and the CVD method are not suitable for heat treatment at high temperatures such as above 1600°C, there is an upper limit on the growth rate. On the other hand, although the sublimation method can expect a high growth temperature or a high growth rate, the uniformity within the substrate surface is still a problem. In this regard, in the method of this embodiment, since it is suitable for heat treatment at high temperatures above 1600°C and epitaxial growth of SiC is performed in a quasi-closed system called a Poly-SiC container, the uniformity is high.

[0081] Furthermore, when the off-angle of the SiC substrate is large (for example, greater than 1°), the polycrystalline phenomenon of the base substrate 40 is likely to continue due to the generation of step flow growth, so that 4H-SiC as the epitaxial layer 41 will grow on the base substrate 40, i.e., 4H-SiC. Therefore, when a 3C-SiC epitaxial layer 41 is required, a SiC substrate with a small off-angle (for example, less than 1°) is preferred.

[0082] Secondly, refer to Figure 6 and Figure 7 , an experiment to confirm the effect of housing the SiC container 3 in the TaC container 2 is described. Figure 6 As shown, in this experiment, SiC containers 3 were arranged inside and outside the TaC container 2 , and epitaxial layers 41 were grown on the base substrates 40 inside the respective SiC containers 3 .

[0083] The experimental results are shown in Figure 7 . Figure 7 (a) is a microscopic photograph of the Si surface and the C surface of the epitaxial layer 41 when the SiC container 3 is arranged outside the TaC container 2 and epitaxially grown. Figure 7 (b) is a microscopic photograph of the Si surface and the C surface of the epitaxial layer 41 when the SiC container 3 is arranged inside the TaC container 2 and epitaxial growth is performed. In this way, by arranging the SiC container 3 inside the TaC container 2, the surface of the epitaxial layer 41 becomes flat, and a high-quality epitaxial layer 41 can be formed. In addition, by arranging the SiC container 3 inside the TaC container 2, the growth rate will also be increased by about 5 times. Therefore, by covering the base substrate 40 with the SiC container 3 and the TaC container 2, a high-quality epitaxial layer 41 can be formed at a high speed.

[0084] Secondly, refer to Figure 8 and Fig. 9, which explains the experiment to confirm that the epitaxial layer 41 can be uniformly formed regardless of the position inside the SiC container 3. Figure 8 As shown in FIG. 1 , the experiment was conducted by placing the substrate 40 under various environments, heating it at 1800°C with a temperature gradient of about 1°C / mm, and comparing the growth amount of the epitaxial layer 41. In particular, the experiment was conducted by changing the distance L from the surface of the substrate 40 to the raw material (SiC container 3 or polycrystalline SiC plate 45). Figure 8 (a) and Figure 8 In (b), although one base substrate 40 is housed in one SiC container 3, Figure 8 (c) and Figure 8 In (d), two base substrates 40 are housed in one SiC container 3. Figure 8 Although the TaC container 2 is omitted in the figure, each SiC container 3 is housed in the TaC container 2.

[0085] The experimental results are shown in Fig. 9 . Fig. 9 is for Figure 8 (a) to Figure 8 The base substrate 40 used in (d) establishes a corresponding curve diagram between the distance L from the surface of the base substrate 40 to the raw material and the growth rate of the epitaxial layer 41 formed on the base substrate 40. Fig. 9 As shown in FIG. 1 , all the base substrates 40 have approximately the same growth rate. Therefore, it was confirmed that as long as the temperature gradient is the same, the epitaxial layer 41 can be uniformly formed regardless of the position inside the SiC container 3. Figure 8 (c) and Figure 8 (d) By housing a plurality of base substrates 40 in one SiC container 3 , the epitaxial layer 41 can be efficiently formed.

[0086] like Fig. 9 As shown, the growth rate of the epitaxial layer 41 is 6 to 8 μm / h at 1800°C, which is 6 to 8 times that of the CVD method of Patent Document 1. Furthermore, in the method of this embodiment, since the heating temperature can be set at 1800°C or above, a faster growth rate can be achieved. In addition, by setting the temperature gradient to be much greater than 1°C / mm, a faster growth rate can also be achieved.

