Arc additive component performance control method based on ultrasonic impact processing and its application
By using impact needles with specific composition and hardness for ultrasonic impact treatment during the arc additive manufacturing process, oxides are formed to recrystallize and refine grains, which solves the problems of structural defects and residual stress in arc additive manufacturing and significantly improves the efficiency of arc additive manufacturing. Mechanical properties and toughness of components.
Patent Information
- Application Number
- CN202111593211.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-12-23
AI Technical Summary
Common structural defects and residual stress problems in arc additive manufacturing affect the comprehensive mechanical properties of components, resulting in insufficient service life and reliability.
In the arc additive manufacturing process, impact needles with specific composition and hardness are used for ultrasonic impact treatment to form oxides to promote material recrystallization, grain refinement and acicular ferrite formation, and arc additive manufacturing is performed simultaneously to enhance components. mechanical properties.
Through ultrasonic impact treatment, the material recrystallizes and the structure is homogenized, the void defects are bridged, and the formation of acicular ferrite is promoted, which significantly improves the comprehensive mechanical properties of the component, especially the toughness and stress corrosion resistance.
Smart Images

Figure CN114473135B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of arc additive manufacturing, and in particular to an arc additive component performance control method based on ultrasonic impact processing and an application thereof. Background Art
[0002] Wire+Arc Additive Manufacturing (WAAM) uses welding arc as heat source and metal wire as raw material for additive manufacturing. It has the characteristics of high cladding rate, low material and equipment consumption, good structural integrity, etc. It can effectively make up for the shortcomings of forging and casting technology in the manufacturing of more complex structural parts and has broad application prospects. However, arc additive manufacturing often has the following shortcomings: 1. The crystallization of arc additive manufacturing molten pool metal is generally based on nucleation at the edge of solidified metal and epitaxial growth, so columnar crystals are mainly in the molten pool, while the heat source of arc additive manufacturing is generally a high-energy point heat source. The arc heats the material locally and moves to work, causing local materials to heat rapidly and cool rapidly. The liquid metal in the molten pool has a large temperature gradient during the crystallization process. It provides more favorable conditions for the growth of columnar crystals, so it is easier to form coarse columnar crystals in the molten pool, which in turn affects the comprehensive mechanical properties of arc additive manufacturing components. 2. The metal regions of arc additive manufacturing undergo multiple unbalanced thermal cycles, resulting in large residual stresses and complex stress states. 3. During the arc additive manufacturing process, the molten pool metal solidifies in a free state without plastic processing such as forging or rolling, so "void" defects such as pores and unfused metals are prone to appear in the solidified metal. These defects are important factors affecting the service life of arc additive components. Therefore, reducing or eliminating various structural defects of arc additives and regulating their residual stress levels are of great significance to improving the comprehensive mechanical properties of arc additive components and ensuring the quality and service reliability of components.
[0003] At present, there are mechanical treatment methods to improve the organization and reduce defects of metal components manufactured by arc additive manufacturing, such as rolling the weld, ultrasonic impact treatment with steel needles or carbide needles; temperature control methods such as using water cooling, liquid carbon dioxide and other medium forced cooling methods during printing to allow the components to cool quickly to reduce the tendency of grain growth. As for ultrasonic impact treatment, current research mostly uses ultrasonic treatment to cause plastic deformation of components, thereby bridging "void" defects such as pores and unfused. For example, Chinese patent CN108067705A provides a CMT-ultrasonic impact composite additive manufacturing method, which performs ultrasonic impact treatment while arc additive manufacturing to cause plastic deformation of the component surface, thereby reducing the number and volume of pores in the formed component. For example, Chinese patent CN111687553A provides a method for improving the residual stress distribution of arc additive manufacturing structural parts by ultrasonic impact, which performs ultrasonic impact treatment at the weld of residual stress to eliminate residual stress.
