A lithium ion battery positive electrode material and its preparation method and application

By forming a gradient distribution coating layer of amorphous phase Li3PO4 and sulfur-rich phase phosphorus and sulfur molecules P4S10+x on the surface of the lithium-ion battery cathode material with a thickness of nanometers, the problem of poor interface stability between the cathode material and the solid electrolyte is solved, and the problem of poor interface stability between the cathode material and the solid electrolyte is improved. Improves the capacity and cycle performance of lithium-ion batteries, achieving higher lithium-ion conductivity and battery stability.

CN114628679BActive Publication Date: 2024-10-11SILVERLEAF ELEMENTS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210159894.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-22
Publication Date
2024-10-11
Estimated Expiration
2042-02-22

AI Technical Summary

Technical Problem

The interface stability between the cathode material and the solid electrolyte of existing lithium-ion batteries is poor, resulting in low capacity and poor cycle stability. Moreover, the lithium ion conductivity of commonly used metal oxide coating materials is low, which limits the use of lithium-ion batteries. performance.

Method used

The composition gradient distribution coating layer formed by the interdiffusion reaction of amorphous phase Li3PO4 with nanometer-thickness and sulfur-rich phase phosphorus and sulfur molecules P4S10+x is used as the coating layer of the cathode active material, which improves the structural stability and stability of the material. Lithium ion conductivity.

Benefits of technology

It significantly improves the capacity and cycle performance of the cathode active material, reduces the surface resistance of the material, and enhances the commercial application value of all-solid-state lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 213629DEST_PATH_IMAGE002
    Figure 213629DEST_PATH_IMAGE002
  • Figure 220222105356
    Figure 220222105356
  • Figure 220222105400
    Figure 220222105400
Patent Text Reader

Abstract

The present invention discloses a composite positive electrode material for lithium-ion batteries and a preparation method and application thereof. The positive electrode comprises a composite material comprising a positive electrode active material and a coating layer with a component gradient distribution of nanometer-level thickness on the surface of the positive electrode active material, wherein the coating layer with a component gradient distribution is a composite material of an amorphous phase Li3PO4 with a nanometer-level thickness and a sulfur-rich phase phosphorus-sulfur molecule P4S 10+x Obtained by mutual diffusion reaction. The S and O element contents in the coating layer are distributed in a gradient from the end close to the positive electrode active material to the outside. The composite positive electrode material of the present invention greatly improves the structural stability of the positive electrode active material, reduces the surface impedance of the material, and thus improves the capacity, initial efficiency and cycle performance of the positive electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a lithium (ion) battery positive electrode material, a design and preparation method thereof and an application thereof. Background Art

[0002] Lithium-ion batteries have been rapidly developed in the fields of electronic equipment and power supply due to their high energy density, high operating voltage and long cycle life. Among them, electric vehicles and hybrid vehicles with lithium-ion batteries as core components have been included in the country's strategic planning. However, most of the lithium-ion batteries currently on the market use flammable and leaky organic electrolytes, which lead to serious safety hazards.

[0003] In contrast, replacing the organic electrolyte with a solid electrolyte layer can effectively solve the safety problem of lithium-ion batteries. At the same time, the use of high-energy-density electrode sheets such as metallic lithium can improve the energy density of the system.

[0004] At present, the solid-state lithium-ion battery system that has been developed generally uses layered transition metal oxides LiMO2 (M=Ni, Co, Mn, Al), LiFePO4, and lithium-rich lithium manganese oxide as cathode materials. Currently, there are problems such as low capacity and poor cycle stability. This is mainly due to the poor interface stability between the cathode material and the solid electrolyte. On the one hand, the voltage window of solid electrolyte materials such as sulfides is relatively narrow, the potential between the cathode material and the electrolyte is not matched, and the interface reaction produces a large number of electronic / ion insulating products, which leads to an increase in interface impedance and slow ion conduction at the interface. On the other hand, the interface instability between the electrode / electrolyte will cause uneven stress in the cathode material during the charge and discharge process, resulting in particle cracking and structural decay, affecting the battery capacity. During the cycle, the cathode and the electrolyte continue to react, the interface impedance continues to increase, and the battery capacity decreases rapidly. In order to solve this problem, researchers often modify the interface by coating a layer of metal oxide with Li ion conductivity on the surface of the cathode particles. Commonly used coating materials include LiNbO3, LiTaO3, LiAlO2, Li2O-ZrO2, Li2O-SiO2, Li2CO3, etc. However, the room temperature lithium ion conductivity of this type of metal oxide is generally low, not exceeding 10 -6 This severely restricts the conduction of lithium ions in the interface layer, thereby limiting its performance.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a composite positive electrode material for lithium (ion) batteries, a preparation method and application thereof. The positive electrode comprises a composite material comprising a positive electrode active material and a coating layer with a component gradient distribution of nanometer-level thickness on the surface of the positive electrode active material, wherein the coating layer with a component gradient distribution is a composite material of an amorphous phase Li3PO4 with a nanometer-level thickness and a sulfur-rich phase phosphorus-sulfur molecule P4S 10+x Obtained by mutual diffusion reaction. The composite positive electrode material of the present invention greatly improves the structural stability of the positive electrode active material, reduces the surface impedance of the material, thereby improving the capacity, first efficiency and long cycle performance of the positive electrode active material. In addition, the present invention can also solve the problems of chemical and electrochemical instability between the solid electrolyte and the positive electrode active material in the all-solid-state secondary battery, thereby realizing the commercial application value of lithium (ion) batteries including all-solid-state secondary batteries.

[0007] To achieve the above purpose, the present invention discloses the following technical contents:

[0008] A lithium-ion battery composite positive electrode material, comprising: a composite material, a positive electrode active material, and

[0009] a coating layer located on the surface of the positive electrode active material,

[0010] The coating layer is a coating layer with a component gradient distribution with a nanometer-level thickness, and the coating layer is a mixture of one or more of an amorphous phase, a crystalline phase, and a glass ceramic phase. The coating layer has a thickness between 5 nanometers and 200 nanometers;

[0011] The coating layer with gradient distribution of components is composed of nanometer-level amorphous phase Li3PO4 and sulfur-rich phase phosphorus-sulfur molecules P4S 10+x Obtained through interdiffusion reaction, expressed as formula 1:

[0012] Formula 1

[0013] aLi3PO4∙bP4S 10+x

[0014] In formula 1

[0015] 30≥ x ≥2; a≤5 wt.%; b<5 wt.%,

[0016] Preferably x =6, 10, 20; a≤5 wt.%, a≤2 wt.%; b≤2.5 wt.%.

