Organic shrinkage-proofing agent for lead-acid battery and method for producing the same

By ultrafiltration treatment of sulfurous acid/sulfite cooking black liquor, an organic anti-shrinkage agent containing lignosulfonic acid is prepared, which solves the problem of reduced charge acceptance of lead-acid batteries and achieves improved charging performance while maintaining discharge characteristics. .

CN114514640BActive Publication Date: 2024-10-29NIPPON PAPER IND CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202180005514.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-08
Publication Date
2024-10-29
Estimated Expiration
2041-03-08

AI Technical Summary

Technical Problem

During the repeated charging and discharging process of lead-acid batteries, the shrinkage of the negative active material causes the discharge performance to decrease, and the charging performance becomes worse when the lead sulfate becomes coarse. Although the existing lignin addition improves the discharge performance, the charge acceptance decreases.

Method used

The sulfurous acid/sulfite cooking black liquor is subjected to ultrafiltration using an ultrafiltration membrane, and the content of substances with a molecular weight of 5000 or less is 30% by mass or less, and the concentrated liquid contains lignosulfonic acid as an organic anti-shrinkage agent for lead storage batteries, And the reducing sugar content per unit solid content is 5 mass% or less.

Benefits of technology

Maintaining the discharge characteristics of lead-acid batteries while improving charge acceptance improves the overall performance of lead-acid batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003565205660000121
    Figure BDA0003565205660000121
  • Figure BDA0003565205660000141
    Figure BDA0003565205660000141
Patent Text Reader

Abstract

The present invention provides an organic shrinkage-proofing agent for lead-acid batteries and a method for producing the same: an organic shrinkage-proofing agent for lead-acid batteries, which is an organic shrinkage-proofing agent for lead-acid batteries containing lignin sulfonic acid, characterized in that the content of reducing sugars per unit solid content is less than 5% by mass of the whole, and the content of substances with a molecular weight of less than 5000 per unit solid content is less than 30% by mass of the whole; and a method for producing an organic shrinkage-proofing agent for lead-acid batteries, characterized in that the method for producing an organic shrinkage-proofing agent for lead-acid batteries comprises: using an ultrafiltration membrane to ultrafilter sulfurous acid / sulfite cooking black liquor, and recovering the concentrated liquid of the obtained sulfurous acid / sulfite cooking black liquor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an organic shrinkage-proofing agent for lead-acid batteries. Background Art

[0002] Lead storage batteries are relatively inexpensive and have stable performance as secondary batteries, and therefore have been widely used as batteries for automobiles, batteries for portable devices, backup batteries for computers, batteries for communications, and the like.

[0003] When a lead-acid battery changes from a discharge state to a charge state during repeated charge and discharge, the negative electrode active material shrinks, the specific surface area decreases, and the discharge performance deteriorates. In addition, in the negative electrode active material, metal lead releases electrons in the discharge reaction and changes into lead sulfate, and in the charge reaction, the lead sulfate gains electrons and changes into metal lead. However, when the lead sulfate is coarsened, it is difficult to dissolve in the charge reaction, and the charge performance deteriorates.

[0004] As an organic shrinkage-preventing agent to be added to a negative electrode active material of a lead-acid battery in order to prevent shrinkage of the negative electrode active material, it has been proposed to add lignin extracted from wood (Patent Documents 1 to 3).

[0005] In addition, various lignins are disclosed as lignin for lead-acid batteries (Patent Documents 4 to 11).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: U.S. Patent No. 2371136

[0009] Patent Document 2: U.S. Patent No. 3523041

[0010] Patent Document 3: Japanese Patent Application Laid-Open No. 62-145655

[0011] Patent Document 4: Japanese Patent Application Publication No. 2002-117856

[0012] Patent Document 5: WO2002 / 039519

[0013] Patent Document 6: Japanese Patent Application Publication No. 2005-294027

[0014] Patent Document 7: Japanese Patent Application Publication No. 2007-165273

[0015] Patent Document 8: Japanese Patent Application Laid-Open No. 11-204111

[0016] Patent Document 9: Japanese Patent Application Laid-Open No. 9-007630

[0017] Patent Document 10: U.S. Patent No. 6346347

[0018] Patent Document 11: U.S. Patent No. 6664002 Summary of the invention

[0019] Problems to be solved by the invention

[0020] Lead acid batteries are required to have various performances. Generally, when lignin is added to the negative electrode of a lead acid battery, although effects such as improving high rate discharge performance and inhibiting sulfation can be obtained, there is a problem that the charge acceptance is reduced due to its properties.

