A preparation method and application of sodium ferrovanadium phosphate material

Through co-precipitation and sintering technology, waste lithium iron phosphate batteries are converted into sodium iron vanadium phosphate materials, which solves the problems of retired battery recycling and lithium resource utilization, and improves the performance and resource efficiency of sodium-ion batteries.

CN114597399BActive Publication Date: 2024-10-18GUANGDONG BRUNP RECYCLING TECH CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210139919.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-15
Publication Date
2024-10-18
Estimated Expiration
2042-02-15

AI Technical Summary

Technical Problem

The recycling and utilization of retired lithium iron phosphate batteries is a difficult problem, especially in the context of how to effectively utilize lithium resources. The development of sodium-ion batteries has become an important demand.

Method used

After crushing the waste lithium iron phosphate battery, acid leaching and oxidation treatment are used to form an iron phosphate solution, and the co-precipitation reaction is carried out with the vanadium-containing solution and alkali solution to generate iron phosphate/iron vanadate eutectic, which is converted into Olivine and orthorhombic structure are combined with sodium source for sintering to prepare sodium vanadium iron phosphate material as the cathode material of sodium ion battery.

Benefits of technology

It realizes the reuse of waste battery resources, improves the specific capacity and element distribution uniformity of the cathode material, avoids the problem of uneven mixing of vanadium and iron, and alleviates the shortage of lithium resources, and the waste liquid can be recycled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114597399B_ABST
    Figure CN114597399B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery material recycling, and discloses a preparation method and application of sodium iron vanadium phosphate material. The preparation method comprises the following steps: crushing the lithium iron phosphate battery, adding acid solution, reacting, solid-liquid separation, obtaining a leachate and a leach residue; removing impurities in the leachate, adding an oxidant, and adjusting the concentration of iron and phosphorus elements, adjusting the pH value to less than 1.5, and obtaining a solution A; adding solution A and a vanadium-containing solution to the acid solution, controlling the pH value to 1.8-2.0, then adding an alkali solution, adjusting the pH value to 2.0-2.5, aging, solid-liquid separation, obtaining a precipitate and a filtrate; calcining the precipitate, then adding a sodium source, a phosphorus source and a carbon source, mixing, sintering, and obtaining. The present invention recycles waste lithium iron phosphate batteries, prepares a sodium ion battery positive electrode material, and allows the resources in the battery to be reused, which is beneficial to environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery material recycling, and specifically relates to a preparation method of sodium ferrovanadium phosphate material and application thereof. Background Art

[0002] With the rise of electric vehicles, the demand for power batteries is increasing. Among them, lithium iron phosphate batteries are one of the important power batteries. However, with the use and consumption of electric vehicles, the amount of retired batteries will also increase, especially after 4-6 years, a large number of lithium iron phosphate batteries will be retired. If a large number of retired power lithium iron phosphate batteries cannot be properly recycled and utilized, it will not only waste resources, but also cause environmental pollution and other problems. Therefore, how to better deal with retired lithium iron phosphate batteries has become an urgent problem that the industry needs to solve.

[0003] Lithium resources on the earth are very limited. As lithium resources become increasingly scarce, sodium, which has abundant reserves, has come into people's view. Sodium and lithium are in the same main group and have similar chemical properties. The content of sodium in the earth's crust is much higher than that of lithium. Therefore, sodium-ion batteries are a very promising secondary battery. At present, common sodium-ion battery cathode materials mainly include layered transition metal oxides, Prussian blue analogs, polyanion compounds, tunnel-type oxides, etc.

[0004] Therefore, there is an urgent need to provide a method that can recycle waste lithium iron phosphate batteries and utilize abundant sodium resources to prepare batteries. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing a sodium ferrovanadium phosphate material, which can use waste lithium iron phosphate batteries to prepare the sodium ferrovanadium phosphate material, and use the sodium ferrovanadium phosphate material as a positive electrode material of a sodium ion battery to prepare a sodium ion battery with excellent performance.

