Low temperature lithium battery

By using composite graphite and plant hard carbon as negative electrode materials and nanoscale lithium iron phosphate as positive electrode materials in lithium batteries, and optimizing the electrolyte formula, the problem of poor discharge performance of lithium batteries at low temperatures has been solved and achieved in extremely cold conditions. excellent discharge performance.

CN114373977BActive Publication Date: 2024-10-22HUNAN SHENGLE NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111614161.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-10-22
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

Lithium batteries have poor discharge performance under low temperature conditions, mainly due to the increased viscosity of the electrolyte and the reduced diffusion capacity of lithium ions in the active electrode material, making it almost impossible to discharge.

Method used

Composite graphite and plant hard carbon are used as the negative electrode material, and nanoscale lithium iron phosphate is used as the positive electrode material. Through a specific electrolyte formula, including organic solvents, electrolytic lithium salts and additives, a stable SEI film is designed and the conductivity of the electrode interface is improved. to improve low temperature performance.

Benefits of technology

Significantly improves the discharge performance and power performance of lithium batteries under extremely cold conditions, ensuring that the battery can be effectively discharged in low-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003436461020000111
    Figure BDA0003436461020000111
Patent Text Reader

Abstract

The present invention discloses a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a diaphragm, an electrolyte and a shell. The negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1 to 1.2, the composite graphite is graphite coated with hard carbon, the mass ratio of hard carbon to the graphite is 0.01 to 0.05:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell; the electrolyte is composed of an organic solvent, an electrolytic lithium salt and an additive, the lithium ion concentration of the electrolytic lithium salt is 0.9 to 1.0 mol / L, the mass percentage of the additive is 3% to 4%, and the rest is an organic solvent; the organic solvent comprises ethylene carbonate and propylene carbonate in a mass ratio of 10:1 to 2, the electrolytic lithium salt comprises lithium tetrafluoroborate and lithium dioxalate borate in a mass ratio of 1:1, and the additive comprises vinylene carbonate. The present invention improves the low-temperature discharge performance of the lithium battery by designing reasonable negative and positive electrode materials and electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium battery preparation, and more specifically, to a low-temperature lithium battery. Background Art

[0002] Lithium-ion secondary rechargeable batteries mainly include positive electrode, negative electrode, electrolyte and diaphragm. When charging, lithium ions are embedded in the negative electrode from the positive electrode through the electrolyte and diaphragm. When discharging, lithium ions are released from the negative electrode and move to the positive electrode through the electrolyte and diaphragm. The charging and discharging process of lithium ions is the movement of lithium ions between the positive electrode-negative electrode-positive electrode. However, at low temperatures (below -20°C), due to the increase in electrolyte viscosity and the decrease in the diffusion capacity of lithium ions in the active electrode material, the low-temperature performance of lithium batteries is poor and it is almost impossible to discharge.

[0003] Therefore, there is an urgent need for a lithium battery with excellent discharge performance at low temperatures. Summary of the invention

[0004] An object of the present invention is to solve at least the above problems and to provide at least the advantages which will be described hereinafter.

[0005] Another object of the present invention is to provide a low-temperature lithium battery, which improves the poor discharge performance of the lithium battery under extreme cold conditions and enhances the low-temperature discharge performance of the lithium battery by designing reasonable negative electrode materials, positive electrode materials and electrolytes.

[0006] In order to achieve these purposes and other advantages according to the present invention, the present invention includes a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a casing, characterized in that the negative electrode material of the negative electrode sheet includes composite graphite and plant hard carbon in a mass ratio of 1:1 to 1.2, the composite graphite is graphite coated with hard carbon, the mass ratio of the hard carbon to the graphite is 0.01 to 0.05:1, and the raw material of the plant hard carbon is one of coconut shells and walnut shells.

[0007] Preferably, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate.

[0008] Preferably, the electrolyte consists of an organic solvent, an electrolytic lithium salt and an additive, the lithium ion concentration of the electrolytic lithium salt is 0.9-1.0 mol / L, the mass percentage of the additive is 3%-4%, and the rest is an organic solvent; the organic solvent includes ethylene carbonate and propylene carbonate in a mass ratio of 10:1-2, the electrolytic lithium salt includes lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, and the additive includes vinylene carbonate.

[0009] Preferably, the electrolyte further includes a modifier with a mass percentage of 15% to 20%, and the modifier is composed of an alkyl imidazole and a dissolution promoter in a mass ratio of 1:5 to 10, the alkyl imidazole is one of 2-undecyl imidazole, 2-butyl imidazole, and 4-methyl imidazole, and the dissolution promoter is one of octyl acetate, methyl butyrate, and ethyl propionate.

[0010] Preferably, the alkylimidazole is 2-undecylimidazole, the solubilizing agent is octyl acetate, and the mass ratio of the 2-undecylimidazole to the octyl acetate is 1:8.

[0011] Preferably, the alkyl imidazole is 2-butyl imidazole, the solubilizing agent is ethyl propionate, and the mass ratio of the 2-butyl imidazole to the ethyl propionate is 1:5.