[0021] An object of the present invention is to provide an organic shrinkage preventing agent capable of improving the charge acceptance while maintaining the discharge characteristics of the above-mentioned lead-acid battery.

[0022] Means for solving problems

[0023] The present inventors have conducted intensive studies on the above-mentioned problems and have found that the above-mentioned problems can be solved by ultrafiltration treatment of sulfurous acid / sulfite (i.e., sulfurous acid and / or sulfite) cooking black liquor using an ultrafiltration membrane to reduce the content of substances with a molecular weight of 5,000 or less to 30% by mass of the total, and using the resulting concentrated liquid as an organic shrinkage-proofing agent for lead-acid batteries, thereby completing the present invention.

[0024] That is, the present inventors provided the following [1] and [2].

[0025] [1] A method for producing an organic shrinkage-proofing agent for lead-acid batteries, comprising producing an organic shrinkage-proofing agent for lead-acid batteries containing lignin sulfonic acid, the method comprising: subjecting sulfurous acid / sulfite cooking black liquor to ultrafiltration treatment using an ultrafiltration membrane, and recovering a concentrated solution of the obtained sulfurous acid / sulfite cooking black liquor.

[0026] [2] An organic shrinkage-proofing agent for a lead-acid battery, comprising lignin sulfonic acid, characterized in that the content of reducing sugars per unit solid content is less than 5% by mass of the total, and the content of substances with a molecular weight of 5,000 or less per unit solid content is less than 30% by mass of the total.

[0027] Effects of the Invention

[0028] According to the present invention, the charge acceptance can be improved while maintaining the discharge characteristics of the lead storage battery. DETAILED DESCRIPTION

[0029] Hereinafter, the present invention will be described in detail with reference to preferred embodiments. However, the present invention is not limited to the following embodiments.

[0030] <Organic shrinkage-proofing agent>

[0031] The organic shrinkage-proofing agent of the present invention preferably contains lignin having a methoxyl content of 3% to 20% by mass per unit solid content. When the methoxyl content is less than 3%, the effect as an organic shrinkage-proofing agent cannot be confirmed due to the small amount of lignin contained. Generally speaking, since methoxyl groups bonded to aromatic rings are present in lignin, the methoxyl content becomes an indicator of the lignin content.

[0032] In the present invention, the methoxy group content is a value measured by a methoxy group quantitative method according to the Viebock and Schwappach method (see "Lignin Chemical Research Methods", pp. 336-340, 1997, published by Uni Publishing Co., Ltd.).

[0033] There are several types of lignin used in the organic shrinkage preventing agent for lead-acid batteries according to the present invention, because the obtained lignin differs depending on the method of treating woody biomass.

[0034] As the lignin used in the present invention, the following lignins can be cited. For example, there are: lignin sulfonic acid, sulfate lignin, alkali lignin, alkali-anthraquinone lignin, organic solvent type lignin, blasted lignin, sulfate lignin, etc. Among them, lignin sulfonic acid is preferably used. It is particularly preferable to use oxylignin (oxylignin) which is partially desulfonated by subjecting lignin sulfonic acid to a high temperature and high pressure reaction under alkaline conditions as described in U.S. Patent No. 6,346,347.

[0035] The lignin used in the present invention may be in powder or liquid form, but is preferably in powder form. As liquid lignin, for example, the powdered lignin may be dissolved in a suitable solvent (e.g., water, sodium hydroxide aqueous solution, etc.) to make liquid lignin.

[0036] The lignin used in the present invention may be one of the above-mentioned lignins or a mixture of two or more thereof.