[0006] A first aspect of the present invention provides a method for preparing a sodium ferrovanadium phosphate material.

[0007] Specifically, a method for preparing sodium ferrovanadium phosphate material comprises the following steps:

[0008] (1) crushing the lithium iron phosphate battery into battery powder, adding acid solution, reacting, and separating the solid and liquid to obtain a leaching solution and a leaching residue;

[0009] (2) removing impurities from the leaching solution of step (1), then adding an oxidant, adjusting the concentrations of iron and phosphorus, and adjusting the pH value to less than 1.5, to obtain solution A;

[0010] (3) adding the solution A obtained in step (2), the vanadium-containing solution and the alkali solution to the acid solution in parallel, controlling the pH value to be 1.8-2.2, then continuing to add the alkali solution to adjust the pH value to 2.0-2.5, aging, and solid-liquid separation to obtain a precipitate and a filtrate;

[0011] (4) calcining the precipitate obtained in step (3), then adding a sodium source, a phosphorus source and a carbon source to mix to obtain a mixture; and then sintering the mixture to obtain the sodium ferrovanadium phosphate material.

[0012] The present invention recovers waste lithium iron phosphate batteries, uses acid solution for leaching and oxidation, and obtains ferrophosphorus solution. The ferrophosphorus solution, vanadium-containing solution, and sodium hydroxide solution are then added to the acid solution in parallel to perform a coprecipitation reaction. By strictly controlling the pH during the coprecipitation reaction, the pH value of the reaction system is first set to 1.8-2.2, so that both ferrophosphate precipitation and ferrovanadate precipitation are generated; then alkali solution is further added to adjust the pH value to 2.0-2.5, so that the iron is completely precipitated. The step-by-step alkali coprecipitation method not only makes the precipitation of vanadium and iron more thorough without the need to add vanadium source during subsequent sintering, thereby avoiding uneven mixing of vanadium and iron; and the coprecipitation forms ferrophosphate / ferrovanadate eutectics, so that iron and vanadium can be mixed at the atomic level, making the element distribution more uniform. The ferrophosphate / ferrovanadate eutectics formed by this coprecipitation are transformed into a more stable mixed crystal form of olivine structure and orthorhombic structure after calcination, which is conducive to the embedding of sodium ions when sintered with a sodium source, and can improve the specific capacity of the prepared positive electrode material.

[0013] Preferably, in step (1), the acid solution is selected from at least one of sulfuric acid, hydrochloric acid or phosphoric acid.

[0014] Preferably, in step (1), the reaction temperature is 40-90°C, and the reaction time is 2-12 hours; further preferably, in step (1), the reaction temperature is 40-100°C, and the reaction time is 2-8 hours.

[0015] Preferably, in step (1), the ratio of the volume of the acid solution to the mass of the battery powder is (1-8) mL:1 g; further preferably, in step (1), the ratio of the volume of the acid solution to the mass of the battery powder is (2-5) mL:1 g.

[0016] Preferably, in step (2), the impurities are copper and aluminum.

[0017] Preferably, the method for removing copper and aluminum is: adding iron to the leaching solution of step (1), adjusting the pH to 4.0-4.7, and filtering out the residue.

[0018] Preferably, the ratio of the molar amount of the iron to the molar amount of the copper ions in the leachate is (1.0-3.0):1; further preferably, the ratio of the molar amount of the iron to the molar amount of the copper ions in the leachate is (1.0-1.5):1.

[0019] Preferably, in step (2), the oxidant is selected from at least one of hydrogen peroxide, oxygen, chlorine, sodium chlorate or hypochlorous acid. There is no particular requirement for the amount of the oxidant, as long as it can be fully oxidized to obtain trivalent iron ions.