[0004] Acicular ferrite (AF) in austenite is a kind of interlocking structure with fine needle-like distribution and large-angle grain boundaries. This structure has good strength and toughness and good fracture resistance. It can improve the strength and toughness of steel, and enhance the steel's resistance to cleavage fracture, thereby significantly improving the stress corrosion resistance and hydrogen embrittlement resistance of metal materials and components. The higher the acicular ferrite content in the component, the better its comprehensive performance. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for controlling the performance of arc additive components based on ultrasonic impact treatment, which can improve the comprehensive mechanical properties of the components.
[0006] In order to solve the above problems, the present invention discloses a method for controlling the performance of arc additive components based on ultrasonic impact treatment, wherein an impact with a specific composition and hardness is used to perform ultrasonic impact treatment on the formed components during arc additive manufacturing;
[0007] The impact needle contains one or more of the following elements: Ti, Al, V, Mg, Ca, Mn, Si, Ni, Mo, Zr; the temperature of the component surface before ultrasonic impact treatment is 150-300°C;
[0008] The hardness of the impact needle is less than or equal to the hardness of the component metal, so that the impact needle element forms an oxide on the layered surface of the component under the ultrasonic impact oxidation effect. The oxide melts simultaneously with the metal used in the component during the subsequent printing process to form a molten pool, and undergoes a metallurgical reaction with the molten pool to form tiny granular oxides, thereby affecting the metal crystallization mode and solid-state phase change.
[0009] The present invention performs ultrasonic impact treatment on the solidified metal during arc additive manufacturing, which has three functions:
[0010] The first is to induce recrystallization of the material, refine the grains, and homogenize the structure. Specifically, the impact needle of the ultrasonic impact treatment continuously impacts the metal manufactured by the arc additive manufacturing with a certain intensity, causing the material in the impact area of the arc additive manufacturing metal to undergo plastic deformation, causing the lattice to be distorted, the grains to be broken, and causing the solidified metal to undergo plastic deformation, with a certain amount of plastic energy storage, providing conditions for the solidified metal to recrystallize under the subsequent arc additive manufacturing thermal cycle, further refining the grains, homogenizing the structure, and improving the comprehensive mechanical properties of the material.
[0011] Secondly, the material in the area impacted by the arc-assisted metal undergoes plastic deformation, which has a forging effect in a small area and fills the void-like defects in the printed metal.
[0012] Third, through the oxidation effect of ultrasonic impact treatment, spherical oxides are formed that are conducive to the nucleation of needle-shaped ferrite, which promotes the formation of needle-shaped ferrite in the crystal, thereby improving the comprehensive mechanical properties of the material. Specifically, the hardness of the impact needle used in the present invention is equal to or less than the hardness of the metal component manufactured by arc additive manufacturing, so that the tip of the impact needle is broken under the action of ultrasonic impact, forming small particles and oxides. In the subsequent printing process, this type of oxide is melted together with the surface additive metal to form a molten pool, and undergoes metallurgical reactions to form tiny oxide particles of specific composition and size. These oxide particles become nucleating agents for needle-shaped ferrite, promote the nucleation of needle-shaped ferrite in austenite crystals, and finally form needle-shaped ferrite in many different grain boundary directions, thereby improving the comprehensive mechanical properties of the material. When ultrasonic impact treatment and arc additive manufacturing are carried out simultaneously, ultrasonic vibration has a stirring effect on the liquid metal in the molten pool, further refining the grains.
[0013] That is, the present invention applies the mechanical strengthening effect, oxidation effect and element transfer effect of ultrasonic impact treatment to the arc additive manufacturing process, effectively improving the comprehensive mechanical properties of the manufactured components.
[0014] Specifically, in one embodiment of the present invention, when the length of the same track during the component printing process is greater than 1m and there is no repeated path on the same track, arc additive manufacturing and ultrasonic impact treatment are performed simultaneously. That is, the arc is in front and the ultrasonic impact gun follows closely. Specifically, the distance between the two is calculated according to the following formula:
[0015] L=T·v
[0016] Wherein, L is the distance between the electric melting head and the ultrasonic impact head, T is the time required for the component to cool in layers to 150-300°C, and v is the speed at which the electric melting head moves.
