Binder for secondary battery electrode, composition for secondary battery electrode mixture layer, secondary battery electrode and secondary battery
By using cross-linked polymers containing carboxyl polymers as secondary battery electrode binders, the problems of high viscosity and poor adhesion of electrode slurries are solved, and low viscosity and excellent adhesion of highly active material slurries are achieved. Improved electrode durability.
Patent Information
- Application Number
- CN202080071240.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-10-02
AI Technical Summary
When existing secondary battery electrode binders increase the adhesion and active material concentration, it is difficult to reduce the viscosity of the electrode slurry, which affects the coating properties and the durability of the electrode.
A carboxyl-containing polymer is used as a binder. Through the combination of specific structural units and the cross-linking method, a cross-linked polymer is formed to improve the adhesion and reduce the viscosity of the electrode slurry.
It achieves the reduction of electrode slurry viscosity and improvement of adhesion under high active material concentration, ensuring good coating properties and electrode durability.
Smart Images

Figure CN114514639B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a binder for secondary battery electrodes, a composition for secondary battery electrode mixture layer, a secondary battery electrode and a secondary battery. Background Art
[0002] As secondary batteries, various power storage devices such as nickel-hydrogen secondary batteries, lithium-ion secondary batteries, and double-layer capacitors are put into practical use. The electrodes used in these secondary batteries are made by coating and drying a composition for forming an electrode mixture layer containing an active material and a binder on a current collector. For example, in lithium-ion secondary batteries, as a binder used in a negative electrode mixture layer composition, an aqueous binder containing styrene-butadiene rubber (SBR) latex and carboxymethyl cellulose (CMC) is used. On the other hand, as a binder used in a positive electrode mixture layer, a solution of N-methyl-2-pyrrolidone (NMP) of polyvinylidene fluoride (PVDF) is widely used.
[0003] On the other hand, as the use of various secondary batteries expands, there is a trend of increasing demand for improved energy density, reliability and durability. For example, in order to increase the capacity of lithium-ion secondary batteries, the use of silicon-based active materials as negative electrode active materials has increased. However, it is known that silicon-based active materials have a large volume change during charge and discharge, and the electrode mixture layer peels off or falls off with repeated use, resulting in a problem of reduced battery capacity and deterioration of cycle characteristics (durability). In order to suppress such undesirable conditions, it is generally effective to use a binder to firmly bond the active materials (adhesion), and for the purpose of improving durability, research related to improving the adhesion of the binder has been conducted.
[0004] Among them, it has recently been reported that acrylic polymers are effective as binders used in negative electrode mixture layers using silicon-based active materials. For example, in Patent Document 1, an acrylic polymer cross-linked by a specific cross-linking agent is disclosed as a binder for forming a negative electrode coating of a lithium-ion secondary battery. Patent Document 2 discloses an aqueous electrode binder for a secondary battery, which contains a water-soluble polymer, and the water-soluble polymer includes a structural unit derived from an ethylenically unsaturated carboxylate monomer and a structural unit derived from a vinyl alcohol monomer. Patent Document 3 discloses an aqueous electrode binder for a secondary battery, which contains a water-soluble polymer, and the water-soluble polymer includes a structural unit derived from an ethylenically unsaturated carboxylate monomer and a structural unit derived from an ethylenically unsaturated monomer with high hydrophilicity that does not contain carboxylic acid. Patent Document 4 discloses a cross-linked acrylic polymer having a specific particle size in a 1% NaCl aqueous solution.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2014 / 065407
[0008] Patent Document 2: International Publication No. 2014 / 207967
[0009] Patent Document 3: International Publication No. 2016 / 067633
[0010] Patent Document 4: International Publication No. 2017 / 073589 Summary of the invention
[0011] Problems to be solved by the invention
[0012] The binders disclosed in Patent Documents 1 to 4 can all impart good adhesion, but as the performance of secondary batteries improves, there is a growing demand for binders with higher adhesion. In addition, secondary battery electrodes are usually obtained by coating and drying a composition for an electrode mixture layer containing an active material and a binder (hereinafter also referred to as "electrode slurry") on the surface of an electrode collector. At this time, from the perspective of improving the drying efficiency of the electrode slurry and improving the productivity of the electrode, it is advantageous to increase the concentration of active materials in the composition for the electrode mixture layer. However, generally, as the concentration of active materials increases, the viscosity of the electrode slurry also increases, making it difficult to ensure good coating properties. Among them, the binders described in Patent Documents 1 and 4 improve the adhesion of acrylic polymers by micro-crosslinking, but due to the micro-crosslinking, the expansion in water is increased, and even a small amount of viscosity increases significantly, so it is difficult to increase the concentration of active materials.
[0013] The present invention is completed in view of such a situation, and its purpose is to provide a secondary battery electrode adhesive, which can exert better bonding than before, and can reduce the electrode slurry viscosity even when the active material concentration in the electrode mixture layer composition is high. In addition, a secondary battery electrode mixture layer composition, a secondary battery electrode and a secondary battery obtained by using the above-mentioned adhesive are also provided.
[0014] Technical solutions to solve problems
[0015] The present inventors conducted intensive research to solve the above-mentioned problems and found that by making the carboxyl-containing polymer contain a specific amount of specific structural units, it is possible to exert better adhesion than before, and even when the concentration of active material in the electrode mixture layer composition is high, the viscosity of the electrode slurry can be reduced, thereby completing the present invention.
[0016] The present invention is as follows.
[0017] [1] A binder for secondary battery electrodes, comprising a carboxyl group-containing polymer or a salt thereof, wherein the carboxyl group-containing polymer or the salt thereof comprises structural units derived from a monomer represented by the general formula (1) and structural units derived from an ethylenically unsaturated carboxylic acid monomer different from the general formula (1), and the carboxyl group-containing polymer or the salt thereof comprises structural units derived from the monomer represented by the general formula (1) in an amount of not less than 0.1% by mass and not more than 20% by mass relative to all structural units of the carboxyl group-containing polymer or the salt thereof.
[0018] [Chemical formula 1]
[0019]
[0020] [2] The binder for secondary battery electrodes according to [1], wherein the carboxyl group-containing polymer or its salt contains 50% by mass or more and 99.9% by mass or less of the structural unit derived from the ethylenically unsaturated carboxylic acid monomer different from that of the general formula (1) relative to all its structural units.
[0021] [3] The binder for secondary battery electrodes according to [1] or [2], wherein the carboxyl group-containing polymer is a cross-linked polymer obtained by polymerizing a monomer composition containing a non-cross-linking monomer and a cross-linking monomer.
[0022] [4] The binder for secondary battery electrodes according to [3], wherein the amount of the crosslinkable monomer used is 0.1 mol % or more and 1.0 mol % or less relative to the total amount of the non-crosslinkable monomer.
[0023] [5] The binder for secondary battery electrodes according to [3] or [4], wherein the sol fraction of the cross-linked polymer is less than 40% by mass.
[0024] [6] The binder for secondary battery electrodes according to any one of [3] to [5], wherein the crosslinked polymer has a water swelling degree of 4.0 or more and 60 or less at pH 8.
[0025] [7] The binder for secondary battery electrodes according to any one of [3] to [6], wherein the crosslinkable monomer includes a compound having two or more allyl ether groups in the molecule.
[0026] [8] A composition for a secondary battery electrode mixture layer, comprising the binder for a secondary battery electrode according to any one of [1] to [7], an active material, and water.
[0027] [9] A secondary battery electrode comprising an electrode mixture layer containing the binder for secondary battery electrodes according to any one of [1] to [7] on a surface of a current collector.
[0028]
[10] A secondary battery comprising the secondary battery electrode described in [9].
[0029] Effects of the Invention
[0030] According to the binder for secondary battery electrodes of the present invention, it is possible to exhibit excellent binding properties and reduce the viscosity of the electrode slurry even when the active material concentration in the electrode mixture layer composition is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a diagram showing an apparatus used for measuring the water swelling degree of a carboxyl group-containing polymer or a salt thereof. DETAILED DESCRIPTION
[0032] The adhesive for secondary battery electrodes of the present invention contains a carboxyl-containing polymer or a salt thereof, which can be prepared into a composition for a secondary battery electrode mixture layer by mixing with an active substance and water. From the perspective of exerting the effect of the present invention, the above-mentioned composition is preferably an electrode slurry in a slurry state that can be applied to the collector, but it can also be prepared into a wet powder state so that it can cope with stamping processing on the collector surface. By forming an electrode mixture layer formed by the above-mentioned composition on the surface of a collector such as copper foil or aluminum foil, a secondary battery electrode of the present invention can be obtained.
[0033] Hereinafter, the binder for secondary battery electrodes, the composition for secondary battery electrode mixture layers obtained by using the binder, the secondary battery electrode, and the secondary battery of the present invention will be described in detail.
[0034] It should be noted that, in the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid, "(meth)acrylate" means acrylate and / or methacrylate, and "(meth)acryloyl" means acryloyl and / or methacryloyl.
[0035] <Adhesive>
[0036] The adhesive of the present invention comprises a carboxyl group-containing polymer or a salt thereof, wherein the carboxyl group-containing polymer has a structural unit derived from a monomer represented by the general formula (1) and a structural unit derived from an ethylenically unsaturated carboxylic acid monomer different from the general formula (1).
[0037] <Structural unit of carboxyl group-containing polymer>
[0038] <Structural unit derived from the monomer represented by the general formula (1)>
[0039] The carboxyl-containing polymer (hereinafter, also referred to as "the present polymer") contains a structural unit derived from a monomer represented by the above-mentioned general formula (1) (hereinafter, also referred to as "component (a)"), and contains 0.1% by mass or more and 20% by mass or less of the component (a) relative to all the structural units of the carboxyl-containing polymer or its salt.
[0040] This polymer contains component (a) in this range, so that even when the active material concentration in the electrode mixture layer composition is high, the electrode slurry viscosity can be reduced to ensure good coating properties, and the binder containing this polymer exerts excellent adhesion, and easily ensures excellent adhesion to the collector. The lower limit is, for example, 0.15% by mass or more, for example, 0.2% by mass or more, for example, 0.25% by mass or more, and for example, 0.3% by mass or more. In the case where the lower limit is 0.1% by mass or more, it is preferred from the perspective of the coating, adhesion and durability of the electrode slurry as a battery. In addition, the upper limit is, for example, 19% by mass or less, for example, 18% by mass or less, for example, 17% by mass or less, and for example, 16% by mass or less. As a range, it can be set to a range formed by appropriately combining such a lower limit and an upper limit.