[0037] Hereinafter, lignin sulfonic acid used in the present invention will be described in detail, but the present invention is not limited to these lignins.

[0038] (Lignin sulfonic acid)

[0039] Lignosulfonic acid refers to a compound in which at least a part of lignin or its decomposition product is substituted with a sulfonic acid (salt) group. The S content of the sulfonic acid (salt) group of the ligninsulfonic acid of the present invention is usually 1.0% by mass to 10.0% by mass.

[0040] The S content of the sulfonic acid (salt) group of lignin sulfonic acid means the S content contained in the sulfonic acid (salt) group relative to the solid content of lignin sulfonic acid. Specifically, it is a value calculated according to the following formula (1).

[0041] Formula (1):

[0042] Sulfonic acid (salt) group S content (mass %) = total S content (mass %) - inorganic S content (mass %)

[0043] (In the formula (1), the S content indicates the S content relative to the solid content of lignin sulfonic acid.)

[0044] In formula (1), the total S content can be quantified by ICP emission spectrometry. Alternatively, the inorganic S content can be calculated as the total amount of the SO 3 content and the SO 4 content quantified by ion chromatography.

[0045] The organic shrinkage-proofing agent for lead-acid batteries containing lignin sulfonic acid of the present invention contains reducing sugars. Reducing sugars usually remain in the process of sulfurous acid / sulfite cooking of woody biomass. The content of reducing sugars is preferably 5% by mass or less, more preferably 3% by mass or less. By making the content of reducing sugars 5% by mass or less, the charge acceptance can be improved while maintaining the discharge characteristics of the lead-acid battery.

[0046] The reducing sugar refers to a sugar showing reducing property, and refers to a sugar that generates an aldehyde group or a ketone group in an alkaline solution.

[0047] As reducing sugars, for example, all monosaccharides; disaccharides such as maltose, lactose, arabinose, and invert sugar of sucrose; and polysaccharides can be listed. As reducing sugars contained in the alkali-treated wastewater, cellulose, hemicellulose, and their decomposition products are generally included. As decomposition products of cellulose and hemicellulose, for example, monosaccharides such as rhamnose, galactose, arabinose, xylose, glucose, mannose, and fructose; oligosaccharides such as xylo-oligosaccharides and cellooligosaccharides can be listed.

[0048] Reducing sugars can be measured by the Somogyi-Schaffer method, and the measured value can be converted into a glucose amount to determine the reducing sugar content.

[0049] The lignin sulfonic acid may be in an unionized state or the hydrogen atoms of the sulfonic acid groups may be replaced by counter ions.

[0050] Examples of the counter ion include a sodium ion, a calcium ion, a magnesium ion, and an ammonium ion.

[0051] It should be noted that the counter ion may be a single counter ion or a combination of two or more counter ions.

[0052] The lignin sulfonic acid of the present invention usually contains an inorganic salt. Examples of the inorganic salt include sodium sulfate, sodium sulfite, sodium chloride, magnesium sulfate, magnesium sulfite, magnesium chloride, calcium sulfate, calcium sulfite, calcium chloride, ammonium sulfate, ammonium sulfite, ammonium chloride, and sodium hydroxide. The content of the inorganic salt in the lignin sulfonic acid is usually 1% to 25% by mass.

[0053] (Method for preparing lignin sulfonic acid)

[0054] Lignosulfonic acid with a low degree of sulfonation can be prepared, for example, as follows: It can be prepared by subjecting a lignocellulose raw material to a sulfite treatment, preferably subjecting the lignocellulose raw material to a sulfite / sulfite cooking treatment.

[0055] The lignocellulose raw material is not particularly limited as long as it contains lignocellulose in the structure, and examples thereof include pulp raw materials such as wood and non-wood.

[0056] Examples of the wood include coniferous wood such as broad-scale pine, red pine, Japanese cedar, and cypress, and broad-leaved wood such as white birch and beech. The age of the wood and the part where it was collected are not limited. Therefore, wood collected from trees of different ages and wood collected from different parts of the tree can be used in combination.