[0017] Where a is the mass percentage of Li3PO4 in the entire positive electrode active material, preferably 2 wt.%, and b is P4S 10+xThe mass percentage of the entire positive electrode active material is preferably 1 wt.%.

[0018] The coating layer with gradient component distribution is obtained by multi-step epitaxial growth on the surface of the positive electrode active material;

[0019] The component gradient distribution refers to that the coating layer has a high O content at the end close to the positive electrode active material and a high S content at the end away from the positive electrode active material; the S and O element contents in the coating layer are gradiently distributed from the end close to the positive electrode active material to the outside.

[0020] The positive electrode active material of the present invention includes lithium nickel manganese oxide, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxide, lithiated layered sulfide, or a combination thereof; the surface of the lithium-ion battery composite positive electrode material includes the surface of primary particles and secondary particles.

[0021] The amorphous phase Li3PO4 and the sulfur-rich phase phosphorus-sulfur molecule P4S of the present invention 10+x By interdiffusion reaction, it means that: the amorphous phase Li3PO4 with a thickness of nanometers is directly epitaxially deposited and grown on the surface of the positive electrode active material by atomic layer deposition technology, and the thickness is between 2 nanometers and 50 nanometers, preferably, 5 nanometers to 20 nanometers; the sulfur-rich phase phosphorus sulfur molecules P4S 10+x It is prepared by eutectic reaction of elemental P and elemental S according to the stoichiometric ratio; in order to realize the sulfur-rich phase phosphorus-sulfur molecule P4S 10+x The eutectic reaction can also be replaced by ball milling-sintering and reaction in an organic solution. The process of the interdiffusion reaction is as follows: ester, ether or ketone organic solvent is used to dissolve the sulfur-rich phase phosphorus sulfur molecules P4S 10+x , to obtain a certain concentration of P4S 10+x In the solution phase, the positive electrode material with amorphous phase Li3PO4 epitaxially grown on the surface with a nanometer thickness obtained by atomic layer deposition is immersed in the P4S 10+x The reaction is carried out in a solution, and the mass ratio between the two, the reaction time, the reaction temperature and other conditions are optimized. Then, the amorphous phase Li3PO4 with a sulfur-rich phase P4S with a nanometer thickness can be achieved by heating, drying and vacuum annealing. 10+x The interdiffusion reaction is carried out in a glove box with an inert atmosphere, or in a dry room with a dew point below -40 degrees Celsius, or in a reactor protected by a vacuum or inert atmosphere.

[0022] The lithium-ion battery composite positive electrode material of the present invention comprises a positive electrode active material surface multi-step epitaxial growth, and the process is as follows: 1) performing multi-step atomic layer deposition on the surface of the positive electrode active material to obtain an amorphous phase Li3PO4 with different thicknesses; 2) subsequently sulfurizing the amorphous phase Li3PO4 by a liquid phase immersion reaction method, and reacting the amorphous phase Li3PO4 with the sulfur-rich phase phosphorus-sulfur molecules P4S 10+x The chemical reaction between the two and the mutual diffusion of P, S, O and Li realize the preparation of the coating layer with component gradient distribution. The component gradient distribution refers to the detection of element composition and content at different depths of the coating layer by X-ray fluorescence spectroscopy (XPS), electron energy spectrum (EDS), time-of-flight-secondary ion mass spectrometry (Tof-SIMS), and X-ray absorption spectroscopy (XAS) testing methods, which can obtain the characteristics of element composition with content gradient distribution at different detection depths.

[0023] In the lithium-ion battery composite positive electrode material of the present invention, the amorphous phase Li3PO4 therein, in order to adapt to the chemical properties of different positive electrode active materials, the P element in the amorphous phase Li3PO4 can be completely or partially replaced by a C metal element, and the C metal element is one or more of Ta, Ge, Ti, Zr, Al, Hf, Nb, V, Zn, Sn, Mo, Ru, Co, Mn, and Fe. The substitution refers to the partial or complete replacement of the P element by adding a precursor containing the C metal element during the atomic layer deposition process.

[0024] The lithium-ion battery composite positive electrode material of the present invention further includes ion conductive additives and conductive additives; the ion conductive additives include sulfide electrolytes, oxide electrolytes, halide electrolytes, or combinations thereof; the conductive agent includes carbon nanofibers, graphite, carbon black, graphene, carbon nanotubes, conductive polymers mainly formed by polymerization of 3,4-ethylenedioxythiophene monomers, or combinations thereof.

[0025] The present invention further discloses a lithium (ion) battery, comprising:

[0026] The positive electrode according to any one of claims 1 to 6;

[0027] a negative electrode; and

[0028] An electrolyte, which is inserted between the positive electrode and the negative electrode and includes a sulfide solid electrolyte, an oxide solid electrolyte, a halide electrolyte, a nitride electrolyte, a polymer electrolyte, an organic electrolyte or a combination thereof. The lithium (ion) battery includes an all-solid battery, a semi-solid battery and a liquid battery;

[0029] The present invention further discloses the application of composite positive electrode materials for lithium-ion batteries in improving the capacity, first effect and long cycle performance of positive electrode active materials. In particular, the application in improving the commercial application value of lithium-ion batteries including all-solid-state secondary batteries; the commercial application value refers to improving the structural stability of positive electrode active materials and reducing the surface impedance of materials. Experimental results show that the positive electrode provided by the present invention, especially the coating layer with a component gradient distribution with a nanometer-level thickness, has obvious effects in at least 1) stabilizing the surface and grain boundaries of the positive electrode active material and reducing structural decay; 2) improving the activity of the positive electrode active material; 3) improving the long cycle stability of the all-solid-state battery; 4) improving the battery rate performance, etc.

[0030] The present invention is described in more detail as follows:

[0031] A lithium-ion battery positive electrode material, comprising:

[0032] A composite material comprising:

[0033] positive electrode active material, and

[0034] a coating layer located on the surface of the positive electrode active material,

[0035] The coating layer is a coating layer with a component gradient distribution having a nanometer-level thickness,

[0036] The coating layer with gradient distribution of components is composed of nanometer-level amorphous phase Li3PO4 and sulfur-rich phase phosphorus-sulfur molecules P4S 10+x Obtained through interdiffusion reaction, expressed as formula 1:

[0037] Formula 1

[0038] aLi3PO4∙bP4S 10+x

[0039] In formula 1

[0040] 30≥ x ≥2; a≤5 wt.%; b<5 wt.%,

[0041] Where a is the mass percentage of Li3PO4 in the entire positive electrode active material, preferably 2 wt.%, and b is P4S 10+x The mass percentage of the whole positive electrode active material is preferably 1 wt.%. The coating layer with gradient component distribution is obtained by multi-step epitaxial growth on the surface of the positive electrode active material.

