Molding compounds containing polyetheramide (PEA)
By optimizing the sub-unit ratio and preparation process of polyether amide, the opacity and sediment problems of polyether amide molding compounds are solved, and a molding compound with high light transmittance and low haze is achieved, which is suitable for a variety of applications and reduces the cost of Use of Toxic Compounds.
Patent Information
- Application Number
- CN202080070900.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-11
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing polyetheramide molding compounds have received negative attention due to their opacity, cloudy appearance and surface deposit formation, and contain toxic alkyl-substituted bis(aminocyclohexyl)methane and bis(aminocyclohexyl)propane, making them difficult to adapt to a wide range of applications. application.
Using polyether amide formed from linear aliphatic diamine and dicarboxylic acid, combined with polyether diamine, the molar mass and functional group content are controlled to form a molding compound with high light transmittance, low haze and no sediment, sub-unit The ratio of 1 and sub-unit 2 is optimized to form hard blocks and soft blocks, and a material with higher light transmittance and low deposits is obtained through a specific preparation process.
A molding compound with high light transmittance and low haze is achieved, which avoids the formation of deposits and reduces the use of toxic compounds. It is suitable for a variety of molded products such as molded parts, films, fibers, etc.
Smart Images

Figure BDA0003586294530000051 
Figure BDA0003586294530000061 
Figure BDA0003586294530000071
Abstract
Description
Technical Field
[0001] The present invention relates to molding compounds containing polyetheramide (PEA), shaped articles produced therefrom, and uses thereof. Background Art
[0002] Polyetheramides (PEA) are block copolymers obtained by polycondensing (oligo)polyamides, in particular acid-regulated polyamides, with alcohol-terminated or amino-terminated polyethers. Acid-regulated polyamides have an excess of carboxylic acid end groups. The skilled person refers to polyamide blocks as hard blocks and polyether blocks as soft blocks. Their preparation is known in principle. DE2712987A1 (US4207410) describes polyamide elastomers of this type, which are formed from dicarboxylic acids, polyether diols and lactams with 10-12 C atoms. The products obtainable according to this document are characterized by long-lasting flexibility and ductility, even at low temperatures, but they are already turbid to opaque in molded parts of medium layer thickness and cause concern when stored for a long time at room temperature due to the presence of surface deposits with a moldy appearance. Polyamide elastomers with a similar structure, composed of aliphatic or aromatic dicarboxylic acids, polyether diols and diamines with 6 to 20 C atoms, are known from EP 0 095 893. The unique properties are increased heat distortion resistance and flexibility. No information can be obtained from this document about the light transmission and deposit formation of the moldings.
[0003] PA11-based and PA12-based PEA molding compounds have also received negative attention due to their opacity, cloudy appearance or surface deposit formation. They have also been observed to have high levels of deposits and low light transmittance. Therefore, current molding compounds are rarely suitable for applications.
[0004] US 2014 / 134371 describes transparent polyamide elastomers. These elastomers contain, among other things, alkyl-substituted bis(aminocyclohexyl)methane and / or alkyl-substituted bis(aminocyclohexyl)propane. However, these compounds are toxic. Summary of the invention
[0005] The object of the present invention is to provide suitable moulding materials which have a high light transmission and a low haze and are free of deposits, even over a long period of time. In addition, they should be less toxic than alkyl-substituted bis(aminocyclohexyl)methane and / or alkyl-substituted bis(aminocyclohexyl)propane.
[0006] This object is achieved by the following molding compound, which comprises a polyetheramide (PEA) based on subunit 1 and subunit 2, wherein subunit 1 is formed by at least one linear aliphatic diamine having 5 to 15 C atoms, preferably 6 to 10 C atoms, and at least one linear aliphatic dicarboxylic acid having 6 to 14 C atoms, preferably 12 to 14 C atoms, and subunit 2 is formed by at least one polyetherdiamine having at least 2.3 C atoms per ether oxygen and having chain-end NH2 groups. The molding compound contains up to 2.5% by weight of a rubber containing functional groups, based on the total weight of the molding compound. The number of C atoms of at least one component of subunit 1 selected from diamines and dicarboxylic acids is at least 13 C atoms; the number-average molar mass of subunit 2 is 200 to 900 g / mol. Preferably, the molar mass of subunit 2 is 300 to 700 g / mol. Subunit 1 thus forms the part generally referred to as the hard block, and subunit 2 forms the soft block. The term "linear" is understood to mean that the carbon chain does not contain any branches.
[0007] In a preferred embodiment, the number average molar mass of subunit 1 is 250 to 4500 g / mol, particularly preferably 400 to 2500 g / mol, more particularly preferably 400 to 2000 g / mol, very particularly preferably 500 to 1600 g / mol. This results in materials with a higher light transmittance and at the same time lower sediment formation.