[0041] <Structural unit derived from an ethylenically unsaturated carboxylic acid monomer different from that of general formula (1)>
[0042] The present polymer has, in addition to the component (a), a structural unit derived from an ethylenically unsaturated carboxylic acid monomer different from that of the general formula (1) (hereinafter also referred to as "component (b)").
[0043] By making this polymer have component (b), the adhesion to the collector is improved, and the desolvation effect and ion conductivity of lithium ions are excellent, so an electrode with low resistance and excellent high rate characteristics can be obtained. In addition, due to the imparting of water swellability, the dispersion stability of active materials in the electrode mixture layer composition can be improved.
[0044] The component (b) can be introduced into the present polymer by, for example, polymerizing a monomer containing an ethylenically unsaturated carboxylic acid monomer different from the general formula (1). Alternatively, it can be obtained by (co)polymerizing (meth)acrylate monomers and then hydrolyzing them. Alternatively, it can be obtained by polymerizing (meth)acrylamide and (meth)acrylonitrile and then treating them with a strong base, or by reacting an acid anhydride with a polymer having a hydroxyl group.
[0045] As ethylenically unsaturated carboxylic acid monomers different from the above-mentioned general formula (1), there can be mentioned (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid; (meth)acrylamide alkyl carboxylic acids such as (meth)acrylamide caproic acid and (meth)acrylamide dodecanoic acid; ethylenically unsaturated monomers having carboxyl groups such as succinic acid monohydroxyethyl (meth)acrylate and ω-carboxyl-caprolactone mono(meth)acrylate, or their (partial) alkali neutralizations, one of which can be used alone or two or more can be used in combination. Among the above, compounds having an acryloyl group as a polymerizable functional group are preferred, and acrylic acid is particularly preferred, from the perspective of obtaining a polymer having a long primary chain length due to a high polymerization rate and improving the bonding strength of the adhesive. When acrylic acid is used as an ethylenically unsaturated carboxylic acid monomer, a polymer having a high carboxyl content can be obtained.
[0046] The content of component (b) in the present polymer is not particularly limited, for example, relative to all structural units of the present polymer, it can include more than 10% by mass and less than 99.9% by mass. By containing component (b) in this range, it is possible to reduce the viscosity of the electrode slurry and ensure good coating properties, and easily ensure excellent adhesion to the collector. The lower limit is, for example, more than 20% by mass, and for example, more than 30% by mass, and for example, more than 40% by mass. In the case where the lower limit is more than 10% by mass, it is preferred from the perspective of the coating properties, adhesion properties and durability of the electrode slurry as a battery. The lower limit can be more than 50% by mass, and can also be more than 60% by mass, and can also be more than 70% by mass, and can also be more than 80% by mass. In addition, the upper limit is, for example, less than 99% by mass, and for example, less than 98% by mass, and for example, less than 95% by mass, and for example, less than 90% by mass. As a range, it can be set to a range formed by appropriately combining such a lower limit and an upper limit.
[0047] <Other structural units>
[0048] In addition to the components (a) and (b), the present polymer further comprises structural units derived from other ethylenically unsaturated monomers that can copolymerize with them (hereinafter, also referred to as "component (c)"). Component (c) is a structural unit derived from a monomer having an ethylenically unsaturated group other than the components (a) and (b), for example, structural units derived from ethylenically unsaturated monomer compounds having anionic groups other than carboxyl groups such as sulfonic acid groups and phosphoric acid groups, or nonionic ethylenically unsaturated monomers. These structural units can be introduced by copolymerizing ethylenically unsaturated monomer compounds having anionic groups other than carboxyl groups such as sulfonic acid groups and phosphoric acid groups, or monomers containing nonionic ethylenically unsaturated monomers.
[0049] The proportion of (c) component can be set to 0% by mass or more and 89.9% by mass or less relative to the total structural units of this polymer. The proportion of (c) component can be 0.5% by mass or more and 70% by mass or less, or 1% by mass or more and 60% by mass or less, or 2% by mass or more and 50% by mass or less, or 5% by mass or more and 40% by mass or less, or 10% by mass or more and 30% by mass or less. The range formed by appropriately combining such lower and upper limits can be set as a range. Here, in the case of containing more than 1% by mass (c) component relative to the total structural units of this polymer, the affinity for the electrolyte is improved, so the effect of improving lithium ion conductivity can also be expected.
[0050] As the (c) component, among the above, from the viewpoint of obtaining an electrode with good bending resistance, a structural unit derived from a nonionic ethylenically unsaturated monomer is preferred, and examples of the nonionic ethylenically unsaturated monomer include (meth)acrylamide and its derivatives, alicyclic structure-containing ethylenically unsaturated monomers, and hydroxyl-containing ethylenically unsaturated monomers.
[0051] Examples of (meth)acrylamide derivatives include N-alkyl (meth)acrylamide compounds such as isopropyl (meth)acrylamide and tert-butyl (meth)acrylamide; N-alkoxyalkyl (meth)acrylamide compounds such as N-n-butoxymethyl (meth)acrylamide and N-isobutoxymethyl (meth)acrylamide; and N,N-dialkyl (meth)acrylamide compounds such as dimethyl (meth)acrylamide and diethyl (meth)acrylamide. Any one of these may be used alone or in combination of two or more.
[0052] Examples of the ethylenically unsaturated monomer containing an alicyclic structure include cycloalkyl (meth)acrylates which may have an aliphatic substituent, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclodecyl (meth)acrylate, and cyclododecyl (meth)acrylate; isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate; and cycloalkyl polyol mono(meth)acrylates such as cyclohexanedimethanol mono(meth)acrylate and cyclodecane dimethanol mono(meth)acrylate. Any one of these may be used alone, or two or more of them may be used in combination.
[0053] Examples of the hydroxyl group-containing ethylenically unsaturated monomer include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate. These may be used alone or in combination of two or more.
[0054] As other nonionic ethylenically unsaturated monomers, for example, (meth)acrylates can be used. Examples of (meth)acrylates include (meth)alkyl acrylate compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; (meth)aryl alkyl acrylate compounds such as phenyl (meth)acrylate, phenylmethyl (meth)acrylate, and phenylethyl (meth)acrylate; and (meth)alkoxyalkyl acrylate compounds such as 2-methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate. One of these compounds may be used alone, or two or more thereof may be used in combination.
[0055] From the aspect of the excellent cohesiveness of the adhesive, this polymer or its salt preferably includes structural units derived from (methyl) acrylamide and its derivatives, ethylenically unsaturated monomers containing alicyclic structures, etc. In addition, as (c) component, in the case of introducing structural units derived from hydrophobic ethylenically unsaturated monomers having a solubility of less than 1g / 100ml in water, it is possible to achieve strong interaction with the electrode material, and good cohesiveness can be exerted to the active material. Thus, it is possible to obtain a firm and well-integrated electrode mixture layer, therefore, as the above-mentioned "hydrophobic ethylenically unsaturated monomers having a solubility of less than 1g / 100ml in water", it is particularly preferred to be ethylenically unsaturated monomers containing alicyclic structures.
[0056] From the perspective of improving the cycle characteristics of the resulting secondary battery, the present polymer or its salt preferably contains a structural unit derived from a hydroxyl-containing ethylenically unsaturated monomer, preferably containing 0.5% by mass or more and 70% by mass or less of the structural unit, more preferably containing 2.0% by mass or more and 50% by mass or less, and further preferably containing 10.0% by mass or more and 50% by mass or less.
[0057] Among nonionic ethylenically unsaturated monomers, compounds having an acryloyl group are preferred because they have a high polymerization rate and can provide a polymer having a long primary chain length, thereby improving the adhesive strength of the adhesive.
[0058] The polymer may be a salt. The type of salt is not particularly limited, and examples thereof include alkali metal salts such as lithium salts, sodium salts and potassium salts; alkaline earth metal salts such as magnesium salts, calcium salts and barium salts; other metal salts such as aluminum salts; ammonium salts and organic amine salts, etc. Among them, alkali metal salts and magnesium salts are preferred, and alkali metal salts are more preferred, from the perspective of not easily causing adverse effects on battery characteristics. In addition, lithium salts are particularly preferred from the perspective of being able to obtain a battery with low resistance.
[0059] <Preferred Embodiments of the Polymer>
[0060] From the aspect that the binder containing the polymer can ensure the coating property of good electrode slurry even at high active material concentration and further exert good bonding performance, the carboxyl-containing polymer of the present invention is preferably a cross-linked polymer (hereinafter referred to as "cross-linked polymer"). The cross-linking method in the cross-linked polymer is not particularly limited, for example, the mode based on the following method can be exemplified.
[0061] 1) Copolymerization of cross-linking monomers
[0062] 2) Chain transfer to polymer chains during free radical polymerization
[0063] 3) After synthesizing a polymer having a reactive functional group, a crosslinking agent is added as needed for post-crosslinking
[0064] Since the polymer has a cross-linked structure, the adhesive containing the polymer or a salt thereof can have excellent adhesive strength. Among the above, the method using copolymerization of a cross-linking monomer is preferred because of its ease of operation and ease of controlling the degree of cross-linking.
[0065] <Crosslinking monomer>
[0066] Examples of the crosslinkable monomer include a polyfunctional polymerizable monomer having two or more polymerizable unsaturated groups and a self-crosslinkable crosslinkable functional group-containing monomer such as a hydrolyzable silyl group.
[0067] The above-mentioned multifunctional polymerizable monomer is a compound having two or more polymerizable functional groups such as (meth) acryloyl groups and alkenyl groups in the molecule, and can include multifunctional (meth) acrylate compounds, multifunctional alkenyl compounds, compounds having both (meth) acryloyl groups and alkenyl groups, etc. These compounds can be used alone or in combination of two or more. Among these, from the aspect of easily obtaining a uniform cross-linked structure, it is preferably a multifunctional alkenyl compound, and particularly preferably a multifunctional allyl ether compound having two or more allyl ether groups in the molecule.