[0057] Examples of non-wood include bamboo, kenaf, reed, and rice.

[0058] As the lignocellulose raw material, one of these materials may be used alone, or two or more of them may be used in combination.

[0059] Sulfite treatment can be carried out by contacting at least one of sulfurous acid and sulfite with the lignocellulosic raw material, and is a treatment to obtain an intermediate product. The conditions for sulfite treatment are not particularly limited, and may be conditions that can introduce a sulfonic acid (salt) group on the α carbon atom of the side chain of lignin contained in the lignocellulosic raw material.

[0060] The sulfite treatment is preferably carried out by a sulfite / sulfite (i.e., sulfurous acid and / or sulfite) cooking method. This allows the lignin in the lignocellulosic raw material to be sulfonated more quantitatively. It should be noted that the sulfite / sulfite cooking method is also called a sulfite cooking method.

[0061] The sulfurous acid / sulfite cooking method is a method of reacting a lignocellulosic raw material at a high temperature in a solution of at least one of sulfurous acid and sulfite (e.g., an aqueous solution: cooking liquor). This method has been established and implemented industrially as a method for producing sulfurous acid / sulfite pulp. Therefore, by performing sulfurous acid treatment by the sulfurous acid / sulfite cooking method, economic efficiency and ease of implementation can be improved.

[0062] As the salt of the sulfite, in the case of sulfurous acid / sulfite cooking, for example, magnesium salt, calcium salt, sodium salt, and ammonium salt can be mentioned.

[0063] The concentration of sulfurous acid (SO2) in the solution of at least one of sulfurous acid and sulfite is not particularly limited, and the ratio of the mass (g) of SO2 to 100 mL of the reaction chemical liquid is preferably 1 g / 100 mL or more, and in the case of sulfurous acid / sulfite cooking, it is more preferably 2 g / 100 mL or more. The upper limit is preferably 20 g / 100 mL or less, and in the case of sulfurous acid / sulfite cooking, it is more preferably 15 g / 100 mL or less. The SO2 concentration is preferably 1 g / 100 mL to 20 g / 100 mL, and in the case of sulfurous acid / sulfite cooking, it is more preferably 2 g / 100 mL to 15 g / 100 mL.

[0064] The pH value of the sulfite treatment is not particularly limited, but is preferably 10 or less, and more preferably 5 or less when sulfurous acid / sulfite cooking is performed. The lower limit of the pH value is preferably 0.1 or more, and more preferably 0.5 or more when sulfurous acid / sulfite cooking is performed. The pH value during the sulfite treatment is preferably 0.1 to 10, and more preferably 0.5 to 5 when sulfurous acid / sulfite cooking is performed.

[0065] The temperature of the sulfiting is not particularly limited, but is preferably 170°C or lower, and more preferably 150°C or lower when sulfurous acid / sulfite cooking is performed. The lower limit is preferably 70°C or higher, and more preferably 100°C or higher when sulfurous acid / sulfite cooking is performed. The temperature conditions of the sulfiting are preferably 70°C to 170°C, and more preferably 100°C to 150°C when sulfurous acid / sulfite cooking is performed.

[0066] The treatment time of the sulfite treatment is not particularly limited and depends on various conditions of the sulfite treatment, but is preferably 0.5 to 24 hours, more preferably 1.0 to 12 hours.

[0067] It is preferred to add a compound that provides a counter cation (salt) during the sulfite treatment. By adding a compound that provides a counter cation, the pH value during the sulfite treatment can be kept constant. Examples of compounds that provide a counter cation include MgO, Mg(OH)2, CaO, Ca(OH)2, CaCO3, NH3, NH4OH, NaOH, NaHCO3, and Na2CO3. The counter cation is preferably a magnesium ion.

[0068] In the sulfite treatment, when a solution of at least one of sulfurous acid and sulfite is used, the solution may contain a cooking penetrant (e.g., cyclic ketone compounds such as anthraquinone sulfonate, anthraquinone, and tetrahydroanthraquinone) in addition to SO2 and counter cations (salts) as needed.