[0042] The component gradient distribution means that the coating layer has a high O content at the end close to the positive electrode active material and a high S content at the end away from the positive electrode active material. The S and O element contents in the coating layer are distributed in a gradient from the end close to the positive electrode active material to the outside.

[0043] The positive electrode active material includes lithium nickel manganese oxide, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxide, lithiated layered sulfide, or a combination thereof. The surface of the positive electrode active material includes the surface of primary particles and secondary particles.

[0044] The coating layer with a component gradient distribution of nanometer-level thickness, wherein the coating layer is a mixture of one or more of an amorphous phase, a crystalline phase and a glass ceramic phase, and the coating layer has a thickness between 5 nanometers and 200 nanometers, preferably between 15 nanometers and 100 nanometers.

[0045] The nanometer-thick amorphous phase Li3PO4 and the sulfur-rich phase phosphorus-sulfur molecules P4S 10+x Through the interdiffusion reaction, the amorphous phase Li3PO4 with a nanometer thickness is directly epitaxially deposited and grown on the surface of the positive electrode active material using atomic layer deposition technology, and the thickness is between 2 nanometers and 50 nanometers, preferably, 5 nanometers to 20 nanometers.

[0046] The nanometer-thick amorphous phase Li3PO4 and the sulfur-rich phase phosphorus-sulfur molecules P4S 10+x Through interdiffusion reaction, the sulfur-rich phase phosphorus sulfur molecules P4S 10+x It is prepared by eutectic reaction of elemental P and elemental S in a stoichiometric ratio. 10+x For quantitative preparation, the eutectic reaction can also be replaced by ball milling-sintering and reaction in an organic solution.

[0047] Nano-thick amorphous phase Li3PO4 and sulfur-rich phase phosphorus-sulfur molecules P4S 10+x By interdiffusion reaction, wherein the interdiffusion reaction process is as follows: using ester, ether or ketone organic solvent to dissolve sulfur-rich phase phosphorus sulfur molecules P4S 10+x , to obtain a certain concentration of P4S 10+x In the solution phase, the positive electrode material with amorphous phase Li3PO4 epitaxially grown on the surface with a nanometer thickness obtained by atomic layer deposition is immersed in the P4S 10+x The reaction is carried out in a solution, and the mass ratio between the two, the reaction time, the reaction temperature and other conditions are optimized. Then, the amorphous phase Li3PO4 with a sulfur-rich phase P4S with a nanometer thickness can be achieved by heating, drying and vacuum annealing. 10+xThe interdiffusion reaction is carried out in a glove box with an inert atmosphere, or in a dry room with a dew point below -40 degrees Celsius, or in a reactor protected by a vacuum or inert atmosphere.

[0048] The aLi3PO4∙bP4S 10+x , of which 30 ≥ x ≥2, preferably x =6, 10; a≤5 wt.%, preferably a≤2wt.%; b<5 wt.%, preferably b≤2.5 wt.%.

[0049] The present invention further discloses multi-step epitaxial growth on the surface of the positive electrode active material, wherein the multi-step epitaxial growth refers to the following process:

[0050] 1) Multi-step atomic layer deposition is performed on the surface of the positive electrode active material to obtain amorphous phase Li3PO4 of different thicknesses;

[0051] 2) Then the amorphous phase Li3PO4 is sulfurized by liquid phase immersion reaction, and the amorphous phase Li3PO4 and the sulfur-rich phase phosphorus sulfur molecules P4S 10+x The chemical reaction between the two and the mutual diffusion of P, S, O and Li realize the preparation of the coating layer with component gradient distribution. The component gradient distribution refers to the detection of element composition and content at different depths of the coating layer by X-ray fluorescence spectroscopy (XPS), electron energy spectrum (EDS), time-of-flight-secondary ion mass spectrometry (Tof-SIMS), and X-ray absorption spectroscopy (XAS) testing methods, which can obtain the characteristics of element composition with content gradient distribution at different detection depths.

[0052] In order to adapt to the chemical characteristics of different positive active materials, the P element in the amorphous phase Li3PO4 can be completely or partially replaced by a C metal element, wherein the C metal element is one or more of Ta, Ge, Ti, Zr, Al, Hf, Nb, V, Zn, Sn, Mo, Ru, Co, Mn, and Fe, and the replacement refers to the partial or complete replacement of the P element by adding a precursor containing a C metal element during the atomic layer deposition process. The surface multi-step epitaxial growth process can also be achieved by chemical vapor deposition, sol-gel, molten salt-assisted thermal deposition, ion replacement reaction in solution, and other reaction processes for mass production.

[0053] The lithium-ion battery cathode material of the present invention further comprises an ion-conducting additive, wherein the ion-conducting additive comprises a sulfide electrolyte, an oxide electrolyte, a halide electrolyte, a nitride electrolyte, a polymer electrolyte, an organic electrolyte or a combination thereof. The sulfide electrolyte comprises a compound represented by the following formula 2:

[0054] Formula 2

[0055] Li α M β PS γ X δ Oε

[0056] In Formula 2,

[0057] 0<α≤7, 0≤β≤6, 0<γ<6, 0≤δ≤6, and 0≤ε≤2;

[0058] M is one or more of Ge, Sn, B, Zn, Sb or Si; and

[0059] X is one or more of F, Cl, Br, or I.

[0060] It further includes a conductive additive, which includes carbon nanofibers, graphite, carbon black, graphene, carbon nanotubes, a conductive polymer mainly formed by polymerization of 3,4-ethylenedioxythiophene monomers, or a combination thereof.

[0061] The present invention further discloses a lithium (ion) battery, comprising:

[0062] The positive electrode described above;

[0063] a negative electrode; and

[0064] An electrolyte is interposed between the positive electrode and the negative electrode and includes a sulfide solid electrolyte, an oxide solid electrolyte, a halide electrolyte, a nitride electrolyte, a polymer electrolyte, an organic electrolyte, or a combination thereof.

[0065] The lithium (ion) battery, wherein the negative electrode comprises lithium metal or a lithium metal alloy; or

[0066] The negative electrode comprises a negative electrode active material, wherein the negative electrode active material comprises carbon, silicon, silicon oxide, silicon alloy, silicon-carbon composite, tin, tin alloy, tin-carbon composite, metal capable of alloying with lithium, its alloy, its oxide, its sulfide or its halide, LiVO2, Li4Ti5O 12 , a metal oxide capable of deintercalating lithium, a metal halide capable of deintercalating lithium, a metal sulfide capable of deintercalating lithium, or a combination thereof.