[0087] The TaC container 2 of this embodiment can be used not only in the process of forming the epitaxial layer 41, but also in the process of etching the base substrate 40 (SiC substrate). As described above, the TaC container 2 can maintain a high-purity Si environment inside, so Fig.10As shown, by placing the SiC substrate in the TaC container 2 directly (not through the SiC container 3) and heating it at a temperature of 1600°C or higher, the SiC substrate can be etched (the above-mentioned Si vapor pressure etching).

[0088] The etching process can be performed at any time. For example, etching can be performed to flatten a SiC substrate that has been cut from an ingot and mechanically polished (i.e., before the formation of the epitaxial layer 41). Etching can also be performed to flatten an epitaxial layer 41 that has become roughened due to ion (impurity) injection (i.e., after the formation of the epitaxial layer 41).

[0089] In the above description, although single crystal 3C-SiC is grown as epitaxial layer 41 on substrate 40 by accommodating SiC container 3 inside TaC container 2 and accommodating substrate 40 inside SiC container 3 to perform vapor phase epitaxial growth, single crystal 4H-SiC, single crystal 6H-SiC, etc. can also be grown as epitaxial layer 41 on substrate 40 using the same method. In addition, for example, the polycrystalline form of epitaxial layer 41 to be grown can be selected by changing the off-angle and temperature of substrate 40.

[0090] in addition, Fig.11 An embodiment is shown in which a plurality of substrate substrates 40 are housed in one SiC container 3, and these are housed in a TaC container 2. As described above, using the method of the present invention, an epitaxial layer 41 of single crystal 3C-SiC having the same growth rate and quality can be formed regardless of the position of the SiC container 3, so a substrate with an epitaxial layer 41 can be formed efficiently.

[0091] As described above, in the present embodiment, the SiC container 3 composed of a material containing polycrystalline SiC is accommodated in the TaC container 2 composed of a material containing TaC, and the base substrate 40 is accommodated in the SiC container 3, and the TaC container 2 is heated by setting a temperature gradient so that the pressure in the TaC container 2 becomes Si vapor pressure. As a result, the C atoms sublimated by etching the inner surface of the SiC container 3 are bonded with the Si atoms in the atmosphere inside the SiC container 3, and an epitaxial layer 41 of single crystal SiC (3C-SiC, 4H-SiC, 6H-SiC, etc.) is grown on the base substrate 40.

[0092] This allows high-purity single crystal SiC epitaxial layer 41 to be formed at high speed. Also, since the source material of epitaxial layer 41 is SiC container 3, epitaxial layer 41 can be grown more uniformly than by CVD or the like in which source gas is introduced.

[0093] In addition, in the vapor phase epitaxial growth method of this embodiment, the material of the base substrate 40 can also be an Al compound or a N compound, the material of the epitaxial layer 41 can also be SiC, and the deviation angle relative to the <11-20> direction or the <1-100> direction can also be less than 1°.

[0094] Thus, by utilizing the method of the present invention, the base substrate 40 is not limited to SiC, and thus a highly versatile epitaxial growth method can be realized. Thus, when the base substrate 40 is SiC and the off-angle is small, the terrace becomes wider, and regardless of the polycrystalline phenomenon of the base substrate 40, a high-quality single-crystal SiC epitaxial layer can be easily formed.

[0095] In the vapor phase epitaxial growth method of the present embodiment, the temperature gradient is preferably 2° C. / mm or less.

[0096] Thus, by using the method of the present invention, the pressure of C atoms in the SiC container 3 becomes high, so that the epitaxial layer can be sufficiently grown even at a low temperature difference as described above. Therefore, the heating device and heating control can be simplified.

[0097] In the vapor phase epitaxial growth method of the present embodiment, a plurality of base substrates 40 are arranged in the SiC container 3 , and epitaxial layers 41 are grown on each of the plurality of base substrates 40 .

[0098] This makes it possible to simultaneously form epitaxial layers 41 on a plurality of substrates 40, thereby improving processing efficiency. In particular, by using the method of the present invention, epitaxial layers 41 can be uniformly formed regardless of the position in the SiC container 3, so that quality is not reduced.