[0069] The equipment used for the sulfite treatment is not limited, and for example, a generally known dissolving pulp production equipment or the like can be used.

[0070] The separation of the intermediate product from the solution of at least one of sulfurous acid and sulfite can be carried out according to a conventional method. For example, the separation method includes a method for separating a sulfurous acid / sulfite digestion effluent after sulfurous acid / sulfite digestion.

[0071] By sulfurous acid / sulfite cooking treatment, lignin sulfonic acid with a high degree of sulfonation can sometimes be obtained. In this case, lignin sulfonic acid with a lower degree of sulfonation can be obtained by partial desulfonation treatment. As a partial desulfonation method, the method described in U.S. Patent No. 2371136 and Japanese Patent Application Laid-Open No. 58-45287 can be cited, but it is not limited to these methods.

[0072] In addition, lignin sulfonic acid having a low degree of sulfonation can also be obtained by the method described in Japanese Patent Application Laid-Open No. 2016-135834.

[0073] The method for producing an organic shrinkage-proofing agent containing lignin sulfonic acid of the present invention comprises the step of ultrafiltration treatment of sulfurous acid / sulfite cooking black liquor using an ultrafiltration membrane (UF membrane) and recovery of concentrated liquid.

[0074] By ultrafiltration of black liquor using a UF membrane, liquid lignin can be recovered as a component of the concentrate. In addition, high molecular weight lignin and other substances can be separated by ultrafiltration. That is, liquid lignin can be produced from black liquor using a UF membrane.

[0075] (UF membrane)

[0076] As the UF membrane, a known UF membrane can be used, and examples thereof include a hollow fiber membrane, a spiral membrane, a tubular membrane, and a flat membrane.

[0077] The UF membrane can be made of a known material, such as cellulose acetate, aromatic polyamide, polyvinyl alcohol, polysulfone, polyvinylidene fluoride, polyethylene, polyacrylonitrile, and ceramics. It should be noted that the UF membrane may be a commercially available product.

[0078] The molecular weight cutoff of the UF membrane is preferably 5000 to 30000, more preferably 10000 to 25000, and further preferably 15000 to 23000. When a UF membrane with a molecular weight cutoff of 5000 or more is used, the separation rate of the black liquor can be prevented from being too slow. In addition, when a UF membrane with a molecular weight cutoff of 30000 or less is used, lignin can be prevented from not being separated from the black liquor.

[0079] The ultrafiltration process using the UF membrane is divided into two steps: concentration and volume fixing. Only one of the two steps can be performed, or both can be performed. When both are performed, it is preferred to perform volume fixing after concentration.

[0080] The concentration ratio of the ultrafiltration treatment using the UF membrane can be set arbitrarily. That is, the ultrafiltration treatment can be stopped when the outflow of the permeate reaches an arbitrary amount. It is preferably concentrated to 2 to 6 times. For example, 4 times concentration means a treatment when the amount of permeate passing through the UF membrane reaches 3 / 4 of the amount of the liquid before treatment.

[0081] The constant volume ratio of the ultrafiltration treatment using the UF membrane can be set arbitrarily. That is, water can be added while keeping the volume of the concentrate constant, and the ultrafiltration treatment is stopped when the permeate reaches an arbitrary amount. It is preferred to add 0.5 to 3 times the amount of water to the concentrate for constant volume. For example, 2 times constant volume means that water is added to the stock solution while keeping the amount of the stock solution (black liquor) constant for ultrafiltration treatment, and the permeate amount reaches 2 times the amount of the stock solution before treatment.

[0082] (Ultrafiltration treatment)

[0083] The temperature of the black liquor during ultrafiltration is not particularly limited, but is preferably 20°C to 80°C, and more preferably 20°C to 70°C in consideration of the heat resistance of the UF membrane material.

[0084] The pH value of the black liquor during ultrafiltration treatment is preferably 2 to 11.

[0085] The solid content concentration (weight / weight) of the black liquor during ultrafiltration treatment is preferably 2% to 30%, more preferably 5% to 15%.