[0012] Preferably, the alkylimidazole is 4-methylimidazole, the solubilizing agent is methyl butyrate, and the mass ratio of the 4-methylimidazole to the methyl butyrate is 1:10.

[0013] The present invention has at least the following beneficial effects:

[0014] The present invention obtains composite graphite by coating hard carbon on graphite, which can reduce the situation of lithium precipitation on the negative electrode surface. At the same time, the composite graphite is mixed with plant hard carbon to prepare the negative electrode material, which can further improve the low temperature and power performance of the lithium battery; by designing ethylene carbonate and propylene carbonate, the combination of the two can improve the situation of negative electrode structure peeling, thereby improving the low temperature performance of the lithium battery; by designing lithium tetrafluoroborate and lithium bis(oxalatoborate), a stable SEI film can be generated at the negative electrode interface; by designing vinylene carbonate, the conductivity and stability of the electrode interface can be improved, thereby improving the low temperature performance of the lithium battery; by designing alkyl imidazole and a dissolution promoter, the alkyl imidazole can be better dissolved in the electrolyte, and the characteristics of the alkyl imidazole itself can improve the low temperature conductivity of the electrolyte, thereby further improving the low temperature discharge performance of the lithium battery.

[0015] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0017] <Example 1>

[0018] The present invention provides a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte and a shell, wherein the negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1, wherein the composite graphite is graphite coated with hard carbon, wherein the mass ratio of the hard carbon to the graphite is 0.01:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell;

[0019] In this embodiment, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate; the hard carbon coated by the composite graphite is common hard carbon, such as resin carbon, organic polymer pyrolytic carbon, etc. Specifically, the hard carbon coated by the composite graphite used in this embodiment is hard carbon prepared by pyrolysis of phenolic resin; the plant hard carbon is coconut shell-based hard carbon;

[0020] The organic solvent of the electrolyte is a mixture of ethylene carbonate and propylene carbonate in a mass ratio of 10:1, the electrolytic lithium salt is a mixture of lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, the additive is vinylene carbonate, the addition amount of the vinylene carbonate is 3%, and the lithium ion concentration of the electrolytic lithium salt is 0.9 mol / L;

[0021] The preparation of the low-temperature lithium battery in this embodiment is as follows:

[0022] Preparation of composite graphite: dissolving phenolic resin in tetrahydrofuran, stirring ultrasonically until dissolved, then adding graphite, stirring until mixed evenly, performing thermal curing in a homogeneous reactor to obtain a mixture, and then pyrolyzing to obtain composite graphite of phenolic resin hard carbon coated graphite, the pyrolysis parameters are: heating from 25°C to 150°C at a heating rate of 4°C / min, keeping warm for 2 hours, then heating to 400°C at a heating rate of 4°C / min and keeping warm for 2 hours, and finally heating to 800°C at a heating rate of 4°C / min and keeping warm for 2 hours, and then cooling to room temperature to obtain composite graphite; the mass ratio of the phenolic resin, the graphite, and the tetrahydrofuran is 2:1:20;

[0023] Preparation of positive electrode sheet: dispersing polyvinylidene fluoride in N-methylpyrrolidone, standing and defoaming after the N-methylpyrrolidone is fully dissolved, then adding conductive carbon black, adding nano-scale lithium iron phosphate after the carbon black is evenly dispersed, and mixing to prepare positive electrode slurry; coating the positive electrode slurry evenly on a positive electrode current collector Al foil with a thickness of 20 μm to obtain a coated electrode sheet, and then placing it at 110° C. and vacuum drying for 12 hours to completely volatilize the solvent in the electrode sheet, and then rolling and cutting to obtain a positive electrode sheet; the mass ratio of the nano-scale lithium iron phosphate, the conductive carbon black, and the polyvinylidene fluoride is 94:3:3;

[0024] Preparation of negative electrode sheet: Sodium carboxymethyl cellulose was dissolved in deionized water (solvent), and then conductive carbon black was added. After the carbon black was evenly dispersed, negative electrode material (composed of composite graphite and coconut shell-based hard carbon in a mass ratio of 1:1) was added, and the solution viscosity was adjusted to 2500 mpa·s. -1 , then add styrene-butadiene rubber, mix evenly to obtain negative electrode slurry; evenly coat the negative electrode slurry on a negative electrode current collector copper foil with a thickness of 10 μm to obtain a coated electrode sheet, and then place it in a vacuum oven at 110° C. for 12 hours to completely evaporate the solvent in the electrode sheet, and then roll and cut the sheet to obtain a negative electrode sheet; the mass ratio of the negative electrode material, the conductive carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber is 95:2:1:2;

[0025] Preparation of electrolyte: In a glove box, weigh the corresponding amount of each formula component, mix them thoroughly, and stir for 2 to 3 days to obtain the electrolyte;

[0026] Diaphragm: Select PE membrane with a thickness of 15 μm and a porosity of 45%;

[0027] Battery assembly: The positive electrode, separator and negative electrode are wound into a battery cell, with the separator located between the positive electrode and the negative electrode. The positive electrode is lead out with an aluminum tab by spot welding, and the negative electrode is lead out with a nickel tab by spot welding. The battery cell is then placed in an aluminum-plastic packaging bag, injected with the above-mentioned electrolyte, and after standing for 12 to 36 hours, it is made into a lithium-ion battery through packaging, formation, capacity and other processes.