[0017] Specifically, in one embodiment of the present invention, when the length of the same track during the component printing process is less than 1m, or when the path is repeated during the component printing process, an arc additive manufacturing is first used to complete a layer of metal, and then ultrasonic impact treatment is used. That is, after printing a layer of metal, the printing is paused, and the ultrasonic impact treatment of the layer of metal is started. After the impact treatment is completed, the additive manufacturing is restarted to start additive manufacturing of the next layer of metal.
[0018] Specifically, in one embodiment of the present invention, during the ultrasonic impact treatment, the moving speed of the ultrasonic impact gun is 0.5 to 3 m / min, and the impact intensity is 1 to 3 s / mm 2, the impact frequency is 100-200 Hz, the power of the ultrasonic impact gun power supply is 300W-1500W, and the frequency is 15-35kHz. It should be noted that the specific process parameters of the ultrasonic impact treatment in the present invention are not limited to the above ranges, and those skilled in the art can adjust the parameters of the ultrasonic impact treatment according to the material, size, layering parameters, etc. of the printed component.
[0019] Specifically, in one embodiment of the present invention, the impact needle is an overall cylindrical, conical or cylindrical with a flat tip, but not limited thereto. Preferably, it is a conical or cylindrical with a flat tip. The length of the impact needle is 30 to 50 mm, but not limited thereto; the diameter of the impact needle is 3 to 4 mm (cylindrical diameter, for cylindrical shape; conical diameter, for conical shape, for the bottom surface of the cone), but not limited thereto.
[0020] Specifically, in one embodiment of the present invention, when the metal used in the component contains Mn, the impact needle contains Ti, Al, and V. This type of impact needle is subjected to ultrasonic impact treatment, which easily forms Ti oxides (TiO, Ti2O3) and Al2O3, and these oxides easily allow the nucleation of acicular ferrite. Among them, the mismatch between TiO and ferrite is small, and the crystal structure is similar, so it is easy to nucleate. Under the condition of containing Mn, Ti2O3 has an adsorption effect on Mn, resulting in a local Mn-poor area, which increases the driving force of the transformation of acicular ferrite, thereby becoming an effective nucleation point. The composite oxide of Al2O3 and MnO (MnO·Al2O3) provides an effective nucleation point for acicular ferrite. The composite phase of MnS+V(C, N) can nucleate acicular ferrite. MnS, CaO particles or other particles wrapped by MnS have the effect of inducing the formation of acicular ferrite. Al2O3·CuS has the ability to induce the nucleation of intracrystalline ferrite. TiO x -MnS type composite particles can remain stable at high temperatures and do not dissolve during the reheating process of multiple thermal cycles, providing conditions for the phase transformation process to induce the nucleation of intragranular acicular ferrite.
[0021] Specifically, the metal used for the component in the present invention can be a common printing metal used for arc additive manufacturing in the art, such as carbon steel and low alloy steel, specifically, Mn-Ni-Mo series materials manufactured by arc additive manufacturing, such as 08MnNiMo, 08Ni1MnMo, etc.; Cr-Mo series materials, such as 12Cr1MoV, 12Cr2Mo, 15CrMo, etc.; carbon steel series, such as 45 steel, Q345, Q690, etc. But not limited to this. The impact needle used in the present invention can be made of titanium alloy, and its exemplary chemical composition is Al6%, V 4%, Ti 90%, but not limited to this.
[0022] Correspondingly, the present invention also discloses the application of the above-mentioned arc additive component performance control method based on ultrasonic impact treatment in arc additive manufacturing, arc welding, and surfacing component preparation.