[0067] The lithium (ion) battery, wherein the sulfide electrolyte comprises a compound represented by the following formula 2, or a combination thereof:

[0068] Formula 2

[0069] Li α M β PS γ Xδ Oε

[0070] In Formula 2,

[0071] 0<α≤7, 0≤β≤6, 0<γ<6, 0≤δ≤6, and 0≤ε≤2;

[0072] M is one or more of Ge, Sn, B, Zn, Sb or Si; and

[0073] X is one or more of F, Cl, Br, or I.

[0074] The lithium (ion) battery, wherein the halide electrolyte includes Li3InCl6, Li3YCl6, Li3LnCl6 (Ln is a rare earth element), LiAlCl4, Li2ZrCl6, a compound represented by the following formula 3, or a combination thereof:

[0075] Formula 3

[0076] Li ζ M η X θ Oι

[0077] In formula 3,

[0078] 0<ζ≤4, 0≤η≤2, 0<θ≤7, and 0≤ι≤5;

[0079] M is one or more of Y, Sc, Ti, Zr, Hf, Nb, Ta, Al, Ga, B, In, Fe, V, Mn, Co, Ni, Ln (Ln is a rare earth element), or Si; and

[0080] X is one or more of F, Cl, Br, or I.

[0081] The lithium (ion) battery described in the present invention includes a fully solid battery, a semi-solid battery and a liquid battery.

[0082] Specifically, the positive electrode composite material includes a positive electrode active material and a coating layer with a component gradient distribution of nanometer-level thickness located on the surface of the positive electrode active material. The coating layer with a component gradient distribution is a nanometer-level thickness amorphous phase Li3PO4 and a sulfur-rich phase phosphorus sulfur molecule P4S 10+x Obtained through interdiffusion reaction, expressed as formula 1:

[0083] aLi3PO4∙bP4S 10+x (Formula 1)

[0084] Among them, 30 ≥ x ≥2; a≤5 wt.%; b<5 wt.%,

[0085] a is the mass percentage of Li3PO4 in the entire positive electrode active material, preferably 2 wt.%, b is P4S 10+x The mass percentage of the entire positive electrode active material is preferably 1 wt.%.

[0086] In the present invention, the coating layer with component gradient distribution is obtained by multi-step epitaxial growth on the surface of the positive electrode active material. The component gradient distribution means that the coating layer has a high O content at the end close to the positive electrode active material and a high S content at the end away from the positive electrode active material. The S and O element contents in the coating layer are distributed in a gradient from the end close to the positive electrode active material to the outside.

[0087] In the present invention, the positive electrode active material includes lithium nickel manganese oxide, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxide, lithiated layered sulfide, or a combination thereof.

[0088] The surface of the positive electrode active material includes the surfaces of primary particles and secondary particles.

[0089] In the present invention, the coating layer with a component gradient distribution of nanometer-level thickness is a mixture of one or more of an amorphous phase, a crystalline phase and a glass ceramic phase. The coating layer thickness is between 5 nanometers and 200 nanometers.

[0090] Preferably, the coating layer has a thickness between 15 nanometers and 100 nanometers.

[0091] In the present invention, the coating layer with a component gradient distribution of nanometer-level thickness is formed by amorphous phase Li3PO4 with a sulfur-rich phase phosphorus-sulfur molecule P4S 10+x The amorphous phase Li3PO4 with a thickness of nanometers is directly grown by epitaxial deposition on the surface of the positive electrode active material using atomic layer deposition technology, with a thickness ranging from 2 nanometers to 50 nanometers.

[0092] Preferably, the nanoscale amorphous phase Li3PO4 has a thickness of 5 nanometers to 20 nanometers.

[0093] In the present invention, the sulfur-rich phase phosphorus-sulfur molecule P4S 10+x It is prepared by eutectic reaction of elemental P and elemental S in a stoichiometric ratio. In order to achieve sulfur-rich phase phosphorus-sulfur molecule P4S 10+x For quantitative preparation, the eutectic reaction can also be replaced by ball milling-sintering and reaction in an organic solution.

[0094] Specifically, the amorphous phase Li3PO4 and the sulfur-rich phase phosphorus-sulfur molecules P4S 10+xThe reaction process of the mutual diffusion reaction between the two is realized by the following method: using ester, ether or ketone organic solvent to dissolve the sulfur-rich phase phosphorus sulfur molecules P4S 10+x , to obtain a certain concentration of P4S 10+x In the solution phase, the positive electrode material with amorphous phase Li3PO4 epitaxially grown on the surface with a nanometer thickness obtained by atomic layer deposition is immersed in the P4S 10+x The reaction is carried out in the solution phase, and the mass ratio between the two, the reaction time, the reaction temperature and other conditions are optimized. Then, the amorphous phase Li3PO4 with a sulfur-rich phase P4S with a nanometer thickness can be achieved by heating, drying and vacuum annealing. 10+x The interdiffusion reaction is carried out in a glove box with an inert atmosphere, or in a dry room with a dew point below -40 degrees Celsius, or in a reactor protected by a vacuum or inert atmosphere.

[0095] In the present invention, the coating layer with a component gradient distribution aLi3PO4∙bP4S 10+x , after optimization, we can get x =6, 10, 20; a≤5 wt.%, preferably a≤2 wt.%; b<5 wt.%, preferably b≤2.5 wt.%.

[0096] In the present invention, the coating layer with component gradient distribution is obtained by a multi-step epitaxial growth method, and the multi-step epitaxial growth method refers to the following process: 1) performing multi-step atomic layer deposition on the surface of the positive electrode active material to obtain an amorphous phase Li3PO4 of different thicknesses; 2) subsequently sulfurizing the amorphous phase Li3PO4 by a liquid phase immersion reaction method, and reacting the amorphous phase Li3PO4 with the sulfur-rich phase phosphorus-sulfur molecules P4S 10+x The mutual diffusion of P, S, O and Li between the two enables the preparation of a coating layer with a component gradient distribution.

[0097] Among them, the component gradient distribution refers to the detection of elemental composition and content at different depths of the coating layer by means of X-ray fluorescence spectroscopy (XPS), electron energy spectrum (EDS), time-of-flight-secondary ion mass spectrometry (ToF-SIMS), and X-ray absorption spectroscopy (XAS) testing methods, which can obtain the characteristics of elemental components having a content gradient distribution with different detection depths.