[0028] <Example 2>

[0029] The present invention provides a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte and a shell, wherein the negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1, wherein the composite graphite is graphite coated with hard carbon, the mass ratio of the hard carbon to the graphite is 0.05:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell;

[0030] In this embodiment, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate; the hard carbon coated by the composite graphite is common hard carbon, such as resin carbon, organic polymer pyrolytic carbon, etc. Specifically, the hard carbon coated by the composite graphite used in this embodiment is hard carbon prepared by pyrolysis of phenolic resin, and the plant hard carbon is walnut shell-based hard carbon;

[0031] The organic solvent of the electrolyte is a mixture of ethylene carbonate and propylene carbonate in a mass ratio of 10:1, the electrolytic lithium salt is a mixture of lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, the additive is vinylene carbonate, the addition amount of the vinylene carbonate is 3%, and the lithium ion concentration of the electrolytic lithium salt is 0.9 mol / L;

[0032] The preparation of the low-temperature lithium battery in this embodiment is as follows:

[0033] Preparation of composite graphite: dissolving phenolic resin in tetrahydrofuran, stirring ultrasonically until dissolved, then adding graphite, stirring until mixed evenly, performing thermal curing in a homogeneous reactor to obtain a mixture, and then pyrolyzing to obtain composite graphite of phenolic resin hard carbon coated graphite, the pyrolysis parameters are: heating from 25°C to 150°C at a heating rate of 4°C / min, keeping warm for 2 hours, then heating to 400°C at a heating rate of 4°C / min and keeping warm for 2 hours, and finally heating to 800°C at a heating rate of 4°C / min and keeping warm for 2 hours, and then cooling to room temperature to obtain composite graphite; the mass ratio of the phenolic resin, the graphite, and the tetrahydrofuran is 2:1:20;

[0034] Preparation of positive electrode sheet: dispersing polyvinylidene fluoride in N-methylpyrrolidone, standing and defoaming after the N-methylpyrrolidone is fully dissolved, then adding conductive carbon black, adding nano-scale lithium iron phosphate after the carbon black is evenly dispersed, and mixing to prepare positive electrode slurry; coating the positive electrode slurry evenly on a positive electrode current collector Al foil with a thickness of 20 μm to obtain a coated electrode sheet, and then placing it at 110° C. and vacuum drying for 12 hours to completely volatilize the solvent in the electrode sheet, and then rolling and cutting to obtain a positive electrode sheet; the mass ratio of the nano-scale lithium iron phosphate, the conductive carbon black, and the polyvinylidene fluoride is 94:3:3;

[0035] Preparation of negative electrode sheet: Sodium carboxymethyl cellulose was dissolved in deionized water (solvent), and then conductive carbon black was added. After the carbon black was evenly dispersed, negative electrode material (composed of composite graphite and walnut shell-based hard carbon in a mass ratio of 1:1) was added, and the solution viscosity was adjusted to 2500 mpa·s. -1 , then add styrene-butadiene rubber, mix evenly to obtain negative electrode slurry; evenly coat the negative electrode slurry on a negative electrode current collector copper foil with a thickness of 10 μm to obtain a coated electrode sheet, and then place it in a vacuum oven at 110° C. for 12 hours to completely evaporate the solvent in the electrode sheet, and then roll and cut the sheet to obtain a negative electrode sheet; the mass ratio of the negative electrode material, the conductive carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber is 95:2:1:2;

[0036] Preparation of electrolyte: In a glove box, weigh the corresponding amount of each formula component, mix them thoroughly, and stir for 2 to 3 days to obtain the electrolyte;

[0037] Diaphragm: Select PE membrane with a thickness of 15 μm and a porosity of 45%;

[0038] Battery assembly: The positive electrode, separator and negative electrode are wound into a battery cell, with the separator located between the positive electrode and the negative electrode. The positive electrode is lead out with an aluminum tab by spot welding, and the negative electrode is lead out with a nickel tab by spot welding. The battery cell is then placed in an aluminum-plastic packaging bag, injected with the above-mentioned electrolyte, and after standing for 12 to 36 hours, it is made into a lithium-ion battery through packaging, formation, capacity and other processes.