[0068] Examples of the polyfunctional (meth)acrylate compound include di(meth)acrylates of diols such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate; poly(meth)acrylates such as tri(meth)acrylates and tetra(meth)acrylates of tri- or higher-valent polyols such as trimethylolpropane tri(meth)acrylate, trimethylolpropane ethylene oxide-modified tri(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; and bisamides such as methylenebisacrylamide and hydroxyethylenebisacrylamide.
[0069] Examples of the polyfunctional alkenyl compound include polyfunctional allyl ether compounds such as trimethylolpropane diallyl ether, trimethylolpropane triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, tetraallyloxyethane, and polyallylsucrose; polyfunctional allyl compounds such as diallyl phthalate; and polyfunctional vinyl compounds such as divinylbenzene.
[0070] Examples of the compound having both a (meth)acryloyl group and an alkenyl group include allyl (meth)acrylate, isopropenyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and 2-(2-vinyloxyethoxy)ethyl (meth)acrylate.
[0071] Specific examples of the monomer having a self-crosslinkable crosslinkable functional group include hydrolyzable silyl group-containing vinyl monomers, N-methylol (meth) acrylamide, N-methoxyalkyl (meth) acrylamide, etc. These compounds may be used alone or in combination of two or more.
[0072] The vinyl monomer containing a hydrolyzable silyl group is not particularly limited as long as it is a vinyl monomer having at least one hydrolyzable silyl group. For example, vinyl silanes such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl methyl dimethoxysilane, and vinyl dimethyl methoxysilane; silyl-containing acrylic acid esters such as trimethoxysilyl propyl acrylate, triethoxysilyl propyl acrylate, and methyl dimethoxysilyl propyl acrylate; silyl-containing methacrylic acid esters such as trimethoxysilyl propyl methacrylate, triethoxysilyl propyl methacrylate, methyl dimethoxysilyl propyl methacrylate, and dimethyl methoxysilyl propyl methacrylate; silyl-containing vinyl ethers such as trimethoxysilyl propyl vinyl ether; silyl-containing vinyl esters such as trimethoxysilyl undecanoic acid vinyl ester, etc.
[0073] In the case where the cross-linked polymer is cross-linked by a cross-linking monomer, the amount of the cross-linking monomer used is preferably 0.010 to 3.0 mol%, more preferably 0.050 to 2.0 mol%, more preferably 0.10 to 1.5 mol%, and more preferably 0.20 to 1.0 mol% relative to the total amount of monomers (non-cross-linking monomers) other than the cross-linking monomer. If the amount of the cross-linking monomer used is 0.010 mol% or more, it is preferred in terms of better adhesion and stability of the electrode slurry. If it is 3.0 mol% or less, it is preferred in terms of better adhesion.
[0074] The amount of the crosslinkable monomer used is preferably 0.05 to 5.0% by mass, more preferably 0.10 to 3.0% by mass, further preferably 0.20 to 2.5% by mass, and further preferably 0.30 to 2.0% by mass, based on the total monomers constituting the crosslinked polymer.
[0075] <Sol fraction of cross-linked polymer>
[0076] The sol fraction of the cross-linked polymer or its salt is preferably less than 40% by mass. In the case where the sol fraction is as described above, an electrode showing excellent adhesion can be obtained, and the cycle characteristics of the secondary battery containing the electrode are also improved. The lower limit of the sol fraction can be more than 0.1% by mass, or more than 0.2% by mass, or more than 0.5% by mass, or more than 1.0% by mass. The upper limit of the sol fraction can be less than 35% by mass, or less than 30% by mass, or less than 25% by mass, or less than 20% by mass, or less than 15% by mass.
[0077] The sol component in this specification is mainly composed of a polymer without a three-dimensional cross-linked structure, and the sol fraction contained in the cross-linked polymer or its salt can be adjusted by a known method. That is, the sol fraction can be set to a desired range by adjusting the type and amount of the cross-linking agent, the primary chain length of the polymer, etc. For example, the sol fraction is usually reduced by increasing the amount of the cross-linking agent used and increasing the primary chain length.
[0078] <Weight average molecular weight of sol component of cross-linked polymer>
[0079] The weight average molecular weight of the sol component of the cross-linked polymer or its salt is preferably 300,000 or less in terms of the value converted to polyethylene oxide / polyethylene glycol. It is more preferably 200,000 or less, further preferably 150,000 or less, and further preferably 100,000 or less. When the weight average molecular weight of the sol component is as above, the coating property of the electrode slurry is excellent, an electrode showing excellent adhesion can be obtained, and an excellent effect is also exerted on the cycle characteristics of the secondary battery containing the electrode. The lower limit of the weight average molecular weight of the sol component can be 1,000 or more, 2,000 or more, 3,000 or more, 5,000 or more, or 10,000 or more.
[0080] It should be noted that the weight average molecular weight of the sol component of the cross-linked polymer is a value calculated in terms of polyethylene oxide / polyethylene glycol.
[0081] <Particle size of cross-linked polymer>
[0082] In the electrode mixture layer composition, when the cross-linked polymer is not present in the form of large-size aggregates (secondary aggregates) but is well dispersed as water-swellable particles with an appropriate particle size, the binder containing the cross-linked polymer can exert good binding properties, which is preferred.
[0083] For the cross-linked polymer or its salt of the present invention, the particle size (water-swollen particle size) when the substance with a neutralization degree of 80 to 100 mol% of the carboxyl group possessed by the cross-linked polymer is dispersed in water is preferably in the range of 0.1 μm or more and 10.0 μm or less in terms of volume-based median particle size. If the particle size is in the range of 0.1 μm or more and 10.0 μm or less, it is uniformly present in the electrode mixture layer composition with a suitable size, so the stability of the electrode mixture layer composition is high and excellent adhesion can be exerted. If the particle size exceeds 10.0 μm, as described above, the adhesion may become insufficient. In addition, from the perspective of difficulty in obtaining a smooth coating surface, the coating may become insufficient. On the other hand, when the particle size is less than 0.1 μm, there is concern from the perspective of stable manufacturing. The lower limit of the above-mentioned particle size can be 0.2 μm or more, 0.3 μm or more, and 0.5 μm or more. The upper limit of the particle size can be 9.0 μm or less, 8.0 μm or less, 7.0 μm or less, 5.0 μm or less, or 3.0 μm or less. The particle size range can be set by appropriately combining the above lower limit and upper limit, for example, 0.1 μm or more and 9.0 μm or less, 0.2 μm or more and 8.0 μm or less, or 0.3 μm or more and 5.0 μm or less.
[0084] It should be noted that the water-swollen particle size can be measured by the method described in the examples of this specification.
[0085] When the cross-linked polymer is not neutralized or the degree of neutralization is less than 80 mol%, it can be neutralized with an alkali metal hydroxide or the like to a degree of neutralization of 80 to 100 mol%, and the particle size when dispersed in water can be measured. Usually, the cross-linked polymer or its salt exists in the form of block particles obtained by association and agglomeration of primary particles in the state of powder or solution (dispersion liquid). When the particle size during the above-mentioned water dispersion is within the above-mentioned range, the cross-linked polymer or its salt has extremely excellent dispersibility. By neutralizing to a degree of neutralization of 80 to 100 mol% and dispersing in water, the block particles are dissociated to form a dispersion of roughly primary particles, or even if it is a secondary agglomerate, a stable dispersion state with a particle size in the range of 0.1 to 10.0 μm is formed.
[0086] From the viewpoint of adhesion and coating properties, the value obtained by dividing the volume average particle size of the water-swellable particle size by the number average particle size, i.e., the particle size distribution, is preferably 10 or less, more preferably 5.0 or less, further preferably 3.0 or less, and further preferably 1.5 or less. The lower limit of the above particle size distribution is usually 1.0.
[0087] The cross-linked polymer or its salt of the present invention preferably has a particle size (dry particle size) when dried in terms of volume-based median particle size of 0.03 μm to 3 μm. The particle size is more preferably in the range of 0.1 μm to 1 μm, and even more preferably in the range of 0.3 μm to 0.8 μm.
[0088] For the cross-linked polymer or its salt, it is preferred that the acid groups such as carboxyl groups derived from ethylenically unsaturated carboxylic acid monomers are neutralized in a neutralization degree of 20 to 100 mol% in the electrode mixture layer composition and used in the form of salts. The above-mentioned neutralization degree is more preferably 50 to 100 mol%, and further preferably 60 to 95 mol%. When the neutralization degree is 20 mol% or more, the water swellability becomes good, and it is easy to obtain a dispersion stabilization effect, which is preferred from this aspect. In this specification, the above-mentioned neutralization degree can be calculated based on the feed value of the monomer having an acid group such as a carboxyl group and the neutralizer used for neutralization. It should be noted that the neutralization degree can be determined by IR measurement of the powder of the cross-linked polymer or its salt after drying for 3 hours at 80°C under reduced pressure conditions, and confirmed by the intensity ratio of the peak of the C=O group derived from the carboxylic acid to the peak of the C=O group derived from the carboxylate.
[0089] <Molecular weight of cross-linked polymer (primary chain length)>
[0090] Cross-linked polymers have a three-dimensional cross-linked structure and exist as microgels in media such as water. Generally, such three-dimensional cross-linked polymers are insoluble in solvents, so their molecular weight cannot be measured. Similarly, it is usually difficult to measure the primary chain length of cross-linked polymers and perform quantitative analysis.
[0091] <Water Swelling Degree of Cross-linked Polymer>
[0092] In this specification, the water swelling degree is defined as the mass of the cross-linked polymer or its salt when dried (W A )g", and the mass of water absorbed when the cross-linked polymer or its salt is saturated with water "(W B )g", calculated based on the following formula.