[0086] (Concentrate)

[0087] The content of substances with a molecular weight of 5000 or less in the concentrate is preferably 30% by mass or less, and more preferably 20% by mass or less. If the content of substances with a molecular weight of 5000 or less exceeds 30% by mass, the amount of low molecular weight impurities in the concentrate increases, and the charge acceptance of the lead acid battery cannot be improved.

[0088] The molecular weight of lignin in the concentrated solution after ultrafiltration can be measured by gel permeation chromatography (GPC). The GPC measurement can be performed under the following conditions by a known method of pullulan conversion.

[0089] Measuring device: Made by Tosoh Corporation

[0090] Column used: Shodex Column OH-pak SB-806HQ, SB-804HQ, SB-802.5HQ

[0091] Eluent: 1.0% sodium tetraborate, 0.3% isopropanol in water

[0092] Eluent flow rate: 1.00 mL / min

[0093] Column temperature: 50°C

[0094] Measured sample concentration: 0.2 mass%

[0095] Standard substance: Pullulan (manufactured by Showa Denko K.K.)

[0096] Detector: RI detector (manufactured by Tosoh Corporation)

[0097] Calibration line: Pullulan standard

[0098] The weight average molecular weight of lignin in the concentrated liquid after ultrafiltration is preferably 10,000 to 40,000, more preferably 20,000 to 35,000.

[0099] The content of lignin with a molecular weight of less than 5000 in the concentrated solution can be calculated as follows. First, the concentrated solution is measured by GPC under the above conditions to obtain a GPC chromatogram with peak intensity (mV) as the vertical axis and dissolution time (Retention Time) as the horizontal axis. The baseline is usually from the dissolution start time of the polymer peak to the dissolution end time. In the case where the dissolution end time is not clearly observed, after making the baseline, it is divided at the middle point of the valley between the peaks, and the point is used as the dissolution end time of the polymer peak. The GPC chromatogram of lignin usually does not give a clear peak, so it can be calculated by starting from the dissolution of the polymer peak, taking the polymer dissolution curve containing multiple peaks as one peak, vertically dividing the peak at the position of the molecular weight 5000, and calculating the area ratio.

[0100] The organic shrinkage-proofing agent of the present invention is mainly added to the negative electrode plate of the lead-acid battery, and the addition rate is usually 0.02 mass % to 1.0 mass % relative to the lead powder.

[0101] The lead-acid battery using the organic shrinkage preventing agent for lead-acid batteries of the present invention can be used as a battery for automobiles, a battery for portable devices, a backup battery for computers, a battery for communications, and the like.

[0102] Example

[0103] The present invention will be described in more detail below by way of examples. The following examples are provided to appropriately illustrate the present invention, but are not intended to limit the present invention.

[0104] <Ultrafiltration treatment of black liquor>

[0105] SANX M100 (manufactured by Nippon Paper Industries, Ltd., concentration 12%, main component: lignin sulfonic acid) was concentrated 4 times by ultrafiltration (molecular weight cutoff 20000), fixed to 1.0 times, and the resulting concentrated solution was powdered using a vacuum dryer (105°C, 24 hours), thereby obtaining lignin sulfonic acid powder (Lignin 1). In addition, SANX M100 was concentrated 4 times by ultrafiltration (molecular weight cutoff 12000), fixed to 1.0 times, and the resulting concentrated solution was powdered using a vacuum dryer (105°C, 24 hours), thereby obtaining lignin sulfonic acid powder (Lignin 2). In addition, SANX M100 was powdered without ultrafiltration, thereby obtaining lignin sulfonic acid powder (Lignin 3).

[0106] The physical property values ​​of Lignin 1 to 3 are shown in the following Table 1. In addition, % in Table 1 represents % with respect to the solid content.