[0039] <Example 3>

[0040] The present invention provides a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte and a shell, wherein the negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1.1, wherein the composite graphite is graphite coated with hard carbon, wherein the mass ratio of the hard carbon to the graphite is 0.01:1, and the raw material of the plant hard carbon is one of wood, coconut shell and walnut shell;

[0041] In this embodiment, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate; the hard carbon coated by the composite graphite is common hard carbon, such as resin carbon, organic polymer pyrolytic carbon, etc. Specifically, the hard carbon coated by the composite graphite used in this embodiment is hard carbon prepared by pyrolysis of phenolic resin; the plant hard carbon is coconut shell-based hard carbon;

[0042] The organic solvent of the electrolyte is a mixture of ethylene carbonate and propylene carbonate in a mass ratio of 10:1, the electrolytic lithium salt is a mixture of lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, the additive is vinylene carbonate, the addition amount of the vinylene carbonate is 3%, and the lithium ion concentration of the electrolytic lithium salt is 0.9 mol / L;

[0043] The preparation of the low-temperature lithium battery in this embodiment is as follows:

[0044] Preparation of composite graphite: dissolving phenolic resin in tetrahydrofuran, stirring ultrasonically until dissolved, then adding graphite, stirring until mixed evenly, performing thermal curing in a homogeneous reactor to obtain a mixture, and then pyrolyzing to obtain composite graphite of phenolic resin hard carbon coated graphite, the pyrolysis parameters are: heating from 25°C to 150°C at a heating rate of 4°C / min, keeping warm for 2 hours, then heating to 400°C at a heating rate of 4°C / min and keeping warm for 2 hours, and finally heating to 800°C at a heating rate of 4°C / min and keeping warm for 2 hours, and then cooling to room temperature to obtain composite graphite; the mass ratio of the phenolic resin, the graphite, and the tetrahydrofuran is 2:1:20;

[0045] Preparation of positive electrode sheet: dispersing polyvinylidene fluoride in N-methylpyrrolidone, standing and defoaming after the N-methylpyrrolidone is fully dissolved, then adding conductive carbon black, adding nano-scale lithium iron phosphate after the carbon black is evenly dispersed, and mixing to prepare positive electrode slurry; coating the positive electrode slurry evenly on a positive electrode current collector Al foil with a thickness of 20 μm to obtain a coated electrode sheet, and then placing it at 110° C. and vacuum drying for 12 hours to completely volatilize the solvent in the electrode sheet, and then rolling and cutting to obtain a positive electrode sheet; the mass ratio of the nano-scale lithium iron phosphate, the conductive carbon black, and the polyvinylidene fluoride is 94:3:3;

[0046] Preparation of negative electrode sheet: Sodium carboxymethyl cellulose was dissolved in deionized water (solvent), and then conductive carbon black was added. After the carbon black was evenly dispersed, negative electrode material (composed of composite graphite and coconut shell-based hard carbon in a mass ratio of 1:1) was added, and the solution viscosity was adjusted to 2500 mpa·s. -1 , then add styrene-butadiene rubber, mix evenly to obtain negative electrode slurry; evenly coat the negative electrode slurry on a negative electrode current collector copper foil with a thickness of 10 μm to obtain a coated electrode sheet, and then place it in a vacuum oven at 110° C. for 12 hours to completely evaporate the solvent in the electrode sheet, and then roll and cut the sheet to obtain a negative electrode sheet; the mass ratio of the negative electrode material, the conductive carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber is 95:2:1:2;

[0047] Preparation of electrolyte: In a glove box, weigh the corresponding amount of each formula component, mix them thoroughly, and stir for 2 to 3 days to obtain the electrolyte;

[0048] Diaphragm: Select PE membrane with a thickness of 15 μm and a porosity of 45%;

[0049] Battery assembly: The positive electrode, separator and negative electrode are wound into a battery cell, with the separator located between the positive electrode and the negative electrode. The positive electrode is lead out with an aluminum tab by spot welding, and the negative electrode is lead out with a nickel tab by spot welding. The battery cell is then placed in an aluminum-plastic packaging bag, injected with the above-mentioned electrolyte, and after standing for 12 to 36 hours, it is made into a lithium-ion battery through packaging, formation, capacity and other processes.

[0050] <Example 4>

[0051] The present invention provides a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte and a shell, wherein the negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1, wherein the composite graphite is graphite coated with hard carbon, wherein the mass ratio of the hard carbon to the graphite is 0.01:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell;

[0052] In this embodiment, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate; the hard carbon coated by the composite graphite is common hard carbon, such as resin carbon, organic polymer pyrolytic carbon, etc. Specifically, the hard carbon coated by the composite graphite used in this embodiment is hard carbon prepared by pyrolysis of phenolic resin; the plant hard carbon is coconut shell-based hard carbon;

[0053] The organic solvent of the electrolyte is a mixture of ethylene carbonate and propylene carbonate in a mass ratio of 10:1, the electrolytic lithium salt is a mixture of lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, the additive is vinylene carbonate, the addition amount of the vinylene carbonate is 3%, and the lithium ion concentration of the electrolytic lithium salt is 0.9 mol / L;

[0054] The electrolyte further includes a modifier with a mass fraction of 18%, wherein the modifier is composed of 2-undecyl and octyl acetate in a mass ratio of 1:8;

[0055] The preparation of the low-temperature lithium battery in this embodiment is as follows:

[0056] Preparation of composite graphite: dissolving phenolic resin in tetrahydrofuran, stirring ultrasonically until dissolved, then adding graphite, stirring until mixed evenly, performing thermal curing in a homogeneous reactor to obtain a mixture, and then pyrolyzing to obtain composite graphite of phenolic resin hard carbon coated graphite, the pyrolysis parameters are: heating from 25°C to 150°C at a heating rate of 4°C / min, keeping warm for 2 hours, then heating to 400°C at a heating rate of 4°C / min and keeping warm for 2 hours, and finally heating to 800°C at a heating rate of 4°C / min and keeping warm for 2 hours, and then cooling to room temperature to obtain composite graphite; the mass ratio of the phenolic resin, the graphite, and the tetrahydrofuran is 2:1:20;

[0057] Preparation of positive electrode sheet: dispersing polyvinylidene fluoride in N-methylpyrrolidone, standing and defoaming after the N-methylpyrrolidone is fully dissolved, then adding conductive carbon black, adding nano-scale lithium iron phosphate after the carbon black is evenly dispersed, and mixing to prepare positive electrode slurry; coating the positive electrode slurry evenly on a positive electrode current collector Al foil with a thickness of 20 μm to obtain a coated electrode sheet, and then placing it at 110° C. and vacuum drying for 12 hours to completely volatilize the solvent in the electrode sheet, and then rolling and cutting to obtain a positive electrode sheet; the mass ratio of the nano-scale lithium iron phosphate, the conductive carbon black, and the polyvinylidene fluoride is 94:3:3;

[0058] Preparation of negative electrode sheet: Sodium carboxymethyl cellulose was dissolved in deionized water (solvent), and then conductive carbon black was added. After the carbon black was evenly dispersed, negative electrode material (composed of composite graphite and coconut shell-based hard carbon in a mass ratio of 1:1) was added, and the solution viscosity was adjusted to 2500 mpa·s. -1, then add styrene-butadiene rubber, mix evenly to obtain negative electrode slurry; evenly coat the negative electrode slurry on a negative electrode current collector copper foil with a thickness of 10 μm to obtain a coated electrode sheet, and then place it in a vacuum oven at 110° C. for 12 hours to completely evaporate the solvent in the electrode sheet, and then roll and cut the sheet to obtain a negative electrode sheet; the mass ratio of the negative electrode material, the conductive carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber is 95:2:1:2;

[0059] Preparation of electrolyte: In a glove box, weigh the corresponding amount of each formula component, mix them thoroughly, and stir for 2 to 3 days to obtain the electrolyte;

[0060] Diaphragm: Select PE membrane with a thickness of 15 μm and a porosity of 45%;

[0061] Battery assembly: The positive electrode, separator and negative electrode are wound into a battery cell, with the separator located between the positive electrode and the negative electrode. The positive electrode is lead out with an aluminum tab by spot welding, and the negative electrode is lead out with a nickel tab by spot welding. The battery cell is then placed in an aluminum-plastic packaging bag, injected with the above-mentioned electrolyte, and after standing for 12 to 36 hours, it is made into a lithium-ion battery through packaging, formation, capacity and other processes.

[0062] <Example 5>

[0063] The present invention provides a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte and a shell, wherein the negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1, wherein the composite graphite is graphite coated with hard carbon, wherein the mass ratio of the hard carbon to the graphite is 0.01:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell;

[0064] In this embodiment, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate; the hard carbon coated by the composite graphite is common hard carbon, such as resin carbon, organic polymer pyrolytic carbon, etc. Specifically, the hard carbon coated by the composite graphite used in this embodiment is hard carbon prepared by pyrolysis of phenolic resin; the plant hard carbon is coconut shell-based hard carbon;

[0065] The organic solvent of the electrolyte is a mixture of ethylene carbonate and propylene carbonate in a mass ratio of 10:1, the electrolytic lithium salt is a mixture of lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, the additive is vinylene carbonate, the addition amount of the vinylene carbonate is 3%, and the lithium ion concentration of the electrolytic lithium salt is 0.9 mol / L;

[0066] The electrolyte further includes a modifier with a mass fraction of 15%, and the modifier is composed of 2-butylimidazole and ethyl propionate with a mass ratio of 1:5;

[0067] The preparation of the low-temperature lithium battery in this embodiment is as follows:

[0068] Preparation of composite graphite: dissolving phenolic resin in tetrahydrofuran, stirring ultrasonically until dissolved, then adding graphite, stirring until mixed evenly, performing thermal curing in a homogeneous reactor to obtain a mixture, and then pyrolyzing to obtain composite graphite of phenolic resin hard carbon coated graphite, the pyrolysis parameters are: heating from 25°C to 150°C at a heating rate of 4°C / min, keeping warm for 2 hours, then heating to 400°C at a heating rate of 4°C / min and keeping warm for 2 hours, and finally heating to 800°C at a heating rate of 4°C / min and keeping warm for 2 hours, and then cooling to room temperature to obtain composite graphite; the mass ratio of the phenolic resin, the graphite, and the tetrahydrofuran is 2:1:20;