[0093] (Water Swelling Degree) = {(W A )+(W B )} / (W A )
[0094] The water swelling degree of the cross-linked polymer or its salt at pH 8 is preferably 4.0 or more and 60 or less. If the water swelling degree is within the above range, the cross-linked polymer or its salt swells moderately in the aqueous medium, so when forming the electrode mixture layer, sufficient bonding area to the active material and the collector can be ensured, and there is a tendency for the adhesion to become good. The above-mentioned water swelling degree can be, for example, 5.0 or more, 6.0 or more, 7.0 or more, 10 or more, or 15 or more. When the water swelling degree is 4.0 or more, the cross-linked polymer or its salt expands on the surface of the active material and the collector, and sufficient bonding area can be ensured, so good adhesion can be obtained. The upper limit of the water swelling degree at pH 8 can be 55 or less, 50 or less, 45 or less, 40 or less, or 35 or less. If the water swelling degree exceeds 60, there is a tendency that the viscosity of the electrode mixture layer composition (electrode slurry) containing a cross-linked polymer or its salt becomes higher, and the uniformity of the mixture layer is insufficient, as a result, sufficient bonding force cannot be obtained sometimes. In addition, the coating property of the electrode slurry is likely to be reduced. The range of the water swelling degree at pH 8 can be set by appropriately combining the above-mentioned upper limit and lower limit, for example, more than 5.0 and less than 60, for example, more than 6.0 and less than 60, for example, more than 5.0 and less than 55.
[0095] The water swelling degree at pH 8 can be obtained by measuring the swelling degree of the cross-linked polymer or its salt in water at pH 8. As the water at pH 8, for example, ion exchange water can be used, and the pH value can be adjusted using an appropriate acid or base, or a buffer solution, etc. as needed. The pH during the measurement is, for example, in the range of 8.0 ± 0.5, preferably in the range of 8.0 ± 0.3, more preferably in the range of 8.0 ± 0.2, and further preferably in the range of 8.0 ± 0.1. In addition, the measurement is performed at 25 ± 5 ° C.
[0096] It should be noted that, those skilled in the art can adjust the water swelling degree by controlling the composition and structure of the cross-linked polymer or its salt. For example, the water swelling degree can be increased by introducing an acidic functional group or a highly hydrophilic structural unit into the cross-linked polymer. In addition, by reducing the cross-linking degree of the cross-linked polymer, the water swelling degree is usually increased.
[0097] <Method for producing the present polymer or its salt>
[0098] The present polymer can be prepared by known polymerization methods such as solution polymerization, precipitation polymerization, suspension polymerization, and emulsion polymerization. From the perspective of productivity, precipitation polymerization and suspension polymerization (reverse phase suspension polymerization) are preferred. From the perspective of obtaining better performance such as adhesion, heterogeneous polymerization methods such as precipitation polymerization, suspension polymerization, and emulsion polymerization are preferred, and precipitation polymerization is more preferred.
[0099] Precipitation polymerization is a method of producing a polymer by carrying out a polymerization reaction in a solvent that dissolves the unsaturated monomer as a raw material but does not substantially dissolve the resulting polymer. As the polymerization proceeds, the polymer particles grow larger by aggregation and growth, and a dispersion can be obtained in which primary particles of tens to hundreds of nm are secondary aggregated into polymer particles of several to tens of μm. In order to control the particle size of the polymer, a dispersion stabilizer can also be used.
[0100] As specific dispersion stabilizers, dispersion stabilizers manufactured by living free radical polymerization, macromonomer dispersion stabilizers, nonionic surfactants, etc. can be cited. It should be noted that the above-mentioned secondary coagulation can also be suppressed by selecting a dispersion stabilizer, a polymerization solvent, etc. Usually, precipitation polymerization in which secondary coagulation is suppressed is also called dispersion polymerization.
[0101] In the case of precipitation polymerization, the polymerization solvent may be selected from water and various organic solvents, etc., in consideration of the types of monomers used, etc. In order to obtain a polymer with a long primary chain length, it is preferred to use a solvent with a small chain transfer constant.
[0102] As specific polymerization solvents, in addition to water-soluble solvents such as methanol, tert-butyl alcohol, acetone, methyl ethyl ketone, acetonitrile and tetrahydrofuran, benzene, ethyl acetate, ethylene dichloride, n-hexane, cyclohexane and n-heptane can also be cited, and one of them can be used alone or in combination of two or more. Alternatively, they can also be used in the form of a mixed solvent with water. In the present invention, a water-soluble solvent refers to a water-soluble solvent having a solubility in water at 20°C greater than 10g / 100ml.
[0103] Among the above, methyl ethyl ketone and acetonitrile are preferred from the perspectives of the formation of coarse particles, low adhesion to the reactor, good polymerization stability, the precipitated polymer particles are not prone to secondary aggregation (or even if secondary aggregation occurs, they are easily dispersed in an aqueous medium), the ability to obtain a polymer with a small chain transfer constant and a large degree of polymerization (primary chain length), and easy handling during the neutralization step described later.
[0104] In addition, in the same process and in order to make the neutralization reaction stable and rapidly proceed, it is preferred to pre-add a small amount of high polarity solvent to the polymerization solvent. As the above-mentioned high polarity solvent, water and methanol can be preferably cited. The amount of the high polarity solvent used is preferably 0.05-20.0 mass %, more preferably 0.1-10.0 mass %, further preferably 0.1-5.0 mass %, and further preferably 0.1-1.0 mass %. If the proportion of the high polarity solvent is 0.05 mass % or more, the effect on the above-mentioned neutralization reaction is observed, and if it is 20.0 mass % or less, no adverse effect on the polymerization reaction is seen. In addition, in the polymerization of highly hydrophilic ethylenically unsaturated carboxylic acid monomers such as acrylic acid, when a high polarity solvent is added, the polymerization rate is increased, and it is easy to obtain a polymer with a long primary chain length. Among the high polarity solvents, water in particular has a large effect on increasing the above-mentioned polymerization rate, so it is preferred.
[0105] In the production of the present polymer or its salt, it is preferred to have a polymerization step of polymerizing a monomer component comprising a monomer represented by the general formula (1) and an ethylenically unsaturated carboxylic acid monomer different from the general formula (1). For example, it is preferred to have a polymerization step of polymerizing a monomer component comprising 0.1% by mass or more and 20% by mass or less of an ethylenically unsaturated carboxylic acid monomer as a source of component (a) and 10% by mass or more and 99.9% by mass or less of other ethylenically unsaturated monomers as a source of component (b).
[0106] By the above-mentioned polymerization step, 0.1 mass % or more and 20 mass % or less of the structural unit derived from the monomer represented by the above-mentioned general formula (1) (component (a)) is introduced into the cross-linked polymer, and 10 mass % or more and 99.9 mass % or less of the structural unit derived from the monomer represented by the above-mentioned general formula (1) (component (b)) is introduced.
[0107] The usage amount of the monomer represented by the above general formula (1) is, for example, 0.1 mass % to 19 mass %, for example, 0.1 mass % to 18 mass %, for example, 0.1 mass % to 17 mass %, for example, 0.1 mass % to 16 mass %.
[0108] The amount of the ethylenically unsaturated carboxylic acid monomer different from that of the general formula (1) is, for example, 20% by mass or more and 99.9% by mass or less, for example, 50% by mass or more and 99.9% by mass or less, for example, 60% by mass or more and 99.9% by mass or less, for example, 70% by mass or more and 99.9% by mass or less, for example, 80% by mass or more and 99.9% by mass or less.
[0109] As the above-mentioned other ethylenically unsaturated monomers, for example, ethylenically unsaturated monomer compounds with anionic groups other than carboxyl groups such as sulfonic acid groups and phosphoric acid groups and nonionic ethylenically unsaturated monomers can be cited. As specific compounds, monomer compounds capable of introducing the above-mentioned (c) component can be cited. The above-mentioned other ethylenically unsaturated monomers can include more than 0 mass % and less than 89.9 mass % relative to the total amount of monomer components, can be more than 0.5 mass % and less than 70 mass %, can also be more than 1 mass % and less than 60 mass %, can also be more than 5 mass % and less than 50 mass %, can also be more than 10 mass % and less than 30 mass %. In addition, the above-mentioned cross-linking monomers can also be used in the same manner.
[0110] The monomer components polymerized in the polymerization step may include a crosslinking monomer. As the crosslinking monomer, as described above, there can be mentioned a multifunctional polymerizable monomer having two or more polymerizable unsaturated groups, and a monomer having a crosslinking functional group such as a hydrolyzable silyl group capable of self-crosslinking, and the amount of the crosslinking monomer used is as described above.
[0111] The monomer concentration during polymerization is preferably high from the viewpoint of obtaining a polymer with a longer primary chain length. However, if the monomer concentration is too high, the aggregation of polymer particles is easy to proceed. In addition, the control of polymerization heat becomes difficult and the polymerization reaction may get out of control. Therefore, for example, in the case of precipitation polymerization, the monomer concentration at the start of polymerization is generally in the range of about 2 to 40% by mass, preferably in the range of 5 to 40% by mass.
[0112] In addition, in this specification, "monomer concentration" means the monomer concentration in the reaction solution at the time of starting polymerization.
[0113] This polymer can be manufactured by carrying out a polymerization reaction in the presence of an alkaline compound (salt-based compound). By carrying out a polymerization reaction in the presence of an alkaline compound, the polymerization reaction can be stably implemented even under conditions of high monomer concentration. The monomer concentration can be 13.0% by mass or more, preferably 15.0% by mass or more, more preferably 17.0% by mass or more, further preferably 19.0% by mass or more, and further preferably 20.0% by mass or more. The monomer concentration is also preferably 22.0% by mass or more, and further preferably 25.0% by mass or more. Generally, the higher the monomer concentration during polymerization, the more high molecular weight can be achieved, and polymers with long primary chains can be manufactured. In addition, polymers with long primary chains tend to be combined into three-dimensional cross-linked structures, so there is a tendency for the sol fraction to decrease.
[0114] The upper limit of the monomer concentration varies depending on the types of monomers and solvents used, the polymerization method, various polymerization conditions, etc., but as long as the heat of the polymerization reaction can be removed, it is approximately 40% in precipitation polymerization, approximately 50% in suspension polymerization, and approximately 70% in emulsion polymerization as described above.
[0115] The above-mentioned basic compound is a so-called basic compound, and any one of an inorganic basic compound and an organic basic compound can be used. By carrying out polymerization reaction in the presence of the basic compound, for example, under the condition of a high monomer concentration exceeding 13.0 mass %, polymerization reaction can also be stably implemented. In addition, the molecular weight of the polymer obtained by polymerization at such a high monomer concentration is high (long primary chain length), so the adhesion is also excellent.