[0023] The implementation of the present invention has the following beneficial effects:
[0024] The present invention performs ultrasonic impact treatment during arc additive manufacturing, which can induce recrystallization of the material, refine the grains, and homogenize the structure. It can also be beneficial to the formation of spherical oxides for the nucleation of acicular ferrite, promote the formation of acicular ferrite within the crystal, and thus improve the comprehensive mechanical properties of the material, especially the toughness. At the same time, the material in the arc additive metal impact area undergoes plastic deformation, has a forging effect in a small area, and fills the void defects in the printed metal. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the component manufacturing process, ultrasonic impact treatment process and sample product in Test Example 1 of the present invention;
[0026] Figure 2 1 is a microstructure morphology diagram (×500) of the component in Experimental Example 1 of the present invention, wherein (a) is an area treated with ultrasonic impact, and (b) is an area not treated with ultrasonic impact;
[0027] Figure 3 This is a tissue diagram (electron microscope diagram) of the area treated by ultrasonic impact in Experimental Example 1 of the present invention;
[0028] Figure 4 is a punching shear yield strength diagram of each sampling position in Test Example 1 of the present invention;
[0029] Figure 5 is a punching shear strength diagram of each sampling position in Test Example 1 of the present invention;
[0030] Figure 6 is an equivalent yield ratio diagram of each sampling position in Test Example 1 of the present invention;
[0031] Figure 7 is a fracture morphology diagram of the A4 position in Experimental Example 1 of the present invention;
[0032] Figure 8 This is the EDS component analysis position point diagram of position A4 in Experimental Example 1 of the present invention. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0034] Test Example 1
[0035] In order to demonstrate the improved effect of the manufacturing method in this application, the following experiments were conducted:
[0036] 1. Experimental Methods
[0037] Arc additive manufacturing was used to prepare a W50×H50×L500 (mm) sample, and AWS A5.23F9A / P4-EF1-F1 welding wire (diameter 4.0 mm) was selected for arc additive manufacturing.
[0038] The process parameters for arc additive manufacturing are as follows:
[0039] The current is 600A, the voltage is 32V, the arc moving speed is 700mm / min, the width of each cladding pass is 18mm, and the thickness of the single-layer cladding is 1.8mm.
[0040] Based on the shape and size of the sample (block-shaped), the additive manufacturing trajectory is formulated as interlayer reciprocating. In view of the fact that the additive manufacturing trajectory is reciprocating and it is intermittent additive manufacturing, the sample is prepared by additive manufacturing one layer and impacting one layer.
[0041] Specifically, a titanium alloy impact needle (Ti6Al4V) was used to perform local ultrasonic impact treatment on the arc-reinforced high-strength steel sample, and the impact area width was about 20×60mm. The impact strength was 1.33s / mm 2 . An impact head with four impact needles is used, and the needle diameter is 4mm. During the impact, the impact gun is held and the impact is maintained uniformly. In order to compare and analyze the effect of ultrasonic impact treatment on thickness, the entire sample thickness is layered for 3 times, and the thickness of each treatment is about 10mm (3-4 layers of cladding thickness). After the additive manufacturing is completed, the sample is impacted in three areas of the surface during the cooling process (the temperature is controlled at 150-300℃) to compare the effect of ultrasonic oxidation treatment under different temperature conditions. The sample manufacturing process, ultrasonic impact treatment photos and sample finished products are shown in the figure. Figure 1 shown.
[0042] 2. Test results
[0043] (I) Microstructure and chemical composition
[0044] Select the ultrasonic impact treated area and the untreated area to observe the microstructure of the two areas. The results of observation under optical microscope are shown in Figure 2 As shown in the figure, it can be seen that the grains in the ultrasonic impact treated area are finer than those in the unimpact treated area, and the amount of acicular ferrite (AF) in the treated area is more than that in the untreated area.