[0098] In the present invention, in order to adapt to the chemical properties of different positive electrode active materials, the P element in the amorphous phase Li3PO4 can be completely or partially replaced by a C metal element, and the C metal element is one or more of Ta, Ge, Ti, Zr, Al, Hf, Nb, V, Zn, Sn, Mo, Ru, Co, Mn, and Fe. The substitution refers to the partial or complete substitution of the P element by adding a precursor containing the C metal element during the atomic layer deposition process.

[0099] Regarding the chemical composition of the coating layer, oxides are easy to achieve surface thin layer deposition through atomic layer deposition technology, but their ion conductivity is poor; sulfides have good ion conductivity, but cannot be deposited in a thin layer on the surface of positive electrode active particles by means of atomic layer deposition, chemical vapor deposition, etc. In addition, the chemical compatibility of sulfide electrolyte materials and positive electrode active materials is poor, and a large number of side reactions are generated during the deposition process. The coating layer with a component gradient distribution with a nanometer-level thickness achieved on the surface of the positive electrode active particles of the present invention can obtain a high ion conduction rate and can also alleviate the chemical reaction between the oxide positive electrode active material and the sulfide, thereby realizing the preparation of a stable surface coating layer. The invention can also be further used to modify the oxide surface film obtained by technical means such as atomic layer deposition and chemical vapor deposition, thereby increasing the application scope of these technologies and obtaining more surface coating layers with better performance.

[0100] Furthermore, for mass production, the atomic layer deposition process can also be achieved by chemical vapor deposition, sol-gel, molten salt assisted thermal deposition, ion replacement reaction in solution and other reaction processes.

[0101] In the present invention, the positive electrode further comprises an ion-conducting additive, and the ion-conducting additive comprises a sulfide electrolyte, an oxide electrolyte, a halide electrolyte, or a combination thereof.

[0102] The sulfide electrolyte as the ion-conductive additive comprises a compound represented by the following Formula 2:

[0103] Li α M β PS γ X δ Oε (Equation 2)

[0104] In Formula 2,

[0105] 0<α≤7, 0≤β≤6, 0<γ<6, 0≤δ≤6, and 0≤ε≤2;

[0106] M is one or more of Ge, Sn, B, Zn, Sb or Si; and

[0107] X is one or more of F, Cl, Br, or I.

[0108] In the present invention, the positive electrode further comprises a conductive additive, and the conductive additive comprises carbon nanofibers, graphite, carbon black, graphene, carbon nanotubes, a conductive polymer mainly formed by polymerization of 3,4-ethylenedioxythiophene monomers, or a combination thereof.

[0109] In some specific embodiments of the present invention, the cathode composite material is applied to a lithium (ion) battery, comprising the cathode of the present invention; a cathode; and a solid electrolyte material inserted between the cathode and the cathode.

[0110] The negative electrode includes lithium metal or lithium metal alloy; or includes carbon, silicon, silicon oxide, silicon alloy, silicon-carbon composite, tin, tin alloy, tin-carbon composite, metal alloyed with lithium, alloy thereof, oxide thereof, sulfide thereof or halide thereof, LiVO2, Li4Ti5O 12 , a metal oxide capable of deintercalating lithium, a metal halide capable of deintercalating lithium, a metal sulfide capable of deintercalating lithium, or a combination thereof.

[0111] In the lithium (ion) battery of the present invention, the solid electrolyte material includes a sulfide solid electrolyte, an oxide solid electrolyte, a halide electrolyte, a nitride electrolyte or a combination thereof.

[0112] The sulfide electrolyte includes a compound represented by the following formula 2, or a combination thereof:

[0113] Li α M β PS γ X δ Oε (Equation 2)

[0114] Among them, 0<α≤7, 0≤β≤6, 0<γ<6, 0≤δ≤6, and 0≤ε≤2;

[0115] M is one or more of Ge, Sn, B, Zn, Sb or Si; and

[0116] X is one or more of F, Cl, Br, or I.

[0117] Wherein, the halide electrolyte includes Li3InCl6, Li3YCl6, Li3LnCl6 (Ln is a rare earth element), LiAlCl4, Li2ZrCl6, a compound represented by the following formula 3, or a combination thereof:

[0118] Li ζ M η X θ Oι (Formula 3)

[0119] in,

[0120] 0<ζ≤4, 0≤η≤2, 0<θ≤7, and 0≤ι≤5;

[0121] M is one or more of Y, Sc, Ti, Zr, Hf, Nb, Ta, Al, Ga, B, In, Fe, V, Mn, Co, Ni, Ln (Ln is a rare earth element), or Si; and

[0122] X is one or more of F, Cl, Br, or I.

[0123] Furthermore, in the present invention, the lithium (ion) battery includes an all-solid battery, a semi-solid battery and a liquid battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0124] Figure 1 aLi3PO4∙bP4S in Example 1 10+x , x =6; a≤5 wt.%; b= 1 wt.% of the positive electrode material;

[0125] Where ac is the SEM image of the material at different magnifications; d is the EDS spectrum of the material;

[0126] Figure 2 aLi3PO4∙bP4S in Example 1 10+x , x =6; a≤5 wt.%; b= 1 wt.% of the positive electrode material with high resolution transmission electron microscopy and EDS element distribution map;

[0127] Wherein, a is a high-resolution transmission electron microscope (HAAD) image, in which two intervals are magnified and energy spectrum detected, namely, the secondary particle surface (marked as Zone 1 in the figure) and the primary particle surface and grain boundary (marked as Zone 2 in the figure); bi is a high-resolution transmission electron microscope image and energy spectrum image at the secondary particle surface, each of which corresponds to the HAAD image of the secondary particle surface (b), the element distribution image of the Ni element (c), the element distribution image of the Co element (d), the element distribution image of the P element (e), the element distribution image of the S element (f), the element distribution image of the O element (g), the representative element distribution image of the superposition of C, O, P, S, and Ni elements (h) and the element content change curve (i); jm is a high-resolution transmission electron microscope image and energy spectrum image at the primary particle surface and grain boundary, each of which corresponds to the HAAD image of the primary particle surface and grain boundary (j), the element distribution image of the Ni element (k), the element distribution image of the P element (l), and the element distribution image of the S element (m);

[0128] Figure 3aLi3PO4∙bP4S in Example 1 10+x , x =6; a≤5 wt.%; b= 1 wt.% of the positive electrode material and the high-energy XPS comparison spectra of the LPO-NMC811 positive electrode material obtained in Comparative Example 2, with energy changes of 3000, 6000 and 8000 eV;