[0116] Examples of the inorganic alkaline compound include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide and potassium hydroxide, alkaline earth metal hydroxides such as calcium hydroxide and magnesium hydroxide, and alkali metal carbonates such as sodium carbonate and potassium carbonate. One or more of these may be used.
[0117] Examples of the organic basic compound include ammonia and organic amine compounds, and one or more of these can be used. Among them, organic amine compounds are preferred from the viewpoint of polymerization stability and the adhesiveness of an adhesive containing the obtained cross-linked polymer or a salt thereof.
[0118] Examples of the organic amine compound include N-alkyl substituted amines such as monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, monobutylamine, dibutylamine, tributylamine, monohexylamine, dihexylamine, trihexylamine, trioctylamine and tri(dodecyl)amine; (alkyl) alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, propanolamine, dimethylethanolamine and N,N-dimethylethanolamine; cyclic amines such as pyridine, piperidine, piperazine, 1,8-bis(dimethylamino)naphthalene, morpholine and diazabicycloundecene (DBU); diethylenetriamine and N,N-dimethylbenzylamine, and one or more of them can be used.
[0119] Among them, when a hydrophobic amine having a long-chain alkyl group is used, greater electrostatic repulsion and steric repulsion can be obtained, so it is preferred from the perspective of easily ensuring polymerization stability even when the monomer concentration is high. Specifically, the higher the value (C / N) represented by the ratio of the number of carbon atoms to the number of nitrogen atoms present in the organic amine compound, the higher the polymerization stabilization effect based on the steric repulsion effect. The above C / N value is preferably 3 or more, more preferably 5 or more, further preferably 10 or more, and further preferably 20 or more.
[0120] The usage amount of the basic compound is preferably set to the range of 0.001 mol % or more and 4.0 mol % or less relative to the above-mentioned ethylenically unsaturated carboxylic acid monomer. If the usage amount of the basic compound is within this range, polymerization reaction can be carried out smoothly. The usage amount can be 0.05 mol % or more and 4.0 mol % or less, 0.1 mol % or more and 4.0 mol % or less, 0.1 mol % or more and 3.0 mol % or less, or 0.1 mol % or more and 2.0 mol % or less.
[0121] It should be noted that in the present specification, the amount of the basic compound used indicates the molar concentration of the basic compound used relative to the ethylenically unsaturated carboxylic acid monomer, and does not refer to the degree of neutralization. That is, the valence of the basic compound used is not taken into consideration.
[0122] The polymerization initiator can use azo compounds, organic peroxides, inorganic peroxides and other known polymerization initiators, without particular limitation. The use conditions can be adjusted in a manner to obtain an appropriate amount of free radical generation by known methods such as thermal initiation, redox initiation with a reducing agent, UV initiation, etc. In order to obtain a cross-linked polymer with a long primary chain length, it is preferred to set the conditions in a manner to reduce the amount of free radical generation within the range allowed by the manufacturing time.
[0123] Examples of the azo compounds include 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(N-butyl-2-methylpropionamide), 2-(tert-butylazo)-2-cyanopropane, 2,2'-azobis(2,4,4-trimethylpentane), and 2,2'-azobis(2-methylpropane). One or more of these compounds may be used.
[0124] Examples of the organic peroxide include 2,2-bis(4,4-di-tert-butylperoxycyclohexyl)propane (manufactured by NOF Corporation, trade name “PERTETRA A”), 1,1-di(tert-hexylperoxy)cyclohexane (manufactured by NOF Corporation, trade name “PERHEXA HC”), 1,1-di(tert-butylperoxy)cyclohexane (manufactured by NOF Corporation, trade name “PERHEXA C”), n-butyl-4,4-di(tert-butylperoxy)valerate (manufactured by NOF Corporation, trade name “PERHEXA V”), 2,2-di(tert-butylperoxy)butane (manufactured by NOF Corporation, trade name “PERHEXA 22”), tert-butyl hydroperoxide (manufactured by NOF Corporation, trade name “PERBUTYL H”), cumene hydroperoxide (manufactured by NOF Corporation, trade name “PERCUMYL H”), 1,1,3,3-tetramethylbutyl hydroperoxide (manufactured by NOF Corporation, trade name “PEROCTA H”), tert-butyl cumyl peroxide (manufactured by NOF Corporation, trade name “PERBUTYL C”), di-tert-butyl peroxide (manufactured by NOF Corporation, trade name “PERBUTYL D”), di-tert-hexyl peroxide (manufactured by NOF Corporation, trade name “PERHEXYL D”), di(3,5,5-trimethylhexanoyl) peroxide (manufactured by NOF Corporation, trade name “PEROYL 355”), dilauroyl peroxide (manufactured by NOF Corporation, trade name “PEROYL L”), bis(4-tert-butylcyclohexyl) peroxydicarbonate (manufactured by NOF Corporation, trade name “PEROYL TCP”), di-2-ethylhexyl peroxydicarbonate (manufactured by NOF Corporation, trade name “PEROYL OPP”), di-sec-butyl peroxydicarbonate (manufactured by NOF Corporation, trade name “PEROYL SBP”), cumyl peroxyneodecanoate (manufactured by NOF Corporation, trade name “PERCUMYL ND”), 1,1,3,3-tetramethylbutyl peroxyneodecanoate (manufactured by NOF Corporation, trade name “PEROCTA ND”), tert-hexyl peroxyneodecanoate (manufactured by NOF Corporation, trade name “PERHEXYL ND”), tert-butyl peroxyneodecanoate (manufactured by NOF Corporation, trade name “PERBUTYL ND”), tert-butyl peroxyneoheptanoate (manufactured by NOF Corporation, trade name “PERBUTYL NHP”), tert-hexyl peroxypivalate (manufactured by NOF Corporation, trade name “PERHEXYL PV”), tert-butyl peroxypivalate (manufactured by NOF Corporation, trade name “PERBUTYL PV”), 2,5-dimethyl-2,5-di(2-ethylhexanoyl)hexane (manufactured by NOF Corporation, trade name “PERHEXA 250”), 1,1,3,3-Tetramethylbutylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name "PEROCTA O"), tert-hexylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name "PERHEXYL O"), tert-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name "PERBUTYL O"), tert-butylperoxylaurate (manufactured by NOF Corporation, trade name "PERBUTYL L"), tert-butylperoxy-3,5,5-trimethylhexanoate (manufactured by NOF Corporation, trade name "PERBUTYL 355"), tert-hexylperoxyisopropylmonocarbonate (manufactured by NOF Corporation, trade name "PERHEXYL I"), tert-butylperoxyisopropylmonocarbonate (manufactured by NOF Corporation, trade name "PERBUTYL I"), tert-butylperoxy-2-ethylhexylmonocarbonate (manufactured by NOF Corporation, trade name "PERBUTYL E”), tert-butyl peroxyacetate (manufactured by NOF Corporation, trade name “PERBUTYL A”), tert-hexyl peroxybenzoate (manufactured by NOF Corporation, trade name “PERHEXYL Z”) and tert-butyl peroxybenzoate (manufactured by NOF Corporation, trade name “PERBUTYL Z”), etc., and one or more of them can be used.
[0125] Examples of the inorganic peroxide include potassium persulfate, sodium persulfate, and ammonium persulfate.
[0126] In addition, in the case of redox initiation, sodium sulfite, sodium thiosulfate, sodium formaldehyde sulfoxylate, ascorbic acid, sulfur dioxide gas (SO2), ferrous sulfate, etc. can be used as the reducing agent.
[0127] When the total amount of the monomer components used is set to 100 parts by mass, the preferred amount of the polymerization initiator used is, for example, 0.001 to 2 parts by mass, for example, 0.005 to 1 part by mass, and for example, 0.01 to 0.1 parts by mass. If the amount of the polymerization initiator used is 0.001 parts by mass or more, the polymerization reaction can be stably carried out, and if it is 2 parts by mass or less, a polymer with a long primary chain length can be easily obtained.
[0128] The polymerization temperature depends on conditions such as the type and concentration of the monomers used, but is preferably 0 to 100° C., more preferably 20 to 80° C. The polymerization temperature may be constant or may vary during the polymerization reaction.
[0129] The polymer dispersion obtained through the polymerization process is subjected to decompression and / or heat treatment in the drying process to distill off the solvent, so that the target polymer can be obtained in a powder state. At this time, for the purpose of removing unreacted monomers (and their salts), impurities derived from initiators, etc. before the above-mentioned drying process, it is preferred to have a solid-liquid separation process such as centrifugation and filtration after the polymerization process, and a washing process using water, methanol or a solvent that is the same as the polymerization solvent. In the case of the above-mentioned washing process, even if the polymer undergoes secondary coagulation, it is easy to dissociate during use, and the residual unreacted monomers are removed, thereby showing good performance in terms of adhesion and battery characteristics.
[0130] In the present manufacturing method, a polymerization reaction of a monomer composition comprising a monomer represented by the above general formula (1) and an ethylenically unsaturated carboxylic acid monomer different from the above general formula (1) is carried out in the presence of an alkaline compound. Alternatively, an alkaline compound may be added to the polymer dispersion obtained by the polymerization process to neutralize the polymer (hereinafter also referred to as "process neutralization"), and then the solvent may be removed in a drying process. Alternatively, after obtaining the powder of the present polymer without performing the above process neutralization treatment, an alkaline compound may be added during the preparation of an electrode slurry to neutralize the polymer (hereinafter also referred to as "post-neutralization"). Among the above, process neutralization is preferred because there is a tendency for the secondary agglomerates to be easily dissociated.
[0131] <Composition for secondary battery electrode mixture layer>
[0132] The composition for a secondary battery electrode mixture layer of the present invention comprises a binder containing the present polymer or a salt thereof, an active material, and water.