[0020] Preferably, in step (2), the iron ion concentration in solution A is 0.5-5.0 mol / L, and the phosphorus concentration is 0.5-3.0 mol / L; further preferably, in step (2), the iron ion concentration in solution A is 1-3.0 mol / L, and the phosphorus concentration is 0.5-2.0 mol / L.

[0021] Preferably, in step (3), the vanadium-containing solution is a solution containing a metavanadate or a vanadate, such as ammonium metavanadate, sodium metavanadate, ammonium vanadate, sodium vanadate.

[0022] Preferably, the concentration of the vanadium-containing solution is 0.1-3.0 mol / L.

[0023] Preferably, in step (3), the flow ratio of solution A to the vanadium-containing solution is (0.5-3):1; further preferably, in step (3), the flow ratio of solution A to the vanadium-containing solution is (0.5-2):1.

[0024] Preferably, in step (3), the acid solution is selected from at least one of sulfuric acid, nitric acid or hydrochloric acid.

[0025] Preferably, in step (3), the alkali solution is at least one of sodium hydroxide solution, potassium hydroxide solution or ammonia water.

[0026] Preferably, the concentration of the sodium hydroxide solution is 0.1-2.0 mol / L.

[0027] Preferably, in step (3), the aging time is 1-5 h; further preferably, in step (3), the aging time is 1-3 h.

[0028] Preferably, in step (3), the filtrate is a lithium-containing solution, and sodium carbonate can be added to prepare lithium carbonate to achieve waste liquid recycling.

[0029] Preferably, in step (4), the calcination temperature is 400-800°C, and the calcination time is 1-10h; further preferably, in step (4), the calcination temperature is 500-600°C, and the calcination time is 3-6h.

[0030] Preferably, in step (4), the sodium source is selected from at least one of sodium carbonate, sodium acetate or sodium oxalate.

[0031] Preferably, in step (4), the phosphorus source is selected from at least one of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, sodium monohydrogen phosphate or sodium dihydrogen phosphate.

[0032] Preferably, in step (4), the carbon source is selected from at least one of glucose, citric acid, oxalic acid, lactose or galactose.

[0033] Preferably, in step (4), the molar ratio of the carbon source to the phosphorus element in the mixture is (1-3):1; further preferably, in step (4), the molar ratio of the carbon source to the phosphorus element in the mixture is (1-2):1.

[0034] Preferably, in step (4), the sintering process is carried out under an inert atmosphere at 500-750° C. for 3-12 hours; further preferably, the sintering process is carried out under an inert atmosphere at 550-650° C. for 6-10 hours.

[0035] The second aspect of the present invention provides the use of the preparation method of the sodium ferrovanadium phosphate material in the preparation of battery positive electrode materials.

[0036] Preferably, the battery is a sodium ion battery.

[0037] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0038] (1) The present invention recycles waste lithium iron phosphate batteries, uses acid solution to leach ferrophosphorus, and then, after impurities removal (copper and aluminum removal) and liquid preparation, performs a coprecipitation reaction with a vanadium-containing solution and an alkaline solution to form an iron phosphate / iron vanadate eutectic, so that iron and vanadium are mixed at the atomic level, and the element distribution is more uniform. There is no need to add a vanadium source during subsequent sintering, thereby avoiding uneven mixing of vanadium and iron. In addition, the iron phosphate / iron vanadate eutectic is transformed into a more stable mixed crystal form of olivine structure and orthorhombic structure while being calcined at high temperature to remove water, which is more conducive to the embedding of sodium ions during subsequent sintering with a sodium source, thereby improving the specific capacity of the prepared positive electrode material.

[0039] (2) The present invention not only recycles waste lithium iron phosphate batteries and prepares positive electrode materials for sodium ion batteries, thereby allowing the resources in the batteries to be reused, which is beneficial to environmental protection; in addition, during the reaction process, the waste liquid can be recycled and further purified to produce lithium salts, thereby alleviating the problem of lithium resource shortage. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the process flow chart of Example 1.