[0129] Wherein a is a schematic diagram of the mechanism of synchrotron radiation X-ray fluorescence spectroscopy; b is the XPS spectra of the P element 1s of the LPO-NMC811 sample obtained in Comparative Example 2 at different energies, c is the XPS spectra of the O element 1s of the LPO-NMC811 sample obtained in Comparative Example 2 at different energies, d is the XPS spectra of the S element 1s of the 1% PS-LPO-NMC811 sample obtained in Example 1 at different energies, e is the XPS spectra of the P element 1s of the 1% PS-LPO-NMC811 sample obtained in Example 1 at different energies, and f is the XPS spectra of the O element 1s of the 1% PS-LPO-NMC811 sample obtained in Example 1 at different energies;

[0130] Figure 4 aLi3PO4∙bP4S in Example 2 10+x , x =6; a≤5 wt.%; b= 5 wt.% of the positive electrode material; wherein a is a scanning electron microscope image at a magnification of 5k, and b is a scanning electron microscope image at a magnification of 10k;

[0131] Figure 5 The figure is a comparison of the charge and discharge curves of the all-solid-state LiIn-NMC811 battery at room temperature in Application Example 1, Comparative Examples 1 and 2; wherein the all-solid-state LiIn-NMC811 battery is charged and discharged at a current density of 100 microamperes, and the cut-off voltage is 1.9-3.7 volts;

[0132] Figure 6 It is a comparison diagram of electrochemical cycles of all-solid-state LiIn-NMC811 batteries at room temperature in Application Example 1, Comparative Examples 1 and 2;

[0133] Figure 7 It is a comparison chart of the electrochemical rate of the all-solid-state LiIn-NMC811 battery at room temperature in Application Example 1, Comparative Examples 1 and 2;

[0134] Figure 8 This is a comparison diagram of electrochemical cycles of all-solid-state LiIn-NMC811 batteries of Application Example 1 and Application Example 2 under room temperature conditions;

[0135] Fig. 9This is a diagram showing the changes in the structure, morphology and surface coating of the positive electrode particles after 100 cycles of the all-solid-state battery in Application Example 1; a is a transmission electron microscope image of the entire particle at a low magnification, b is a high-resolution transmission electron microscope diffraction fringe image, and c is a transmission electron microscope diffraction fringe image at a higher magnification and its corresponding atomic arrangement;

[0136] Fig.10 It is a diagram showing the changes in the structure, morphology and surface coating of the positive electrode particles after 100 cycles of the all-solid-state battery in Comparative Example 2; a is a transmission electron microscopy image of the entire particle at a low magnification, b is a high-resolution transmission electron microscopy image of the grain boundary of the primary particle, c is a high-resolution transmission electron microscopy image of the grain boundary of the primary particle at a higher magnification, d is a high-resolution transmission electron microscopy image in the box marked as d in Figure c, e is a high-resolution transmission electron microscopy image in the box marked as e in Figure c, and f is a demonstration image of the phase change of the surface structure of the primary particle;

[0137] Fig.11 The result diagram of the chemical reaction theory calculation of the interdiffusion reaction between LPO-NMC-10nm and sulfur-rich phase P4S16 or non-sulfur-rich phase P2S5 in Application Example 1 and Comparative Example 3; Chinese and English comparison in Table 1;

[0138]

[0139]

[0140] Table 1 shows the specific Chinese meanings of the English words mentioned in the drawings of the specification. DETAILED DESCRIPTION

[0141] The present invention is described below by specific embodiments. Unless otherwise specified, the technical means used in the present invention are methods known to those skilled in the art. In addition, the embodiments should be understood as illustrative rather than limiting the scope of the present invention, and the essence and scope of the present invention are limited only by the claims. For those skilled in the art, various changes or modifications to the material composition and dosage in these embodiments, without departing from the essence and scope of the present invention, also belong to the protection scope of the present invention. The raw materials and reagents used in the present invention are all commercially available.

[0142] The following X-ray diffraction was measured using copper Kα rays (X-ray diffractometer: Bruker, Germany, model D8 Advance) and a synchrotron radiation source (Canadian Light Source, beamline: SXRMB (soft X-ray microcharacterization beamline)).

[0143] The following ion conductivity method uses AC impedance testing, and the testing method is: weigh 150 mg of solid electrolyte in the glove box, then press it into a sheet in the mold battery at a pressure of 350 MPa, then measure the thickness of the electrolyte layer and record it as L, then directly assemble it into a carbon / electrolyte / carbon symmetrical battery in the mold battery, measure the AC impedance of the battery under open circuit conditions, and record the impedance value as R, which is calculated using the formula σ = L / (R·A), where σ is the ionic conductivity, L is the thickness of the electrolyte layer, R is the impedance value, and A is the electrode area of ​​the electrolyte sheet.

[0144] Example 1

[0145] The positive electrode active material is LiNi 0.8 Mn 0.1 Co 0.1 O2 (NMC811), coated with aLi3PO4∙bP4S 10+x , x =6; a≤5wt.%; b= 1 wt.% is prepared as follows:

[0146] Weigh 10g of commercially purchased NMC811 material, dry it in a vacuum oven, and evenly disperse it in the tray of an atomic layer deposition device (Cambridge Nanotech, USA). Use lithium tert-butyl alcohol (LiOtBu) and trimethyl phosphate (TMPO) as precursors for atomic layer deposition reaction. The reaction rate is set to deposit 0.07 nanometers of amorphous phase Li3PO4 per cycle. Different thicknesses of amorphous phase Li3PO4 can be deposited on the surface of NMC811 by using different numbers of cycles. In this embodiment, the number of cycles is set to 70 cycles (~5 nm), 150 cycles (~10 nm), and 300 cycles (~20 nm). The samples obtained after the atomic layer deposition reaction are directly transferred to the glove box and marked as LPO-NMC-7nm, LPO-NMC-10nm, and LPO-NMC-20nm, respectively, for standby. On the other hand, 1.24g of elemental P and 5.12g of elemental S were accurately weighed according to a molar ratio of 4:16, ground and mixed in a mortar, and then directly poured into a single-head sealed quartz tube with an inner diameter of 10mm. After vacuum sealing, the tube was placed in a muffle furnace at 350 degrees Celsius for 2 days. After the reaction was completed, the quartz tube was opened in a drying room to take out the sample, and after grinding, the sulfur-rich phase molecule P4S 16 .