[0133] The amount of the present polymer or its salt used in the electrode composite layer composition of the present invention is, for example, 0.1% by mass or more and 20% by mass or less relative to the total amount of the active material. The above-mentioned amount is, for example, 0.2% by mass or more and 10% by mass or less, for example, 0.3% by mass or more and 8% by mass or less, for example, 0.4% by mass or more and 5% by mass or less. In the case where the amount of the present polymer and its salt is less than 0.1% by mass, sufficient adhesion is sometimes not obtained. In addition, sometimes the dispersion stability of the active material, etc. becomes insufficient, and the uniformity of the formed composite layer is reduced. On the other hand, in the case where the amount of the present polymer and its salt exceeds 20% by mass, sometimes the electrode composite layer composition becomes high viscosity, and the coating property of the collector is reduced. As a result, uneven stripes (Japanese original: ブツ) and concave-convex are produced on the obtained composite layer, and there is concern that the electrode characteristics are adversely affected.
[0134] If the usage amount of this polymer and its salt is within the above-mentioned range, a composition with excellent dispersion stability can be obtained, and a mixture layer with extremely high adhesion to the collector can be obtained, resulting in improved durability of the battery. In addition, even if the above-mentioned polymer and its salt are a small amount (e.g., less than 5% by mass) relative to the active material, they also show sufficiently high adhesion, and owing to having carboxyl anions, an electrode with little interface resistance and excellent high rate characteristics can be obtained.
[0135] Among the above-mentioned active materials, lithium salts of transition metal oxides can be used as positive electrode active materials, for example, layered rock salt type and spinel type lithium-containing metal oxides can be used. Specific compounds of layered rock salt type positive electrode active materials include lithium cobalt oxide, lithium nickel oxide, and NCM {Li(Ni x ,Co y , Mn z ), x+y+z=1} and NCA{Li(Ni 1-a-b Co a Al b )}, etc. In addition, as the spinel type positive electrode active material, lithium manganate, etc. can be cited. In addition to oxides, phosphates, silicates and sulfur, etc. are also used. As phosphates, olivine type lithium iron phosphate, etc. can be cited. As the positive electrode active material, one of the above can be used alone, or two or more can be combined and used in the form of a mixture or a composite.
[0136] It should be noted that, when the positive electrode active material of the lithium-containing metal oxide of the layered rock salt type is dispersed in water, the lithium ions on the surface of the active material are exchanged with the hydrogen ions in the water, so that the dispersion shows alkalinity. Therefore, aluminum foil (Al) as a common positive electrode collector material is likely to be corroded. In such a case, it is preferred to use an unneutralized or partially neutralized polymer as a binder to neutralize the alkali component dissolved from the active material. In addition, the usage amount of the unneutralized or partially neutralized polymer is preferably used in a manner that the unneutralized carboxyl amount of the polymer is equivalent to or more than the alkali amount dissolved from the active material.
[0137] The electrical conductivity of the positive electrode active material is low, so a conductive aid is usually added for use. As the conductive aid, carbon materials such as carbon black, carbon nanotubes, carbon fibers, graphite powder, and carbon fibers can be cited, among which carbon black, carbon nanotubes, and carbon fibers are preferred from the perspective of easily obtaining excellent electrical conductivity. In addition, as carbon black, Ketjen black and acetylene black are preferred. The conductive aid can be used alone or in combination with two or more. From the viewpoint of taking into account both electrical conductivity and energy density, the amount of the conductive aid used can be set to, for example, 0.2 to 20% by mass relative to the total amount of the active material, and can be set to, for example, 0.2 to 10% by mass. In addition, the positive electrode active material can use a material coated with a conductive carbon material.
[0138] On the other hand, as the negative electrode active material, for example, carbon-based materials, lithium metal, lithium alloys and metal oxides can be cited, and one of them or a combination of two or more thereof can be used. Among them, active materials containing carbon-based materials such as natural graphite, artificial graphite, hard carbon and soft carbon (hereinafter also referred to as "carbon-based active materials") are preferred, and graphites such as natural graphite and artificial graphite, and hard carbon are more preferred. In addition, in the case of graphite, from the perspective of battery performance, spheroidized graphite is preferably used, and the preferred range of its particle size is, for example, 1 to 20 μm, and another example is 5 to 15 μm. In addition, in order to improve the energy density, metals or metal oxides such as silicon and tin that can absorb lithium can also be used as negative electrode active materials. Among them, silicon has a higher capacity than graphite, and active materials containing silicon-based materials such as silicon oxides such as silicon, silicon alloys and silicon monoxide (SiO) can be used (hereinafter also referred to as "silicon-based active materials"). However, the above-mentioned silicon-based active material has a high capacity, but the volume change accompanying charging and discharging is large. Therefore, it is preferably used in combination with the above-mentioned carbon-based active material. In this case, the amount of the silicon active material used is preferably 2 to 80% by mass relative to the total amount of the carbon active material and the silicon active material. The amount of the silicon active material used may be 5 to 70% by mass, 8 to 60% by mass, or 10 to 50% by mass.
[0139] The present polymer has a structural unit (component (a)) derived from a monomer represented by the above general formula (1) and a structural unit (component (b)) derived from an ethylenically unsaturated carboxylic acid monomer different from the above general formula (1), and components (a) and (b) have high affinity for silicon-based active materials and show good adhesion. Therefore, the binder of the present invention also shows excellent adhesion when using a high-capacity active material containing a silicon-based active material, and is therefore considered to be effective in improving the durability of the resulting electrode.
[0140] In addition, from the aspect of being able to suppress or reduce the viscosity increase of the electrode slurry, the present polymer is preferably a cross-linked polymer having a structural unit (component (c)) derived from a specific monomer having a hydroxyl group. The reason for obtaining this effect is not clear, but it is speculated that since the present polymer has a relatively flexible hydroxyl group in the side chain of the polymer, it interacts with the carboxyl group in the present polymer, resulting in the expansion of the cross-linked polymer in water being suppressed. However, the above speculation does not limit the scope of the present invention.
[0141] Since the carbon-based active material itself has good electrical conductivity, it is not necessary to add a conductive additive. In the case where a conductive additive is added for the purpose of improving cycle characteristics, from the perspective of energy density, its usage amount relative to the total amount of the active material is, for example, 10% by mass or less, and for example, 5% by mass or less.
[0142] When the secondary battery electrode mixture layer composition is in a slurry state, the amount of active material used is, for example, in the range of 10 to 75% by mass relative to the total amount of the composition. If the amount of active material used is 10% by mass or more, the migration of adhesives and the like can be suppressed. In addition, from the aspect that the drying cost of the medium is also advantageous, the amount of active material used is preferably 30% by mass or more, more preferably 40% by mass or more, and further preferably 50% by mass or more. On the other hand, if it is 75% by mass or less, the fluidity and coating properties of the composition can be ensured, and a uniform mixture layer can be formed.
[0143] The secondary battery electrode mixture layer composition uses water as a medium. In addition, for the purpose of adjusting the properties and dryness of the composition, it can also be made into a mixed solvent with lower alcohols such as methanol and ethanol, carbonates such as ethylene carbonate, ketones such as acetone, tetrahydrofuran, N-methylpyrrolidone and other water-soluble organic solvents. The proportion of water in the mixed medium is, for example, 50% by mass or more, and for example, 70% by mass or more.
[0144] When the electrode mixture layer composition is made into a coatable slurry state, the solid content concentration is not limited to about 50 mass %, and from the viewpoint of the coatability of the electrode slurry, the energy cost required for drying and the productivity, the content of the medium containing water in the entire composition can be set in the range of, for example, 25 to 90 mass %, 35 to 70 mass %, or 45 to 70 mass %.
[0145] The adhesive of the present invention can be composed only of the above-mentioned polymer or its salt. In addition, other adhesive components such as styrene / butadiene latex (SBR), acrylic latex and polyvinylidene fluoride latex can also be used in combination. In the case of using other adhesive components, the amount used can be set to 0.1 to 5% by mass or less relative to the active material, for example, it can be set to 0.1 to 2% by mass or less, and for example, it can be set to 0.1 to 1% by mass or less. If the amount of other adhesive components used exceeds 5% by mass, sometimes the resistance increases and the high rate characteristics become insufficient. Among the above, styrene / butadiene latex is preferred from the aspect of excellent balance between adhesion and bending resistance.
[0146] The above-mentioned styrene / butadiene latex refers to an aqueous dispersion of a copolymer having a structural unit derived from an aromatic vinyl monomer such as styrene and a structural unit derived from an aliphatic conjugated diene monomer such as 1,3-butadiene. As the above-mentioned aromatic vinyl monomer, in addition to styrene, α-methylstyrene, vinyltoluene, divinylbenzene, etc. can also be mentioned, and one or more of them can be used. Mainly from the viewpoint of adhesion, the structural unit derived from the above-mentioned aromatic vinyl monomer in the above-mentioned copolymer can be set to the range of 20 to 60 mass %, for example, and can be set to the range of 30 to 50 mass %.
[0147] As the above-mentioned aliphatic conjugated diene monomer, in addition to 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, etc. can also be mentioned, and one or more of them can be used. From the aspect that the adhesiveness of the binder and the flexibility of the obtained electrode become good, the structural unit derived from the above-mentioned aliphatic conjugated diene monomer in the above-mentioned copolymer can be set to the range of 30-70 mass %, and can be set to the range of 40-60 mass %.
[0148] In addition to the above monomers, styrene / butadiene latex may also use nitrile-containing monomers such as (meth)acrylonitrile, and carboxyl-containing monomers such as (meth)acrylic acid, itaconic acid, and maleic acid as comonomers in order to further improve properties such as adhesion.
[0149] The content of the structural unit derived from the other monomer in the copolymer may be, for example, in the range of 0 to 30% by mass, or, for example, in the range of 0 to 20% by mass.