[0069] Preparation of positive electrode sheet: dispersing polyvinylidene fluoride in N-methylpyrrolidone, standing and defoaming after the N-methylpyrrolidone is fully dissolved, then adding conductive carbon black, adding nano-scale lithium iron phosphate after the carbon black is evenly dispersed, and mixing to prepare positive electrode slurry; coating the positive electrode slurry evenly on a positive electrode current collector Al foil with a thickness of 20 μm to obtain a coated electrode sheet, and then placing it at 110° C. and vacuum drying for 12 hours to completely volatilize the solvent in the electrode sheet, and then rolling and cutting to obtain a positive electrode sheet; the mass ratio of the nano-scale lithium iron phosphate, the conductive carbon black, and the polyvinylidene fluoride is 94:3:3;

[0070] Preparation of negative electrode sheet: Sodium carboxymethyl cellulose was dissolved in deionized water (solvent), and then conductive carbon black was added. After the carbon black was evenly dispersed, negative electrode material (composed of composite graphite and coconut shell-based hard carbon in a mass ratio of 1:1) was added, and the solution viscosity was adjusted to 2500 mpa·s. -1 , then add styrene-butadiene rubber, mix evenly to obtain negative electrode slurry; evenly coat the negative electrode slurry on a negative electrode current collector copper foil with a thickness of 10 μm to obtain a coated electrode sheet, and then place it in a vacuum oven at 110° C. for 12 hours to completely evaporate the solvent in the electrode sheet, and then roll and cut the sheet to obtain a negative electrode sheet; the mass ratio of the negative electrode material, the conductive carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber is 95:2:1:2;

[0071] Preparation of electrolyte: In a glove box, weigh the corresponding amount of each formula component, mix them thoroughly, and stir for 2 to 3 days to obtain the electrolyte;

[0072] Diaphragm: Select PE membrane with a thickness of 15 μm and a porosity of 45%;

[0073] Battery assembly: The positive electrode, separator and negative electrode are wound into a battery cell, with the separator located between the positive electrode and the negative electrode. The positive electrode is lead out with an aluminum tab by spot welding, and the negative electrode is lead out with a nickel tab by spot welding. The battery cell is then placed in an aluminum-plastic packaging bag, injected with the above-mentioned electrolyte, and after standing for 12 to 36 hours, it is made into a lithium-ion battery through packaging, formation, capacity and other processes.

[0074] <Example 6>

[0075] The present invention provides a low-temperature lithium battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte and a shell, wherein the negative electrode material of the negative electrode plate comprises composite graphite and plant hard carbon in a mass ratio of 1:1, wherein the composite graphite is graphite coated with hard carbon, wherein the mass ratio of the hard carbon to the graphite is 0.01:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell;

[0076] In this embodiment, the positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate; the hard carbon coated by the composite graphite is common hard carbon, such as resin carbon, organic polymer pyrolytic carbon, etc. Specifically, the hard carbon coated by the composite graphite used in this embodiment is hard carbon prepared by pyrolysis of phenolic resin; the plant hard carbon is coconut shell-based hard carbon;

[0077] The organic solvent of the electrolyte is a mixture of ethylene carbonate and propylene carbonate in a mass ratio of 10:1, the electrolytic lithium salt is a mixture of lithium tetrafluoroborate and lithium dioxalatoborate in a mass ratio of 1:1, the additive is vinylene carbonate, the addition amount of the vinylene carbonate is 3%, and the lithium ion concentration of the electrolytic lithium salt is 0.9 mol / L;

[0078] The electrolyte further includes a modifier with a mass fraction of 20%, and the modifier is composed of 4-methylimidazole and methyl butyrate in a mass ratio of 1:10;

[0079] The preparation of the low-temperature lithium battery in this embodiment is as follows:

[0080] Preparation of composite graphite: dissolving phenolic resin in tetrahydrofuran, stirring ultrasonically until dissolved, then adding graphite, stirring until mixed evenly, performing thermal curing in a homogeneous reactor to obtain a mixture, and then pyrolyzing to obtain composite graphite of phenolic resin hard carbon coated graphite, the pyrolysis parameters are: heating from 25°C to 150°C at a heating rate of 4°C / min, keeping warm for 2 hours, then heating to 400°C at a heating rate of 4°C / min and keeping warm for 2 hours, and finally heating to 800°C at a heating rate of 4°C / min and keeping warm for 2 hours, and then cooling to room temperature to obtain composite graphite; the mass ratio of the phenolic resin, the graphite, and the tetrahydrofuran is 2:1:20;

[0081] Preparation of positive electrode sheet: dispersing polyvinylidene fluoride in N-methylpyrrolidone, standing and defoaming after the N-methylpyrrolidone is fully dissolved, then adding conductive carbon black, adding nano-scale lithium iron phosphate after the carbon black is evenly dispersed, and mixing to prepare positive electrode slurry; coating the positive electrode slurry evenly on a positive electrode current collector Al foil with a thickness of 20 μm to obtain a coated electrode sheet, and then placing it at 110° C. and vacuum drying for 12 hours to completely volatilize the solvent in the electrode sheet, and then rolling and cutting to obtain a positive electrode sheet; the mass ratio of the nano-scale lithium iron phosphate, the conductive carbon black, and the polyvinylidene fluoride is 94:3:3;