[0041] Figure 2 This is the SEM image of the sodium ferrovanadium phosphate material prepared in Example 2. DETAILED DESCRIPTION

[0042] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0043] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0044] Example 1

[0045] A method for preparing sodium ferrovanadium phosphate material, the process flow chart of which is as follows Figure 1 As shown, the following steps are included:

[0046] (1) crushing the discarded lithium iron phosphate battery and collecting the battery powder, adding the collected battery powder to a sulfuric acid solution with a mass concentration of 40% at a liquid-to-solid ratio of 2 mL:1 g, and soaking the solution, setting the reaction temperature to 40° C., and reacting for 8 hours; after the reaction is completed, filtering, and solid-liquid separation to obtain a leachate and a leach residue;

[0047] (2) adding iron powder to the leachate to react, adjusting the pH value to 4.5 after the reaction is complete, filtering out the filter residue, and obtaining a solution for removing copper and aluminum; then adding hydrogen peroxide, and adding trivalent iron salt, phosphate, and sulfuric acid to obtain solution A, wherein the iron ion concentration in solution A is 1.0 mol / L, the phosphorus concentration is 0.5 mol / L, and the pH value of solution A is 0.1;

[0048] (3) preparing a sodium hydroxide solution with a concentration of 0.1 mol / L and an ammonium metavanadate solution with a concentration of 0.5 mol / L; adding sulfuric acid with a pH of 2.0 as a bottom liquid to the reactor until it covers the bottom stirring paddle, starting stirring, and then adding solution A, ammonium metavanadate solution, and sodium hydroxide solution to the reactor in parallel, with the flow ratio of solution A to ammonium metavanadate solution being 1:1, and controlling the pH in the reactor to be 1.8-2.2 and the reaction temperature to be about 70° C.; after the addition is completed, continuing to add sodium hydroxide solution to the reactor to adjust the pH to 2.5, and aging for 2 h; then performing solid-liquid separation on the slurry in the reactor to obtain a precipitate and a filtrate;

[0049] (4) The precipitate was calcined at 550° C. for 5 h, and then glucose, sodium carbonate, ammonium monohydrogen phosphate and the calcined precipitate were added into deionized water according to the molar ratio of each element in the target product chemical formula of Na:P:Fe:V:glucose=7:7:4:2:7, and the mixture was fully mixed and stirred in a mixing tank. After spray drying, the mixture was sintered at 550° C. for 10 h in an inert atmosphere and crushed to obtain Na 7 Fe 4 V 2 (PO 4 ) 7 @C's sodium vanadium iron phosphate material.

[0050] Example 2

[0051] A method for preparing sodium ferrovanadium phosphate material comprises the following steps:

[0052] (1) crushing the discarded lithium iron phosphate battery and collecting the battery powder, adding the collected battery powder to a sulfuric acid solution with a mass concentration of 25% at a liquid-to-solid ratio of 3 mL:1 g, and soaking the solution. The reaction temperature was set to 50° C. and the reaction was performed for 6 hours. After the reaction was completed, filtering was performed to separate the solid and the liquid to obtain a leachate and a leach residue.

[0053] (2) adding iron powder to the leachate to react, adjusting the pH value to 4.5 after the reaction is complete, filtering out the filter residue, and obtaining a solution for removing copper and aluminum; then adding sodium chlorate, and adding trivalent iron salt, phosphate, and sulfuric acid to obtain solution A, wherein the iron ion concentration in solution A is 1.5 mol / L, the phosphorus concentration is 1.0 mol / L, and the pH value of solution A is 0;