[0150] The composition for the secondary battery electrode mixture layer of the present invention has the above-mentioned active material, water and binder as essential components, and can be obtained by mixing the components using known means. There is no particular limitation on the mixing method of the components, and a known method can be used. It is preferably a method in which the powder components such as the active material, the conductive aid and the present polymer particles as a binder are dry-mixed, and then mixed with a dispersion medium such as water to disperse and knead. In the case of obtaining the electrode mixture layer composition in a slurry state, it is preferably finished into an electrode slurry without poor dispersion and agglomeration. As a mixing means, a planetary mixer, a thin film rotary mixer and a self-rotation revolution mixer and other known mixers can be used. Considering the aspect of obtaining a good dispersion state in a short time, it is preferably carried out using a thin film rotary mixer. In addition, when a thin film rotary mixer is used, it is preferably pre-dispersed in advance with a mixer such as a dispenser. In addition, the viscosity of the above slurry can be set to a range of 500 to 10,000 mPa·s, for example. From the viewpoint of coating properties of the electrode slurry, the upper limit of the viscosity is preferably 7,000 mPa·s or less, more preferably 6,000 mPa·s or less, further preferably 5,000 mPa·s or less, further preferably 4,000 mPa·s or less, and still more preferably 3,000 mPa·s or less. It should be noted that the slurry viscosity can be measured by the method described in the Examples at a liquid temperature of 25°C.
[0151] On the other hand, when the electrode material mixture layer composition is obtained in a wet powder state, it is preferably kneaded by a Henschel mixer, a stirrer, a planetary mixer, a twin-screw kneader or the like until it reaches a uniform state without concentration unevenness.
[0152] <Secondary battery electrode and secondary battery>
[0153] The secondary battery electrode of the present invention is formed by having a mixture layer formed by the above-mentioned electrode mixture layer composition on the surface of a current collector such as copper or aluminum. The mixture layer is formed by drying and removing a medium such as water after applying the electrode mixture layer composition of the present invention on the surface of the current collector. The method for coating the electrode mixture layer composition is not particularly limited, and known methods such as a blade coating method, a dipping method, a roller coating method, a comma coating method, a curtain coating method, a gravure coating method, and an extrusion method can be used. In addition, the above-mentioned drying can be carried out by known methods such as warm wind blowing, decompression, (far) infrared rays, microwave irradiation, etc.
[0154] Usually, the composite layer obtained after drying is subjected to compression treatment based on mold pressing, roller pressing, etc. The active material and the binder can be closely attached by compression, and the strength of the composite layer and the close adhesion with the collector can be improved. By compression, the thickness of the composite layer can be adjusted to, for example, about 30 to 80% before compression, and the thickness of the composite layer after compression is usually about 4 to 200 μm.
[0155] The secondary battery electrode of the present invention can be provided with a separator and an electrolyte to produce a secondary battery. The electrolyte may be in a liquid state or a gel state.
[0156] The separator is arranged between the positive electrode and the negative electrode of the battery, and is responsible for preventing the short circuit caused by the contact between the two electrodes, maintaining the electrolyte and ensuring the ionic conductivity. The separator is preferably a film-like insulating microporous film with good ion permeability and mechanical strength. As specific raw materials, polyolefins such as polyethylene and polypropylene, polytetrafluoroethylene, etc. can be used.
[0157] The electrolyte can use a commonly used known electrolyte according to the type of active material. In lithium-ion secondary batteries, as specific solvents, cyclic carbonates with high dielectric constants and high electrolyte solubility such as propylene carbonate and ethylene carbonate, and low-viscosity chain carbonates such as ethyl methyl carbonate, dimethyl carbonate and diethyl carbonate can be cited, which can be used alone or as a mixed solvent. The electrolyte is used by dissolving lithium salts such as LiPF6, LiSbF6, LiBF4, LiClO4, and LiAlO4 in these solvents. In nickel-hydrogen secondary batteries, potassium hydroxide aqueous solution can be used as an electrolyte. The secondary battery is obtained by making the positive plate and the negative plate separated by the separator into a winding or stacked structure, and accommodating them in a shell, etc.
[0158] As described above, the adhesive for secondary battery electrodes disclosed in this specification shows excellent adhesion to the electrode material and excellent adhesion to the collector in the mixture layer. Therefore, it is expected that the secondary battery with the electrode obtained by using the above-mentioned adhesive can ensure good integrity, even if it is repeatedly charged and discharged, it also shows good durability (cycle characteristics), and is suitable for vehicle-mounted secondary batteries, etc.
[0159] Example
[0160] Hereinafter, the present invention will be specifically described based on examples. It should be noted that the present invention is not limited to these examples. It should be noted that, hereinafter, unless otherwise specified, "parts" and "%" refer to parts by mass and mass %.
[0161] In the following examples, evaluation of the carboxyl group-containing polymer (salt) was carried out by the following method.
[0162] (1) Water swelling at pH 8
[0163] The water swelling degree at pH 8 was measured by the following method. The measuring apparatus is shown in Figure 1 .
[0164] The measuring device is Figure 1 It is composed of <1>~<3>.
[0165] <1> It comprises a burette 1 with a branch tube for exhausting air, a spring clamp 2, a silicon tube 3 and a polytetrafluoroethylene tube 4.
[0166] <2> The funnel 5 is provided with a support cylinder 8 having a large number of holes on the bottom surface, and a filter paper 10 for the device is further provided thereon.
[0167] <3> A sample 6 (measurement sample) of a carboxyl group-containing polymer or a salt thereof is sandwiched between two pieces of sample fixing filter paper 7, and the sample fixing filter paper is fixed by an adhesive tape 9. All the filter papers used are ADVANTEC No. 2, with an inner diameter of 55 mm.
[0168] <1> and <2> are connected via a silicon tube 3 .
[0169] The funnel 5 and the support cylinder 8 are fixed at a height relative to the burette 1, and the lower end of the polytetrafluoroethylene tube 4 provided inside the burette branch is set at the same height as the bottom surface of the support cylinder 8 ( Figure 1 ).
[0170] The measurement method is described below. The following operations were performed at 25°C unless otherwise specified.
[0171] Remove the spring clamp 2 at <1>, add ion exchange water adjusted to pH 8.0 from the upper part of the burette 1 through the silicon tube 3, and form a state where the burette 1 to the filter paper 10 for the device is filled with ion exchange water 12. Next, close the spring clamp 2, and remove air from the polytetrafluoroethylene tube 4 connected to the burette branch tube through the rubber stopper. In this way, the ion exchange water 12 is continuously supplied from the burette 1 to the filter paper 10 for the device.
[0172] Next, after removing the excess ion exchange water 12 that has seeped out of the filter paper 10 for the device, the scale reading (a) of the burette 1 is recorded.
[0173] Weigh 0.1 to 0.2 g of the dry powder of the measurement sample and place it evenly in the center of the sample fixing filter paper 7 as shown in <3>. Use another piece of filter paper to sandwich the sample, and fix the two filter papers with adhesive tape 9 to fix the sample. Place the filter paper with the fixed sample on the device filter paper 10 shown in <2>.
[0174] Next, the reading of the scale of the burette 1 after 30 minutes have passed from the time when the cap 11 was placed on the filter paper 10 for the device is recorded (b).
[0175] The total (c) of the water absorption of the measured sample and the water absorption of the two sample fixing filter papers 7 is obtained from (ab). By the same operation, the water absorption (d) of only the two filter papers 7 of the sample not containing the carboxyl group-containing polymer or its salt is measured.
[0176] The above operation was performed and the water swelling degree was calculated according to the following formula: In addition, the solid content used for calculation used the value measured by the method described later.
[0177] Water swelling degree = {dry mass of the measured sample (g) + (c-d)} / {dry mass of the measured sample (g)}
[0178] Here, dry mass of the measured sample (g) = mass of the measured sample (g) × (solid content (%) ÷ 100)
[0179] Here, the method for measuring the solid content is described below.
[0180] Take about 0.5 g of the sample and put it into a weighing bottle with a pre-measured mass [mass of weighing bottle = B (g)]. After accurately weighing it together with the weighing bottle [W0 (g)], place the sample together with the weighing bottle in a windless dryer and dry it at 155°C for 45 minutes. Measure the mass at this time together with the weighing bottle [W1 (g)] and calculate the solid content using the following formula.
[0181] Solid content (%) = (W1-B) / (W0-B) × 100
[0182] (2) Determination of sol fraction
[0183] An aqueous dispersion of a carboxyl-containing polymer (salt) having a concentration of 0.5% by mass was prepared, and after centrifugation at 4,000 rpm for 30 minutes, the supernatant was collected. The supernatant was diluted 15 times with ion exchange water to prepare a measurement sample. The Li (or Na, K) concentration in the measurement sample was measured by ICP emission spectrometry (ICAP 7600 / Thermo Fischer Scientific).
[0184] The sol fraction is calculated by the following formula from the ratio of the Li (or Na, K) concentration [M2 (ppm)] in the above-mentioned measurement sample to the Li (or Na, K) concentration [M1 (ppm)] calculated from the charging value recorded in Table 1.
[0185] Sol fraction (%) = M2 / M1×100
[0186] 《Manufacturing of carboxyl-containing polymer salts》
[0187] (Production Example 1: Production of Carboxyl Group-Containing Polymer Salt R-1)
[0188] For the polymerization, a reactor equipped with a stirring blade, a thermometer, a reflux condenser and a nitrogen inlet pipe was used.
[0189] 567 parts of acetonitrile, 2.20 parts of ion exchange water, 90.0 parts of acrylic acid (hereinafter referred to as "AA"), 10.0 parts of β-carboxyethyl acrylate (hereinafter referred to as "CEAA"), 0.2 parts of trimethylolpropane diallyl ether (manufactured by Daiso, trade name "NEOALLYL T-20"), and 1.0 mol% of triethylamine relative to the above AA were added to the reactor. After the reactor was fully purged with nitrogen, it was heated to raise the internal temperature to 55°C. After confirming that the internal temperature was stable at 55°C, 0.040 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd., trade name "V-65") as a polymerization initiator was added. As a result, white turbidity was confirmed in the reaction liquid, so this point was used as the polymerization initiation point. It should be noted that the calculated monomer concentration was 15.0%. The reaction solution was cooled 12 hours after the polymerization initiation point, and after the internal temperature dropped to 25°C, 49.8 parts of lithium hydroxide monohydrate (hereinafter referred to as "LiOH·H2O") powder was added. After the addition, stirring was continued at room temperature for 12 hours to obtain a slurry-like polymerization reaction solution in which particles of the carboxyl-containing polymer salt R-1 (Li salt, neutralization degree 90 mol%) were dispersed in the medium.