[0147] In the glove box, weigh 0.2g of sulfur-rich phase molecule P4S in a beaker. 16 Then, diethylene glycol dimethyl ether (DEGDME) was added until the total solution mass was 20 g, and the solution was allowed to stand for 12 hours to allow P4S 16Fully dissolved in DEGDME solution, the resulting solution is 1 wt.% P4S 16 / DEGDME solution. Subsequently, 1 g of LPO-NMC-7nm, LPO-NMC-10nm and LPO-NMC-20nm samples were weighed and placed in a 5 ml bottle, and 1 g of 1 wt.% P4S 16 / DEGDME solution, stirred overnight with a magnetic stirrer, placed in a vacuum oven and dried at 80 degrees Celsius for 12 hours to obtain a positive electrode active material of LiNi 0.8 Mn 0.1 Co 0.1 O2 (NMC811), coated with aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.%; b= 1 wt.% of the positive electrode material, the material is marked as PS-LPO-NMC811 or 1%PS-LPO-NMC811.

[0148] The samples were characterized by scanning electron microscopy, transmission electron microscopy, XPS, XAS and ToF-SIMS to detect the morphology, structure and composition curve of the surface coating layer with component gradient distribution.

[0149] Figure 1 aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.%; b= 1 wt.% of the positive electrode material;

[0150] Figure 2 aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.%; b= 1 wt.% high-resolution transmission electron microscopy and EDS element distribution diagram of the positive electrode material. It can be seen from the figure that a coating layer with a component gradient distribution is obtained on the surface of NMC811, in which the oxygen content gradually increases with the depth of detection, and the change curve of sulfur content is just the opposite.

[0151] Figure 3 aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.%; b= 1 wt.%, the energy changes are 3000, 6000 and 8000 eV. It can be seen from the figure that a coating layer with a gradient distribution of components is obtained on the surface of NMC811. With the increase of XPS energy, that is, the deeper the detection depth, the content of PS-Li chemical components gradually decreases, and its PO x Sy The content of -Li chemical components gradually increases, which further proves that a coating layer with gradient distribution of components is formed on the surface of NMC.

[0152] Example 2

[0153] The positive electrode active material is LiNi 0.8 Mn 0.1 Co 0.1 O2 (NMC811), coated with aLi3PO4∙bP4S 10+x , x =12; a≤5 wt.%; b= 2.5 or 5 wt.% is prepared as follows:

[0154] Similar to Example 1, except that 1) the sulfur-rich phase molecule P4S 10+x In x Optimized to 10 instead of 6; 2) P4S 10+x / DEGDME solution optimized to 2.5 wt.% P4S 20 / DEGDME solution and 5 wt% P4S 20 / DEGDME solution. The two were labeled as 2.5%PS-LPO-NMC811 and 5%PS-LPO-NMC811, respectively.

[0155] The samples were characterized by scanning electron microscopy, transmission electron microscopy, XPS, XAS and ToF-SIMS to detect the morphology, structure and composition curve of the surface coating layer with component gradient distribution.

[0156] Figure 4 aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.%; b= 5 wt.% of the positive electrode material;

[0157] Example 3

[0158] Similar to Example 1, except that the positive electrode active material is changed to LiCoO2, the number of cycles during the atomic layer deposition reaction is set to 100, and lithium tert-butoxide (LiOtBu), trimethyl phosphate (TMPO), and tetrakis(dimethylamido)zirconium (IV) are used as precursors.

[0159] Example 4

[0160] Similar to Example 1, except that the positive electrode active material is changed to lithium-rich lithium manganese oxide, the number of cycles during the atomic layer deposition reaction is set to 200, and lithium tert-butoxide (LiOtBu), H2O, and tantalum pentaethanol (Ta(EtOH)5) are used as precursors.

[0161] Example 5

[0162] Similar to Example 1, except that 1) the sulfur-rich phase molecule P4S 10+x In x The optimized value is 20 instead of 6; 2) the positive electrode active material is changed to lithium iron phosphate, 3) the number of cycles in the atomic layer deposition reaction is set to 150, and lithium tert-butoxide (LiOtBu), trimethyl phosphate (TMPO), and titanium (IV) isopropoxide are used as precursors.

[0163] Example 6

[0164] Similar to Example 1, except that 1) the positive electrode active material is changed to lithium nickel cobalt aluminum oxide, 2) the number of cycles in the atomic layer deposition reaction is set to 300, and trimethylaluminum, lithium trimethylsilane and Ozone are used as precursors.

[0165] Application Example 1

[0166] The positive electrode active material prepared in Example 1 is LiNi 0.8 Mn 0.1 Co 0.1 O2 (NMC811), coated with aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.%; b= 1 wt.% of positive electrode material (for application of solid-state lithium (ion) full battery. The specific operation is as follows:

[0167] The positive electrode material prepared in Example 1, Li 10 GeP2S 12 The solid electrolyte materials were mixed in a ratio of 70:30 (mass ratio) and ground manually for 5 minutes. The mixing process was carried out in a glove box. The obtained sample was the positive electrode powder of the secondary battery. The metal thin indium sheet was used as the negative electrode, and the electrolyte was also Li 10 GeP2S 12 Solid electrolyte material; take 150 mg Li 10 GeP2S 12 The solid electrolyte was placed in a mold battery liner with a cross-sectional area of ​​0.785 square centimeters and pressed at a pressure of 100 MPa to obtain the electrolyte layer. 10 GeP2S 12Add 10 mg of positive electrode powder to one end of the solid electrolyte layer, spread it evenly, and then press it for the second time at a pressure of 350 MPa to press the positive electrode layer and the electrolyte layer together; after pressing, put an indium sheet as the negative electrode layer at the other end and press it for the third time at a pressure of 50 MPa; after the whole process is completed, put the inner tank into the mold battery, press it tightly and tighten the screws to seal it. After sealing, you can get a fully solid-state LiIn-NMC811 secondary battery.

[0168] Application Example 2

[0169] Similar to Application Example 1, except that the positive electrode active material prepared in Example 2 is LiNi 0.8 Mn 0.1 Co 0.1 O2 (NMC811), coated with aLi3PO4∙bP4S 10+x , x =6; a≤5 wt.% ; b= 2.5 or 5 wt.% of positive electrode materials for application in solid-state lithium (ion) full batteries.

[0170] Application Example 3

[0171] Similar to Application Example 1, except that the positive electrode active material prepared in Example 6 is lithium nickel cobalt aluminum oxide, and the coating layer is aLiAlO2∙bP4S 10+x , x =6; a≤5 wt.% ; b= 1 wt.% positive electrode material for application in solid-state lithium (ion) full batteries.