[0107] [Table 1]

[0108]

[0109] <Production of Lead Acid Batteries>

[0110] The positive active material paste of the lead-acid battery of this embodiment and the comparative example is manufactured as follows according to Japanese Patent Laid-Open No. 9-237632. First, a lead powder containing 70% to 80% by weight of lead monoxide, 13% by weight of dilute sulfuric acid (specific gravity 1.26:20°C) relative to the lead powder, and 12% by weight of water relative to the lead powder are kneaded to prepare a positive active material paste. About 25 g of the above paste-like positive active material is filled into a current collector comprising a grid body made of lead alloy, and then placed (aged) at 80°C for 24 hours in a nitrogen atmosphere without drying to prepare a positive plate that is not chemically converted.

[0111] Next, lead powder containing 70% to 80% lead monoxide by weight, 13% dilute sulfuric acid (specific gravity 1.26:20°C) relative to the lead powder, 12% water relative to the lead powder, 1.2% barium sulfate and 0.3% organic shrinkage-proofing agent were added and kneaded to prepare a negative electrode active material paste. About 25g of the negative electrode active material paste was filled into a current collector containing a lead alloy grid, and then placed (aged) at 80°C for 24 hours in a nitrogen atmosphere without drying to prepare a non-chemically converted negative electrode plate.

[0112] The negative electrode plate and the positive electrode plate obtained by the above-mentioned manufacturing method were combined to produce a lead-acid battery with a rated capacity of 28Ah-2V.

[0113] (High rate discharge characteristics test)

[0114] A high rate discharge characteristic test of 150 A was carried out in accordance with JIS D5301. The discharge duration was evaluated. The longer the discharge duration, the better the evaluation.

[0115] (Charge acceptance test)

[0116] The charge acceptance test was carried out according to JIS D 5301. The charging current at 10 minutes after the start of charging was evaluated. The higher the current value, the better the evaluation.

[0117] (5-hour rate capacity test)

[0118] A 5-hour rate capacity test was performed in accordance with JIS D 5301. The discharge duration was evaluated. The longer the discharge duration, the better the evaluation.

[0119] The test results are shown in Table 2.

[0120] [Table 2]

[0121]

[0122] As shown in Table 2, the organic shrinkage-proofing agent for lead-acid batteries of the present invention of embodiment 1 and 2 is compared with the organic shrinkage-proofing agent for lead-acid batteries of comparative example, and high rate discharge characteristics are basically the same, and charge acceptance is more excellent. In addition, the organic shrinkage-proofing agent for lead-acid batteries of the present invention of embodiment 1 and 2 is compared with the organic shrinkage-proofing agent for lead-acid batteries of comparative example, and 5 hour rate capacity is also more excellent.

Claims

1. An organic shrinkage-proofing agent for lead-acid batteries, comprising lignin sulfonic acid, characterized in that: The content of reducing sugars per unit solid content is 2.6 to 5% by mass of the whole, and the content of substances with a molecular weight of 5000 or less per unit solid content is 9 to 30% by mass of the whole. The weight average molecular weight of the lignin sulfonic acid is 20,000 to 35,000.

2. A method for producing an organic shrinkage-proofing agent for lead-acid batteries, comprising producing the organic shrinkage-proofing agent for lead-acid batteries containing lignin sulfonic acid according to claim 1, characterized in that: The production method comprises the steps of: ultrafiltration treatment of sulfurous acid / sulfite cooking black liquor using an ultrafiltration membrane, and recovery of the concentrated liquid of the obtained sulfurous acid / sulfite cooking black liquor; The molecular weight cut-off of the ultrafiltration membrane is 15000 to 23000. The ultrafiltration process is divided into two steps: concentration and volume setting. The concentration ratio of the ultrafiltration treatment using the ultrafiltration membrane is 2 to 6 times. The constant volume ratio of the ultrafiltration treatment using the ultrafiltration membrane is: 0.5 to 3 times the amount of water is added to the concentrated liquid to make the constant volume.

Citation Information

Patent Citations

  • Improving method for fluidity of coal-water slurry

    JP1983045287A

  • Sealed lead storage battery

    JP1987145655A

  • Lignin compound to be added to lead-acid battery, its manufacture, and lead-acid battery

    JP1997007630A

  • Plate for lead acid battery and manufacture thereof

    JP1997237632A

  • Lead-acid battery

    JP1999204111A