[0190] The obtained polymerization reaction liquid is centrifuged to allow the polymer particles to settle, and the supernatant is removed. Then, the precipitate is redispersed in acetonitrile of the same mass as the polymerization reaction liquid, and the polymer particles are precipitated by centrifugation, and the supernatant is removed, and the washing operation is repeated twice. The precipitate is recovered and dried at 80°C for 3 hours under reduced pressure to remove the volatile components, thereby obtaining a powder of the carboxyl-containing polymer salt R-1. The carboxyl-containing polymer salt R-1 is hygroscopic, so it is sealed and stored in a container with water vapor barrier properties. It should be noted that the powder of the carboxyl-containing polymer salt R-1 is subjected to IR measurement, and the neutralization degree is calculated based on the intensity ratio of the peak of the C=O group derived from the carboxylic acid to the peak of the C=O group derived from the carboxylic acid Li, and the result is equal to the calculated value derived from the feed, which is 90 mol%.
[0191] The water swelling degree was 63.4, and the sol fraction was 30% by mass.
[0192] (Production Examples 2 to 14 and Comparative Production Example 1: Production of Carboxyl Group-Containing Polymer Salts R-2 to R-15)
[0193] The same operation as in Production Example 1 was carried out except that the charge amount of each raw material was set as shown in Table 1, thereby obtaining a polymerization reaction liquid containing carboxyl group-containing polymer salts R-2 to R-15.
[0194] Next, the same operation as in Production Example 1 was carried out on each polymerization reaction solution to obtain powdered carboxyl group-containing polymer salts R-2 to R-15. Each carboxyl group-containing polymer salt was sealed and stored in a container having water vapor barrier properties.
[0195] The physical properties of each of the obtained polymer salts were measured in the same manner as in Production Example 1. The results are shown in Table 1.
[0196] [Table 1]
[0197]
[0198] The details of the compounds used in Table 1 are shown below.
[0199] AA: acrylic acid (purity: 99.9 mass % or more, content of the monomer represented by the general formula (1): less than 0.1 mass %)
[0200] CEAA: β-carboxyethyl acrylate (manufactured by SIGMA-ALDRICH, trade name “2-carboxyethyl acrylate”)
[0201] CEAO: β-carboxyethyl acrylate, n=1 to 3 (manufactured by SIGMA-ALDRICH, trade name “2-carboxyethyl acrylate oligomer”)
[0202] ·HEA: 2-Hydroxyethyl Acrylate
[0203] ·T-20: trimethylolpropane diallyl ether (manufactured by Daiso, trade name "NEOALLYL T-20")
[0204] · P-30: Pentaerythritol triallyl ether (manufactured by Daiso, trade name "NEOALLYL P-30")
[0205] ·TEA: Triethylamine
[0206] AcN: acetonitrile
[0207] ·V-65: 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Wako Pure Chemical Industries, Ltd.)
[0208] ·LiOH·H2O: Lithium hydroxide·monohydrate
[0209] Na2CO3: Sodium carbonate
[0210] K2CO3: Potassium carbonate
[0211] Example 1
[0212] An electrode using the carboxyl group-containing polymer salt R-1 was prepared and evaluated. The specific procedure and evaluation method are shown below.
[0213] (Preparation of composition for electrode mixture layer (electrode slurry))
[0214] A substance obtained by coating carbon on the surface of SiOx (0.8<x<1.2) by CVD method (hereinafter referred to as "Si-based active material") was prepared, and a substance obtained by mixing graphite (manufactured by Nippon Black Lead Co., Ltd., trade name "CGB-10") and Si-based active material was used as active material. Water was used as diluent solvent, and graphite: Si-based active material: R-1 = 90:10:2.8 (solid content) was fully mixed in advance in such a manner that the solid content concentration of the electrode mixture layer composition became 45% by mass. After adding ion exchange water, the mixture was pre-dispersed with a dispenser, and then the main dispersion was performed for 15 seconds using a thin film rotary mixer (manufactured by PRIMIX Co., Ltd., FM-56-30) at a peripheral speed of 20 m / sec, thereby obtaining a slurry-like electrode mixture layer composition (electrode slurry). For the electrode mixture layer composition using each carboxyl-containing polymer salt as a binder, the slurry viscosity and the peel strength between the formed mixture layer / collector (i.e., the adhesiveness of the binder) were measured.
[0215] <Measurement of viscosity of electrode slurry>
[0216] The electrode slurry obtained above was measured using a rheometer (Physica MCR301) manufactured by Anton Paar using a CP25-5 cone plate (diameter 25 mm, cone angle 5°) at a shear rate of 60 s at 25°C. -1 The viscosity of the obtained product was 9,700 mPa·s.
[0217] Next, the electrode slurry was applied onto a copper foil having a thickness of 12 μm using a variable applicator and dried in a ventilated dryer at 100°C for 15 minutes to form a composite layer. Then, the composite layer was prepared to have a thickness of 50 ± 5 μm and a packing density of 1.60 ± 0.10 g / cm 3 The negative electrode plate is obtained by rolling.
[0218] <90° peel strength (adhesion)>
[0219] The mixture layer of the above negative electrode plate with a size of 100mm×25mm was attached to a 120mm×30mm acrylic plate via a double-sided tape (NICETACKNW-20 manufactured by Nichiban Co., Ltd.) to prepare a sample for peeling test. After drying at 60°C and reduced pressure for one night, a tensile tester (Tensilon Universal Testing Material Machine RTE-1210 manufactured by ORIENTEC Co., Ltd.) was used to measure the 90° peeling at a temperature of 25°C and a tensile speed of 50mm / min, and the peel strength between the mixture layer and the copper foil was measured to evaluate the adhesion. The peel strength is as high as 11.4N / m, which is good.
[0220] Examples 2 to 14 and Comparative Example 1
[0221] The negative electrode material layer composition was prepared by the same operation as in Example 1 except that the carboxyl group-containing polymer salt used as the binder was used as shown in Table 2. The slurry viscosity and 90° peel strength of each negative electrode material layer composition were evaluated. The results are shown in Table 2.
[0222] [Table 2]
[0223]
[0224] The results of Examples 1 to 14 show that the electrode slurry containing the binder for secondary battery electrodes of the present invention has a low viscosity, and the peel strength between the mixture layer and the current collector of the obtained electrode is high, showing excellent adhesiveness.
[0225] In contrast, when a polymer salt containing no structural unit derived from the monomer represented by the general formula (1) was used (Comparative Example 1), the viscosity of the electrode slurry was higher than that of the Examples, and the peel strength between the mixture layer of the obtained electrode and the current collector was low.
[0226] Industrial Applicability
[0227] The adhesive for secondary battery electrodes of the present invention can exert better adhesion than before, and can reduce the viscosity of electrode slurry even when the concentration of active material in the electrode mixture layer composition is high. Therefore, it is expected that the secondary battery with the electrode obtained by using the above-mentioned adhesive shows good durability (cycle characteristics), and it is expected to be applied to vehicle-mounted secondary batteries. In addition, it is also useful for the use of active materials containing silicon, and it is expected to contribute to the high capacity of the battery.
[0228] The binder for secondary battery electrodes of the present invention is particularly suitable for use in non-aqueous electrolyte secondary battery electrodes, and is particularly useful for non-aqueous electrolyte lithium ion secondary batteries having a high energy density.
Claims
1. A binder for secondary battery electrodes, comprising a carboxyl-containing polymer or a salt thereof, The carboxyl group-containing polymer or its salt comprises a structural unit derived from a monomer represented by the general formula (1) and a structural unit derived from an ethylenically unsaturated carboxylic acid monomer different from the general formula (1). The carboxyl group-containing polymer or its salt contains 0.1% by mass or more and 20% by mass or less of the structural unit derived from the monomer represented by the general formula (1) relative to all the structural units of the carboxyl group-containing polymer or its salt, The carboxyl group-containing polymer or its salt contains 50% by mass or more and 99.9% by mass or less of the structural unit derived from the ethylenically unsaturated carboxylic acid monomer different from the general formula (1) relative to all structural units thereof, The carboxyl group-containing polymer or its salt does not include a structural unit derived from vinylidene fluoride, 2. The binder for secondary battery electrodes according to claim 1, in, The carboxyl group-containing polymer is a cross-linked polymer obtained by polymerizing a monomer composition containing a non-cross-linking monomer and a cross-linking monomer.
3. The binder for secondary battery electrodes according to claim 2, in, The usage-amount of the said crosslinkable monomer is 0.1 mol% or more and 1.0 mol% or less with respect to the total amount of the said non-crosslinkable monomer.
4. The binder for secondary battery electrodes according to claim 2 or 3, in, The sol fraction of the cross-linked polymer is less than 40% by mass.
5. The binder for secondary battery electrodes according to claim 2 or 3, in, The cross-linked polymer has a water swelling degree of 4.0 or more and 60 or less at pH 8.
6. The binder for secondary battery electrodes according to claim 2 or 3, in, The crosslinkable monomer includes a compound having two or more allyl ether groups in the molecule. 7 . A composition for a secondary battery electrode mixture layer, comprising the binder for a secondary battery electrode according to claim 1 , an active material, and water. 8 . A secondary battery electrode comprising an electrode mixture layer containing the binder for secondary battery electrodes according to claim 1 on a surface of a current collector. 9 . A secondary battery comprising the secondary battery electrode according to claim 8 .
Citation Information
Patent Citations
Binder for lithium cell, composition for producing electrode, and electrode
WO2014065407A1
Negative-electrode mixture for non-aqueous electrolyte secondary cell, negative electrode for non-aqueous electrolyte secondary cell containing said mixture, non-aqueous electrolyte secondary cell provided with said negative electrode, and electrical device
WO2014207967A1
Paste composition for negative electrode for lithium-ion rechargeable battery, composite particles for negative electrode for lithium-ion rechargeable battery, slurry composition for negative electrode for lithium-ion rechargeable battery, negative electrode for lithium-ion rechargeable battery, and lithium-ion rechargeable battery
WO2016067633A1
Binder for nonaqueous electrolyte secondary cell electrode, method for producing binder, and use thereof
WO2017073589A1
Binder for nonaqueous secondary batteries, composition for nonaqueous secondary battery functional layers, functional layer for nonaqueous secondary batteries, and nonaqueous secondary battery
CN107004859A