[0008] The polyetherdiamine of the PEA is preferably selected from diamined polypropylene glycol, diamined polytetramethylene glycol, copolyethers of these substances and mixtures thereof.
[0009] In the PEA, the sum of the C atoms from diamine and dicarboxylic acid is 19 to 24.
[0010] Suitable polyamides for subunit 1 are selected from, for example, 6,13, 6,14, 10,14.
[0011] The molding compound according to the invention contains up to 2.5% by weight of a rubber containing functional groups. Preferably, it contains up to 0.5% by weight and preferably up to 0.1% by weight. Particularly preferably, it contains no such rubber. Such rubbers are described, for example, in EP-A-1518901.
[0012] The molding compound according to the invention preferably contains up to 8 mol % of alkyl-substituted bis(aminocyclohexyl)alkane derivatives selected from alkyl-substituted bis(aminocyclohexyl)methane and alkyl-substituted bis(aminocyclohexyl)propane. The data mentioned relate to the sum of the molar amounts of the linear aliphatic diamine and the alkyl-substituted bis(aminocyclohexyl)alkane derivatives of subunit 1. Preferably up to 5 mol % and particularly preferably up to 2 mol %. In a very particularly preferred embodiment, no bis(aminocyclohexyl)methane and no bis(aminocyclohexyl)propane are contained in the molding compound.
[0013] The present invention further provides a shaped article prepared from the molding compound according to the invention. The shaped article is preferably a molding, a film, a bristle, a fiber or a foam. The shaped article can be prepared, for example, by compression molding, foaming, extrusion, coextrusion, blow molding, 3D blow molding, coextrusion blow molding, coextrusion 3D blow molding, coextrusion blister molding or injection molding. Such methods are known to those skilled in the art.
[0014] The invention further provides for the use of the shaped articles according to the invention, for example as fiber composite components, shoe soles, upper layers of skateboards or snowboards, media lines, frames, design articles, sealing materials, body protection, insulation materials or shell parts with films. DETAILED DESCRIPTION
[0015] Example
[0016] Preparation of polyetheramide (PEA)
[0017] General operation method for preparing PEA:
[0018] In a 100-liter double-bottle polycondensation reactor equipped with an anchor stirrer, diamine, 10% of its mass of deionized (VE) water, dicarboxylic acid and polyether diamine ( RP405 or RP 2005). PPG diamine forms subunit 2. Add 0.1% of 1098 (BASF SE) was used as a process stabilizer. 0.3% of 50% strength hypophosphorous acid, based on the total solids content, was added as a catalyst. After multiple pressurization inertization with N2, the contents of the autoclave were heated to 180-190°C; at 160°C, the stirrer was switched on. The starting materials were stirred for 1 hour and then transferred to a polycondensation reactor equipped with a screw stirrer and a torque recorder. After pressure equalization between the two vessels, the reactor valve was closed and the contents were brought to 228-232°C within 6 hours with stirring at 25 rpm. When an autogenous pressure of 21 bar was reached - typically with an internal temperature between 210°C and 215°C - a two-hour pressure maintenance phase was maintained, after which the pressure was continuously released to atmospheric pressure with further temperature increase. After 3-4 hours at atmospheric pressure - as long as the desired final torque had not yet been reached - a vacuum was applied within 5 hours until a final vacuum of 40-60 mbar was reached. Further stirring was carried out under these conditions until the desired final torque was reached. The melt was extruded as strands into a water bath, pelletized and dried in a drum dryer at 70-90° C. until the water content was <0.1%.
[0019] Molar ratio of subunit 1 to subunit 2: 100:103
[0020] The PEAs prepared are summarized in the following Table 1. The molar mass of the subunit 1 results from the molar ratio of the dicarboxylic acid used and the diamine.
[0021] Table 1: Prepared PEA
[0022]
[0023] All initial weights are in kg, *mass ratios, corrected to the equivalent weight of the polyether diamine
[0024] Diamine 6 = hexamethylenediamine Diamine 10 = 1,10-decamethylenediamine
[0025] Dicarboxylic acid 13 = tridecanedioic acid Dicarboxylic acid 14 = 1,14-tetradecanedioic acid
[0026] Dicarboxylic acid 18 = 1,18-octadecane dioic acid
[0027] Diamine A: Polypropylene glycol diamine
[0028] Diamine B: Hexamethylenediamine / bis(4-amino-3-methylcyclohexyl)methane, ratio in mole %
[0029] The extrusion strand appearance and relative viscosity η of the prepared PEA were studied. reland melting point Tm (see Table 2). Appearance of extruded strands: visual. Viscosity: ISO 307. Tm: DSC, second heat, according to ISO 11357.
[0030] Table 2: Properties of prepared PEA
[0031]
[0032] Testing of the prepared polyetheramide
[0033] Sediment testing
[0034] Injection-molded plaques with dimensions of 60 mm×60 mm×2 mm were prepared from polyetheramide as test specimens. After storage of the test specimens in a closed container under saturation with water vapor at 75° C. for a test period of 10 days, the deposit formation was determined. The deposits were assessed visually using a four-point scale (0-3, where 0=no deposits and 3=severe deposits occurred).