[0054] (3) preparing a sodium hydroxide solution with a concentration of 1.0 mol / L and a sodium metavanadate solution with a concentration of 0.5 mol / L; adding sulfuric acid with a pH of 2.2 as a bottom liquid to the reactor until it covers the bottom stirring paddle, starting stirring, and then adding solution A, sodium metavanadate solution, and sodium hydroxide solution to the reactor in parallel, with the flow ratio of solution A to sodium metavanadate solution being 1:1, controlling the pH in the reactor to be 1.8-2.2 and the reaction temperature to be about 70° C.; after the addition is completed, continuing to add sodium hydroxide solution to the reactor to adjust the pH to 2.0, and aging for 2 h; then performing solid-liquid separation on the slurry in the reactor to obtain a precipitate and a filtrate;

[0055] (4) The precipitate was calcined at 600° C. for 5 h, and then glucose, sodium acetate, ammonium monohydrogen phosphate and the calcined precipitate were added into deionized water according to the molar ratio of each element in the target product chemical formula of Na:P:Fe:V:glucose=9:9:6:2:9, and the mixture was fully mixed and stirred in a mixing tank. After spray drying, the mixture was sintered at 580° C. for 9 h in an inert atmosphere and crushed to obtain Na 9 Fe 6 V 2 (PO 4 ) 9 @C's sodium vanadium iron phosphate material. Figure 2 This is the SEM image of sodium ferrovanadium phosphate material. Figure 2 It can be seen that the particles of the sodium vanadium iron phosphate material are uniform, without agglomeration or uneven coating.

[0056] Example 3

[0057] A method for preparing sodium ferrovanadium phosphate material comprises the following steps:

[0058] (1) crushing the discarded lithium iron phosphate battery and collecting the battery powder, adding the collected battery powder to a sulfuric acid solution with a mass concentration of 20% at a liquid-to-solid ratio of 5 mL:1 g, setting the reaction temperature to 90° C., and reacting for 2 hours; after the reaction is completed, filtering, and solid-liquid separation to obtain a leachate and a leach residue;

[0059] (2) adding iron powder to the leachate to react, adjusting the pH value to 4.7 after the reaction is complete, filtering out the filter residue, and obtaining a solution for removing copper and aluminum; then adding hypochlorous acid, and adding trivalent iron salt, phosphate, and sulfuric acid to obtain solution A, wherein the iron ion concentration in solution A is 2.0 mol / L, the phosphorus concentration is 0.5 mol / L, and the pH value of solution A is 0.1;

[0060] (3) preparing a sodium hydroxide solution with a concentration of 0.1 mol / L and an ammonium vanadate solution with a concentration of 1.5 mol / L; adding sulfuric acid with a pH of 1.8 as a bottom liquid to the reactor until it covers the bottom stirring paddle, starting stirring, and then adding solution A, ammonium vanadate solution, and sodium hydroxide solution to the reactor in parallel, with the flow ratio of solution A to ammonium vanadate solution being 1:1, and controlling the pH in the reactor to be 1.8-2.2 and the reaction temperature to be 75° C.; after the addition is completed, continuing to add sodium hydroxide solution to the reactor to adjust the pH to 2.4, and aging for 1.5 h; then performing solid-liquid separation on the slurry in the reactor to obtain a precipitate and a filtrate;

[0061] (4) The precipitate is calcined at 500° C. for 6 h, and then oxalic acid, sodium oxalate, sodium monohydrogen phosphate and the calcined precipitate are added to deionized water according to the molar ratio of each element in the target product chemical formula of Na:P:Fe:V:oxalic acid=17:17:8:6:17, and the mixture is fully mixed and stirred in a mixing tank. After spray drying, the mixture is sintered at 650° C. for 6 h in an inert atmosphere and crushed to obtain a product with the chemical formula of Na 17 Fe 8 V 6 (PO 4 ) 17 @C's sodium vanadium iron phosphate material.