[0045] The structure of the area treated by ultrasonic impact was observed by scanning electron microscopy. Figure 3 shown. Figure 3It can be seen that the main structures in this area are acicular ferrite (AF) and martensite-austenite islands (M / A islands). The nucleation particles of acicular ferrite are spherical particles. The components that have not been treated with ultrasonic impact were tested, and their chemical compositions are shown in Table 1. The spherical particles are multi-element oxides, among which the contents of O and Al are relatively high, and they also contain a small amount of Ti, Si and Mn elements. Comparing the composition of the spherical oxides with the composition of the components that have not been treated with ultrasonics shown in Table 1, it can be seen that the Al and Ti elements are transferred from the impact needle to the additive component (the welding wire and the cladding metal do not contain Al and Ti elements). Under the oxidation effect of ultrasonic impact treatment, oxides are generated, and spherical oxides that are beneficial to the nucleation of acicular ferrite are formed in the metallurgical reaction of the molten pool.
[0046] Table 1 Chemical composition of the area not treated with ultrasonic impact (wt.%)
[0047] C Si Mn P S Cr Mo 0.081 0.33 1.5 0.0052 0.0031 0.013 0.57 Ni Nb V Ti Cu B Al 1.36 0.0016 0.0049 0.0078 0.0064 0.0004 0.022
[0048] Table 2 Figure 3 Element composition of spherical particles at point A (wt.%)
[0049] O Al Si Ti Mn Fe 40.36 9.91 2.48 0.33 1.78 Bal.
[0050] (II) Mechanical properties and fracture morphology of ultrasonic impact treated and untreated areas
[0051] 2.1 Mechanical properties analysis
[0052] The punching shear yield strength, punching shear strength and equivalent yield strength ratio (punching shear yield strength / punching shear strength) of the micro-punching shear test were plotted after three tests at each test point in two locations and the average value was taken. Figures 4 to 6 As shown, A represents the ultrasonic impact treated area and B represents the untreated area. For specific test methods, see "Study on the Effect of Ultrasonic Impact Treatment on the Mechanical Properties of Multi-Pass Welding Seams of High-Strength Steel", Petroleum Pipes and Instruments, December 2020)
[0053] Since positions A and B are located on the same additive manufacturing path, the processes at the two positions are the same and the thermal cycles they experience are also consistent. Positions A1, A2 and A4 are ultrasonic impact treated positions, and the corresponding points B1, B2 and B4 are untreated positions. Figure 4 , Figure 5 It can be seen that the punching shear strength and punching shear yield strength at positions A1, A2 and A4 are lower than those at untreated positions B1, B2 and B4, that is, ultrasonic impact treatment reduces the punching shear yield strength. Figure 6 It can be seen that the equivalent yield strength ratio of the ultrasonic impact treatment position is lower than that of the untreated area, indicating that the ultrasonic impact treatment has the effect of increasing the plastic reserve of the additive sample, which is beneficial to ensure the overload safety of the component obtained by this manufacturing method.
[0054] 2.2 Fracture morphology analysis
[0055] The fracture of the 4th test point of the punching and shearing specimen at position A (ultrasonic impact treatment position) was analyzed by scanning electron microscope. Figure 7 shown.
[0056] Depend on Figure 7 It can be seen that the fracture form of the punching and shearing specimen is ductile fracture, and the microscopic morphology of the fracture is mainly dimples. A number of larger particles with a size of 0.2 to 0.5 μm appear in the fracture. These small particles affect the mechanical properties of the additive specimen and are particles for grain growth and nucleation, affecting the grain size and phase composition of the specimen.
[0057] Select the characteristic points on the fracture surface (such as Figure 8 The composition of each point was tested by EDS, as shown in Table 3.
[0058] Table 3 Element contents at various positions on the fracture surface of micro-punching shear specimens (mass percentage wt%)
[0059]
[0060] As shown in Table 3, the content of O in the oxide particles is relatively high, and the contents of Al, Si, Ti, and Mn are significantly higher than the corresponding elements in the substrate (Ti and Al in the parent material shown in Table 1 are trace elements). This indicates that the ultrasonic impact treatment forms oxide particles mainly composed of Ti, Al, and Mn elements in the sample, among which Ti and Al elements are transferred from the impact needle. This once again proves that the spherical oxides formed by ultrasonic oxidation provide nucleation points for the formation of intracrystalline needle-shaped ferrite.