[0035] Determination of light transmittance
[0036] The light transmittance of the above test samples was determined visually. Here, the following evaluations were performed (with light transmittance in descending order):
[0037] 0 = Translucent++
[0038] 1 = Translucent +
[0039] 2 = Translucent 0
[0040] 3 = opaque / milky, 0 = translucent
[0041] 4 = opaque / milky, translucent -
[0042] 5 = milky white.
[0043] Determination of haze value
[0044] The haze value determines the illumination which passes through the article in transmitted light. The haze value is measured here with the aid of 60×60×2 mm plates in accordance with ASTM standard D 1003 using a Konica-Minolta CM-3600d. If the sample is opaque-milky, or even milky, the determination of the haze value is usually omitted.
[0045] Table 3: Test results of PEA 6,13-405 (according to the invention)
[0046]
[0047] The samples of PEA 6,13 showed no sedimentation at high light transmittance and low haze values.
[0048] Table 4: Test results of PEA 6,14-405 (according to the invention)
[0049]
[0050] The test samples of PEA 6,14 were transparent with low haze. They either contained no sediment or had a small amount of sediment.
[0051] Table 5: Test results of PEA 10,14-405 (according to the invention)
[0052]
[0053] The PEA 10,14 samples showed high light transmittance and passed the sediment test.
[0054] Table 6: Test results of PEA 10,14-405 / 2005 (not of the present invention)
[0055]
[0056] *Mass ratio
[0057] PEA 10,14 with subunits containing monomers with a high molar mass of 2005 g / mol showed little to no sediment. However, the test samples were milky white.
[0058] Table 7: Test results of PEA 6,13 (not of the present invention) containing diamine B
[0059]
[0060] The obtained shaped bodies containing diamine B are transparent, but they have precipitates. In addition, there are demoulding problems during injection molding. In addition, the test bars are semicircular in shape (along the longitudinal axis).
Claims
1. A molding compound comprising a polyetheramide (PEA) based on subunit 1, wherein subunit 1 is formed from at least one linear aliphatic diamine having 5 to 15 C atoms and at least one linear aliphatic dicarboxylic acid having 6 to 14 C atoms, and subunit 2 is formed from at least one polyetherdiamine having at least 2.3 C atoms per ether oxygen and having chain-end NH2 groups, wherein the molding compound contains up to 2.5% by weight of a rubber containing functional groups, wherein: the number of C atoms of at least one component of subunit 1 selected from diamines and dicarboxylic acids is at least 13 C atoms, The number average molar mass of subunit 2 is 300 to 700 g / mol; The number average molar mass of the subunit 1 is 250 to 4500 g / mol; The polyether diamine is selected from diamined polypropylene glycol, diamined polytetramethylene glycol, copolyethers of these substances and mixtures thereof; and The sum of the C atoms from the diamine and the dicarboxylic acid is 19-24.
2. The molding compound according to claim 1, characterized in that The number average molar mass of the subunit 1 is 400 to 2500 g / mol.
3. The molding compound according to claim 1 or 2, characterized in that The subunit 1 is selected from polyamide 6,13, 6,14 and 10,14.
4. The molding compound according to claim 1 or 2, characterized in that The proportion of rubber is at most 0.5% by weight.
5. The molding compound according to claim 4, characterized in that The proportion of rubber is at most 0.1% by weight.
6. The molding compound according to claim 1 or 2, characterized in that The diamines contain 6 to 10 C atoms.
7. The molding compound according to claim 1 or 2, characterized in that The dicarboxylic acids contain 12 to 14 C atoms.
8. A shaped article produced from the molding compound according to any one of claims 1 to 7.
9. The shaped article according to claim 8, characterized in that The shaped article is a molding, a film, bristles, fibers or a foam.
10. The shaped article according to claim 8 or 9, characterized in that The shaped article is prepared by compression molding, foaming, extrusion, coextrusion, blow molding, 3D blow molding, coextrusion blow molding, coextrusion 3D blow molding, coextrusion blister molding or injection molding.
11. Use of the shaped article according to any one of claims 8 to 10 as a fiber composite component, a shoe sole, a skateboard or snowboard cover, a media line, a frame, a design article, a sealing material, a body protection, an insulating material or a shell part with a film.
Citation Information
Patent Citations
Process for the production of thermoplastic polyetheresteramides with starting component units randomly distributed in the polymer chain
DE2712987A1
Transparent polyamide elastomers
US20140134371A1
Method for the preparation and use of polyether ester amides with units of the starting components randomly distributed in the polymer chain
US4207410A
Transparent polyamide elastomers
CN101796099A
Composite formed from a polyamide moulding composition and a vulcanized elastomer
CN102858531A