[0062] Example 4

[0063] A method for preparing sodium ferrovanadium phosphate material comprises the following steps:

[0064] (1) crushing the discarded lithium iron phosphate battery and collecting the battery powder, adding the collected battery powder to a phosphoric acid solution with a mass concentration of 30% at a liquid-to-solid ratio of 3 mL:1 g, and soaking the collected battery powder. The reaction temperature was set to 90° C. and the reaction was performed for 2 hours. After the reaction was completed, filtering and solid-liquid separation were performed to obtain a leachate and a leach residue;

[0065] (2) adding iron powder to the leachate to react, adjusting the pH value to 4.7 after the reaction is complete, filtering out the filter residue, and obtaining a solution for removing copper and aluminum; then adding chlorine gas, and adding trivalent iron salt, phosphate, phosphoric acid, and sulfuric acid to obtain solution A, wherein the iron ion concentration in solution A is 1.2 mol / L, the phosphorus concentration is 1.0 mol / L, and the pH value of solution A is 0.1;

[0066] (3) preparing a sodium hydroxide solution with a concentration of 0.1 mol / L and a sodium vanadate solution with a concentration of 1.5 mol / L; adding hydrochloric acid with a pH of 1.8 as a bottom liquid to the reactor until it covers the bottom stirring paddle, starting stirring, and then adding solution A, sodium vanadate solution, and sodium hydroxide solution to the reactor in parallel, with the flow ratio of solution A to sodium vanadate solution being 1:2, controlling the pH in the reactor to be 1.8-2.2 and the reaction temperature to be 65° C.; after the addition is completed, continuing to add sodium hydroxide solution to the reactor to adjust the pH to 2.4, and aging for 1.5 h; then performing solid-liquid separation on the slurry in the reactor to obtain a precipitate and a filtrate;

[0067] (4) The precipitate was calcined at 550° C. for 5 h, and then glucose, sodium acetate, sodium dihydrogen phosphate and the calcined precipitate were added into deionized water according to the molar ratio of each element in the target product chemical formula of Na:P:Fe:V:glucose=15:15:12:2:15, and the mixture was fully mixed and stirred in a mixing tank. After spray drying, the mixture was sintered at 650° C. for 7 h in an inert atmosphere and crushed to obtain Na 15 Fe 12 V 2 (PO 4 ) 15 @C's sodium vanadium iron phosphate material.

[0068] Comparative Examples 1-4

[0069] Comparative Examples 1-4 all adopt the solid phase method to prepare sodium vanadium ferrophosphate materials, which correspond to Examples 1-4 respectively. According to the molar ratios of sodium, iron, vanadium, phosphorus and carbon source of the sodium vanadium ferrophosphate materials obtained in Examples 1-4, iron nitrate, vanadium pentoxide and the same sodium source, phosphorus source and carbon source are taken, mixed, and calcined under the same conditions to obtain sodium vanadium ferrophosphate materials with the same chemical formula.

[0070] Product effect testing

[0071] The sodium ferrovanadium phosphate materials prepared in Examples 1-4 and Comparative Examples 1-4 were used as positive electrode materials for sodium ion batteries and assembled into batteries. The specific process is as follows: N-methylpyrrolidone was used as a solvent, and the positive electrode active material was mixed evenly with acetylene black and PVDF in a mass ratio of 8:1:1, and coated on aluminum foil, and dried at 60-80°C for 8 hours, and then vacuum dried at 100-120°C for 12 hours. The battery was assembled in an argon-protected glove box, and a metal sodium sheet was used as the negative electrode of the counter electrode, and 1 mol / L NaPF6 was used as the electrolyte to assemble a CR2032 button battery.

[0072] Then, the rate performance of each CR2032 button cell was tested at 25°C, 2.0-4.5V voltage range, and 1C rate.-1 ) to set the magnification, and the results are shown in Table 1.