[0082] Preparation of negative electrode sheet: Sodium carboxymethyl cellulose was dissolved in deionized water (solvent), and then conductive carbon black was added. After the carbon black was evenly dispersed, negative electrode material (composed of composite graphite and coconut shell-based hard carbon in a mass ratio of 1:1) was added, and the solution viscosity was adjusted to 2500 mpa·s. -1 , then add styrene-butadiene rubber, mix evenly to obtain negative electrode slurry; evenly coat the negative electrode slurry on a negative electrode current collector copper foil with a thickness of 10 μm to obtain a coated electrode sheet, and then place it in a vacuum oven at 110° C. for 12 hours to completely evaporate the solvent in the electrode sheet, and then roll and cut the sheet to obtain a negative electrode sheet; the mass ratio of the negative electrode material, the conductive carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber is 95:2:1:2;

[0083] Preparation of electrolyte: In a glove box, weigh the corresponding amount of each formula component, mix them thoroughly, and stir for 2 to 3 days to obtain the electrolyte;

[0084] Diaphragm: Select PE membrane with a thickness of 15 μm and a porosity of 45%;

[0085] Battery assembly: The positive electrode, separator and negative electrode are wound into a battery cell, with the separator located between the positive electrode and the negative electrode. The positive electrode is lead out with an aluminum tab by spot welding, and the negative electrode is lead out with a nickel tab by spot welding. The battery cell is then placed in an aluminum-plastic packaging bag, injected with the above-mentioned electrolyte, and after standing for 12 to 36 hours, it is made into a lithium-ion battery through packaging, formation, capacity and other processes.

[0086] <Comparative Example 1>

[0087] The difference between this comparative example and Example 1 is that the negative electrode material is made of only graphite, and the rest is the same as Example 1.

[0088] <Comparative Example 2>

[0089] The difference between this comparative example and Example 4 is that 2-undecyl imidazole is not added, and the other aspects are the same as Example 4.

[0090] <Comparative Example 3>

[0091] This comparative example is different from Example 4 in that octyl acetate is not added, and the rest is the same as Example 4.

[0092] <Comparative Example 4>

[0093] This comparative example is different from Example 5 in that 2-butylimidazole is not added, and the other aspects are the same as Example 5.

[0094] <Comparative Example 5>

[0095] This comparative example is different from Example 5 in that ethyl propionate is not added, and the rest is the same as Example 5.

[0096] <Comparative Example 6>

[0097] This comparative example is different from Example 6 in that 4-methylimidazole is not added, and the rest is the same as Example 6.

[0098] <Comparative Example 7>

[0099] This comparative example is different from Example 6 in that methyl butyrate is not added, and the rest is the same as Example 6.

[0100] <Low Temperature Discharge Performance Test>

[0101] Method: Charge the battery at room temperature with a current of 0.5C, leave it for 5 minutes, and then discharge it to 2.5V with a current of 0.2C. Record this capacity as C1. Charge the battery again with a current of 0.5C, place it at -20℃ and -40℃ respectively, and start discharging it with a current of 0.2C. Record this capacity as C2 and C3 respectively. C2 represents the capacity at -20℃, and C3 represents the capacity at -40℃. Then:

[0102] The capacity retention rate of the battery at -20°C is: 100%×C2 / C1;

[0103] The capacity retention rate of the battery at -40°C is: 100%×C3 / C1;

[0104] Sample: Take the batteries in Examples 1 to 6 and Comparative Examples 1 to 7 and conduct low-temperature discharge performance tests at -20 and -40°C, respectively. Specific data are shown in Table 1, Table 2, Table 3, and Table 4:

[0105] Table 1 Low temperature discharge performance test data of lithium batteries in Examples 1-3 and Comparative Example 1

[0106] Experimental example -20℃ / 0.2C low temperature discharge capacity retention rate -40℃ / 0.2C low temperature discharge capacity retention rate Example 1 65.5% 58.3% Example 2 66.1% 59.4% Example 3 64.8% 58.7% Comparative Example 1 48.2% 40.1%

[0107] It can be seen from the data in Table 1 that the 0.2C low-temperature discharge capacity retention rates of the batteries prepared in Examples 1 to 3 at -20°C and -40°C are higher than those of the battery prepared in Comparative 1. The negative electrode materials in Examples 1 to 3 are prepared by mixing composite graphite and plant hard carbon, wherein the composite graphite is graphite coated with phenolic resin hard carbon. Since phenolic resin hard carbon has better low-temperature performance, it can effectively improve the lithium precipitation on the negative electrode surface, thereby improving the low-temperature discharge performance of the battery.