[0099] In the vapor phase epitaxial growth method of the present embodiment, the inner surface of the TaC container 2 is set to Si or a Si compound, and Si atoms are sublimated from the inner surface of the TaC container 2 by heating during the growth of the epitaxial layer 41, thereby setting the Si vapor pressure inside the TaC container 2.

[0100] This can reduce the burden on the operator compared to a method of injecting solid Si or the like into the TaC container 2. In addition, by forming Si or the like in a wide region on the inner surface of TaC, a uniform Si environment can be achieved.

[0101] Although preferred embodiments of the present invention have been described above, the above configuration can be modified as follows, for example.

[0102] The shapes of the TaC container 2 and the SiC container 3 are arbitrary and can be changed as appropriate. For example, the TaC container 2 and the SiC container 3 may be different shapes or the same (similar) shapes. Figure 8As shown in (d), the TaC container 2 or the SiC container 3 may have a plurality of spaces. In addition, a plurality of SiC containers 3 may be housed in one TaC container 2, and a plurality of substrate substrates 40 may be housed in the SiC container 3 to form an epitaxial layer 41.

[0103] For example, when it is desired to accurately control the growth amount of the epitaxial layer 41 , an inert gas (Ar gas or the like) may be introduced when the epitaxial layer 41 is formed to reduce the growth rate of the epitaxial layer 41 .

[0104] The environment of the internal space of the TaC container 2 and the internal space of the SiC container 3 (especially the partial pressures of Si and C) changes according to the amount of the Si source, the degree of the carbon adsorption function of TaC, the volume of the TaC container 2, the volume of the SiC container 3, etc. Therefore, by changing these conditions, the growth rate and quality of the epitaxial layer 41 can be controlled.

[0105] Description of Reference Numerals

[0106] 2 TaC container

[0107] 2a Upper container

[0108] 2b lower container

[0109] 3 SiC container

[0110] 3a Upper container

[0111] 3b Lower container

[0112] 11 High temperature vacuum furnace

[0113] 40 SiC substrate

[0114] 41 Epitaxial layer

[0115] 45 Polycrystalline SiC board.

Claims

1. A SiC container for a vapor phase epitaxial growth method, characterized in that: In the vapor phase epitaxial growth method, an epitaxial layer growth process is performed. The SiC container is a container heated under Si vapor pressure. The SiC container includes an upper container and a lower container that can be fitted into each other, whereby gas atoms can move from the inside to the outside of the Si container or from the outside to the inside, and Si vapor and C vapor are generated in the internal space during the heating process. In the epitaxial layer growth process, the substrate is accommodated in the inner space of the SiC container which becomes a quasi-closed system during the heat treatment. The outside of the SiC container is formed to have Si vapor pressure, The inner space of the SiC container is formed as a Si+C environment, By setting a temperature gradient and performing a heat treatment, a single crystal SiC epitaxial layer is grown on the base substrate.

2. The SiC container according to claim 1, characterized in that: By placing the container in a TaC container composed of a material containing TaC and heating it, a single crystal SiC epitaxial layer is grown on the base substrate placed in the inner space.

3. The SiC container according to claim 1 or 2, characterized in that: The present invention comprises polycrystalline SiC.

4. A SiC container for a vapor phase epitaxial growth method, characterized in that: The SiC container composed of a material containing polycrystalline SiC is contained in a TaC container composed of a material containing TaC, including an upper container and a lower container that can be fitted with each other, and the substrate is contained in the inner space of the SiC container, which is a quasi-closed system. The TaC container is heated by setting a temperature gradient so that the inside of the TaC container is at Si vapor pressure and the outside of the SiC container is at Si vapor pressure, Gas atoms can move from the inside to the outside of the Si container or from the outside to the inside. Thus, an epitaxial layer growth process of growing an epitaxial layer of single crystal SiC on the base substrate is performed by bonding C atoms sublimated by etching the inner surface of the SiC container with Si atoms supplied by the Si vapor pressure.

5. The SiC container according to claim 4, characterized in that: The utility model comprises an upper container and a lower container which can be fitted with each other.

6. The SiC container according to claim 1 or 4, characterized in that: The structure is capable of accommodating a plurality of the base substrates.