[0061] According to research, ultrasonic impact treatment using a titanium alloy impact needle (Ti6Al4V) can form mixed oxides such as TiO, TiO2, FeO, Fe2O3 and Al2O3 on the surface of the impact zone. The high-melting-point oxides (such as TiO2 and Al2O3) formed by ultrasonic impact treatment are not easy to burn out during the arc and molten pool metallurgical reaction process. They will remain in the molten pool and disperse with the stirring flow of the molten pool. They are the main source of oxide particles in the sample. The Mn content of the oxide is higher than that of the parent material, so the Mn concentration around the oxide is reduced, which causes the formation of a Mn-poor zone around the particles. The formation of a Mn-poor zone around the oxide particles provides favorable conditions for the nucleation and growth of acicular ferrite under appropriate thermodynamic conditions.
[0062] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A method for controlling the performance of arc additive components based on ultrasonic impact treatment, characterized in that: Using an impact needle to perform ultrasonic impact treatment on the formed component during arc additive manufacturing; The impact needle contains one or more of the following elements: Ti, Al, V, Mg, Ca, Mn, Si, Ni, Mo, Zr; the temperature of the component surface before ultrasonic impact treatment is 150-300°C; The hardness of the impact needle is less than or equal to the hardness of the component metal, so that the impact needle element forms an oxide on the layered surface of the component under the ultrasonic impact oxidation effect. The oxide melts simultaneously with the metal used for the component in the subsequent printing process to form a molten pool, and undergoes a metallurgical reaction with the molten pool to form a tiny granular oxide, thereby affecting the metal crystallization mode and solid-state phase change; During ultrasonic impact treatment, the moving speed of the ultrasonic impact gun is 0.5-3m / min, and the impact intensity is 1-3s / mm 2 , the impact frequency is 100-200Hz, the power of the ultrasonic impact gun power supply is 300W-1500W, and the occurrence frequency is 15-35kHz.
2. The arc additive component performance control method based on ultrasonic impact processing according to claim 1, characterized in that: When the length of the same track during component printing is greater than 1 m and there is no repeated path on the same track, arc additive manufacturing and ultrasonic impact treatment are carried out simultaneously.
3. The arc additive component performance control method based on ultrasonic impact processing according to claim 1, characterized in that: When the length of the same trajectory during the component printing process is less than 1m, or when the path is repeated during the component printing process, a layer of metal is first manufactured using arc additive manufacturing, and then ultrasonic impact treatment is used.
4. The arc additive component performance control method based on ultrasonic impact processing according to claim 2, characterized in that: The distance between the arc of arc additive manufacturing and the ultrasonic impact gun used in ultrasonic processing is calculated according to the following formula: L=T·v Wherein, L is the distance between the electric melting head and the ultrasonic impact head, T is the time required for the component to cool in layers to 150-300°C, and v is the speed at which the electric melting head moves.
5. The arc additive component performance control method based on ultrasonic impact processing according to claim 1, characterized in that: The metal used for the component contains Mn, and the impact needle contains Ti, Al, and V.
6. The arc additive component performance control method based on ultrasonic impact processing according to claim 1, characterized in that: The impact needle has a diameter of 3 to 4 mm, a length of 30 to 50 mm, and is pointed.
7. Application of the arc additive component performance control method based on ultrasonic impact treatment as described in any one of claims 1 to 6 in arc additive manufacturing, arc welding, and surfacing component preparation.
Citation Information
Patent Citations
CMT-ultrasonic peening composite additive manufacturing method
CN108067705A
Method for improving residual stress distribution of electric arc additive manufacturing structural member through ultrasonic impact
CN111687553A
Method For Manufacturing Components Or Coupons Made Of A High Temperature Superalloy
CN103088275A
Method for repairing titanium alloy by ultrasound-assisted laser
CN103114286A
Method for refining laser additive manufacturing titanium alloy grain through ultrasonic impact and induction heating
CN107649682A