[0108] Table 2 Low temperature discharge performance test data of lithium batteries in Example 1, Example 4 and Comparative Examples 2-3

[0109]

[0110]

[0111] As can be seen from Table 2, by comparing Example 4 with Example 1 and Comparative Example 2, it can be seen that the low-temperature discharge performance of the battery prepared after adding 2-undecyl imidazole is greatly improved, and by comparing Example 4 with Comparative Example 3, it can be seen that after adding the chaotropic agent octyl acetate, octyl acetate can improve the solubility of 2-undecyl imidazole in the electrolyte, thereby significantly improving the low-temperature discharge performance of the battery.

[0112] Table 3 Low temperature discharge performance test data of lithium batteries in Example 1, Example 5 and Comparative Examples 4-5

[0113] Experimental example -20℃ / 0.2C low temperature discharge capacity retention rate -40℃ / 0.2C low temperature discharge capacity retention rate Example 5 84.4% 78.3% Example 1 65.5% 58.3% Comparative Example 4 66.4% 58.8% Comparative Example 5 72.1% 66.4%

[0114] As can be seen from Table 3, by comparing Example 5 with Example 1 and Comparative Example 4, it can be seen that the low-temperature discharge performance of the battery prepared after adding 2-butylimidazole is greatly improved, and by comparing Example 4 with Comparative Example 5, it can be seen that after adding the chaotropic agent ethyl propionate, ethyl propionate can improve the solubility of 2-butylimidazole in the electrolyte, thereby improving the low-temperature discharge performance of the battery.

[0115] Table 4 Low temperature discharge performance test data of lithium batteries in Example 1, Example 6 and Comparative Examples 6-7

[0116] Experimental example -20℃ / 0.2C low temperature discharge capacity retention rate -40℃ / 0.2C low temperature discharge capacity retention rate Example 6 86.1% 78.6% Example 1 65.5% 58.3% Comparative Example 4 65.2% 59.1% Comparative Example 5 73.4% 65.9%

[0117] As can be seen from Table 4, by comparing Example 6 with Example 1 and Comparative Example 6, it can be seen that the low-temperature discharge performance of the battery prepared after adding 4-methylimidazole is greatly improved, and by comparing Example 4 with Comparative Example 7, it can be seen that after adding the solubilizing agent methyl butyrate, methyl butyrate can increase the solubility of 4-methylimidazole in the electrolyte, thereby improving the low-temperature discharge performance of the battery.

[0118] In general, from the data in Table 2, Table 3, and Table 4, it can be seen that the discharge performance of the lithium battery at low temperatures can be effectively improved by adding alkyl imidazole and a dissolution promoter. This is because the alkyl imidazole itself is a bipolar organic molecule, which can lose an electron and be oxidized, and can also gain an electron and be reduced. Therefore, it can react at the positive and negative electrodes at the same time, thereby increasing the transfer rate of electrons at the positive and negative electrodes, thereby increasing the reaction rate of lithium ions at the positive and negative electrodes, and thus improving the discharge performance of the lithium battery at low temperatures. Overall, the lithium battery of the present invention has excellent low-temperature discharge performance.

[0119] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown and described herein.

Claims

1. Low-temperature lithium battery, including positive electrode sheet, negative electrode sheet, diaphragm, electrolyte and shell, It is characterized in that The negative electrode material of the negative electrode plate includes composite graphite and plant hard carbon in a mass ratio of 1:1 to 1.2, wherein the composite graphite is graphite coated with hard carbon, the mass ratio of the hard carbon to the graphite is 0.01 to 0.05:1, and the raw material of the plant hard carbon is one of coconut shell and walnut shell; the hard carbon coated by the composite graphite is hard carbon prepared by pyrolysis of phenolic resin; The electrolyte is composed of an organic solvent, an electrolytic lithium salt and an additive. The lithium ion concentration of the electrolytic lithium salt is 0.9-1.0 mol / L, the mass percentage of the additive is 3%-4%, and the rest is an organic solvent; the organic solvent comprises ethylene carbonate and propylene carbonate in a mass ratio of 10:1-2, the electrolytic lithium salt comprises lithium tetrafluoroborate and lithium dioxalate borate in a mass ratio of 1:1, and the additive comprises vinylene carbonate; The electrolyte further comprises a modifier in an amount of 15% to 20% by mass, wherein the modifier is composed of an alkyl imidazole and a dissolving agent in a mass ratio of 1:5 to 10; Wherein, the alkyl imidazole is 2-undecyl imidazole, the solubilizing agent is octyl acetate, and the mass ratio of the 2-undecyl imidazole to the octyl acetate is 1:8; Or, the alkyl imidazole is 2-butyl imidazole, the solubilizing agent is ethyl propionate, and the mass ratio of the 2-butyl imidazole to the ethyl propionate is 1:5; Alternatively, the alkylimidazole is 4-methylimidazole, the solubilizing agent is methyl butyrate, and the mass ratio of the 4-methylimidazole to the methyl butyrate is 1:

10.

2. The low-temperature lithium battery according to claim 1, It is characterized in that The positive electrode material of the positive electrode plate is nano-scale lithium iron phosphate.