[0073] Table 1

[0074] <![CDATA[1C discharge capacity mAh g -1 > 100 cycles capacity retention Example 1 120 96.6% Comparative Example 1 102 82.3% Example 2 126 95.3% Comparative Example 2 105 81.1% Example 3 122 95.8% Comparative Example 3 104 80.3% Example 4 126 96.1% Comparative Example 4 106 83.3%

[0075] As shown in Table 1, the sodium ferrovanadium phosphate material prepared in the embodiment is used as the positive electrode material of the sodium ion battery, and the first charge and discharge capacity of the prepared battery is greater than or equal to 120 mAh g -1 After 100 cycles, the capacity retention rate of the battery is greater than 95%, which is significantly better than the battery prepared in the comparative example.

Claims

1. A method for preparing sodium ferrovanadium phosphate material, characterized in that: The following steps are involved: (1) crushing the lithium iron phosphate battery into battery powder, adding acid solution, reacting, and separating the solid and liquid to obtain a leaching solution and a leaching residue; (2) removing impurities from the leaching solution of step (1), then adding an oxidant, adjusting the concentrations of iron and phosphorus, and adjusting the pH value to less than 1.5, to obtain solution A; (3) adding the solution A obtained in step (2), the vanadium-containing solution and the alkali solution to the acid solution in parallel, controlling the pH value to be 1.8-2.2, then continuing to add the alkali solution to adjust the pH value to 2.0-2.5, aging, and solid-liquid separation to obtain a precipitate and a filtrate; (4) calcining the precipitate obtained in step (3), then adding a sodium source, a phosphorus source and a carbon source to mix to obtain a mixture; and then sintering the mixture to obtain the sodium ferrovanadium phosphate material.

2. The preparation method according to claim 1, characterized in that: In step (2), the impurities are copper and aluminum; the method for removing copper and aluminum is: adding iron to the leaching solution of step (1), adjusting the pH to 4.0-4.7, and filtering out the residue.

3. The preparation method according to claim 2, characterized in that: The ratio of the molar amount of the iron to the molar amount of the copper ions in the leaching solution is (1.0-3.0):

1.

4. The preparation method according to claim 1, characterized in that: In step (2), the oxidant is selected from at least one of hydrogen peroxide, oxygen, chlorine, sodium chlorate or hypochlorous acid.

5. The preparation method according to claim 1, characterized in that: In step (2), the concentration of iron ions in the solution A is 0.5-5.0 mol / L, and the concentration of phosphorus is 0.5-3.0 mol / L.

6. The preparation method according to claim 1, characterized in that: In step (3), the alkaline solution is at least one of sodium hydroxide solution, potassium hydroxide solution or ammonia water.

7. The preparation method according to claim 1, characterized in that: In step (3), the acid solution is selected from at least one of sulfuric acid, nitric acid or hydrochloric acid.

8. The preparation method according to claim 1, characterized in that: In step (4), the calcination temperature is 400-800° C., and the calcination time is 1-10 h.

9. The preparation method according to claim 1, characterized in that: In step (4), the molar ratio of the carbon source to the phosphorus element in the mixture is (1-3):

1.

10. The preparation method according to claim 1, characterized in that: In step (4), the sodium source is selected from at least one of sodium carbonate, sodium acetate or sodium oxalate; the phosphorus source is selected from at least one of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, sodium monohydrogen phosphate or sodium dihydrogen phosphate; and the carbon source is selected from at least one of glucose, citric acid, oxalic acid, lactose or galactose.

11. The preparation method according to claim 10, characterized in that: In step (4), the sintering process is carried out under an inert atmosphere at 500-750° C. for 3-12 hours.

Citation Information

Patent Citations

  • Method for preparing lithium iron vanadium phosphate from waste lithium iron phosphate positive plates

    CN107579304A

  • Selective recovery process of mixed waste of lithium nickel cobalt manganese oxide and lithium iron phosphate

    CN110371943A

  • Method for recycling positive electrode material of waste lithium iron phosphate battery

    CN113735087A

  • Method for regenerating lithium composite oxide, lithium composite oxide, electrochemical device and lithium ion secondary battery

    WO2016067497A1