[0172] The specific operations are as follows:

[0173] The positive electrode material, Li3InCl6 solid electrolyte material and carbon black prepared in Example 6 are mixed in a ratio of 70:25:5 (mass ratio). The mixing method is manual grinding for 5 minutes. The mixing process is carried out in a glove box. The obtained sample is the positive electrode powder of the secondary battery. A thin metal lithium sheet is used as the negative electrode, and the electrolyte is composed of a double-layer electrolyte layer using Li3InCl6 and Sb-doped Li6PS5Cl solid electrolyte materials; 50 mg of Li3InCl6 solid electrolyte is put into a mold battery liner with a cross-sectional area of ​​0.785 square centimeters, and the tablet is pressed at a pressure of 100 MPa, and then 50 mg of Sb-doped Li6PS5Cl solid electrolyte material is added to one end of the previously pressed Li3InCl6 solid electrolyte sheet, flattened and pressed at a pressure of 100 MPa to obtain a double-layer electrolyte layer. Then, add 10 mg of positive electrode powder to one end of the Li3InCl6 solid electrolyte layer, spread it evenly, and press it for the third time at a pressure of 350 MPa to press the positive electrode layer and the electrolyte layer together; after pressing, put a metal lithium sheet as the negative electrode layer at the other end and press it for the fourth time at a pressure of 50 MPa; after the whole process is completed, put the inner tank into the mold battery, press it tightly and tighten the screws to seal it. After sealing, you can get a fully solid lithium-lithium nickel cobalt aluminum oxide fully solid secondary battery.

[0174] Application Example 4

[0175] Similar to Application Example 1, the difference is that the positive electrode active material prepared in Example 3 is LiCoO2, and the coating layer is aLi3P 0.4 Zr 0.5 O4∙bP4S 10+x , x =6; a=2 wt.%; b= 1 wt.% of positive electrode materials are used for solid-state lithium (ion) full batteries.

[0176] The specific operations are as follows:

[0177] The positive electrode material prepared in Example 3, Li3YO 0.1 Cl 5.8The solid electrolyte material and carbon black were mixed in a ratio of 70:25:5 (mass ratio). The mixing method was manual grinding for 5 minutes. The mixing process was carried out in a glove box. The obtained sample was the positive electrode powder of the secondary battery. Graphite was used as the negative electrode, and the electrolyte was composed of O-doped Li6POS5Cl solid electrolyte material to form a double-layer electrolyte layer; 100 mg of O-doped Li6POS5Cl solid electrolyte material was placed in a mold battery liner with a cross-sectional area of ​​0.785 square centimeters, flattened and pressed at a pressure of 100 MPa. Subsequently, 10 mg of positive electrode powder was added to one end of the solid electrolyte layer, and after spreading, the positive electrode layer and the electrolyte layer were pressed together at a pressure of 100 MPa for the second time; graphite powder was placed at the other end of the electrolyte sheet as the negative electrode layer and pressed for the third time at a pressure of 350 MPa; after pressing, 0.1 ml of ester electrolyte (1 mol L-1 LiPF6 / DMC-DEC organic electrolyte) was added to both the positive and negative sheets, and the sheets were left to stand for 1 hour. After the whole process was completed, the inner liner was placed in the mold battery, pressed and tightened to seal. After sealing, a fully solid-state graphite-lithium cobalt oxide semi-solid secondary battery was obtained.

[0178] Comparative Example 1

[0179] Similar to Application Example 1, the difference is that NMC811 without surface coating modification is used as the positive electrode material.

[0180] Comparative Example 2

[0181] Similar to Application Example 1, the difference is that the intermediate product LPO-NMC-10nm material obtained in Example 1 is used as the positive electrode material. This material is a coating of amorphous Li3PO4 with a nanometer thickness on the surface of NMC811, and the construction of a coating layer with a component gradient distribution is not achieved. This material is marked as LPO-NMC811.

[0182] Comparative Example 3

[0183] Similar to Application Example 1, the difference is that the surface coating layer of NMC811 is constructed by using a similar interdiffusion process between non-sulfur-rich P2S5 and LPO-NMC-10nm. 0.8 Mn 0.1 Co 0.1 O2 (NMC811), coated with aLi3PO4∙bP4S 10+x , x=6; a≤5 wt.%; b= 1 wt.% of the positive electrode materials are similar in composition, but because Li3PO4 and P2S5 do not undergo spontaneous chemical reaction, the construction of a coating layer with a component gradient distribution on the NMC811 surface cannot be achieved.

[0184] Figure 5 The figure is a comparison of the charge and discharge curves of the all-solid-state LiIn-NMC811 battery at room temperature in Application Example 1, Comparative Examples 1 and 2; wherein the all-solid-state LiIn-NMC811 battery is charged and discharged at a current density of 100 microamperes, and the cut-off voltage is 1.9-3.7 volts. It can be seen from the figure that the positive electrode material with a coating layer having a surface gradient distribution can obtain higher electrochemical activity and charge and discharge capacity, first efficiency, lower electrode polarization and other effects.

[0185] Figure 6 This is a comparison of the electrochemical cycles of all-solid-state LiIn-NMC811 batteries at room temperature in Application Example 1, Comparative Examples 1 and 2. As can be seen from the figure, the use of a positive electrode material with a coating layer having a surface gradient distribution can achieve better long-cycle stability and other effects. No drastic capacity decay was observed after 250 cycles.

[0186] Figure 7 This is a comparison chart of the electrochemical rate of the all-solid-state LiIn-NMC811 battery at room temperature in Application Example 1, Comparative Examples 1 and 2. As can be seen from the figure, the positive electrode material with a coating layer having a surface gradient distribution can achieve higher rate performance.

[0187] Figure 8 This is a comparison diagram of electrochemical cycles at room temperature for all-solid-state LiIn-NMC811 batteries in Application Example 1 and Application Example 2. As can be seen from the figure, the optimized positive electrode material with a surface gradient coating layer is the key to achieving high electrochemical activity and high cycle stability.

[0188] Fig. 9 This is a diagram showing the changes in the structure, morphology and surface coating of the positive electrode particles after 100 cycles of the all-solid-state battery in Application Example 1. As can be seen from the figure, after a long cycle, the positive electrode material with a coating layer with a surface gradient distribution has no obvious structural decay in its particles, and only a structural change of about 2 nanometers occurs on the surface.

[0189] Fig.10 The figure shows the changes in the structure, morphology and surface coating of the positive electrode particles after 100 cycles of the all-solid-state battery in comparative example 2. It can be seen from the figure that after a long cycle, the positive electrode material without a coating layer with a surface gradient distribution has obvious structural decay in its particles, and an obvious transition from a layered structure with high electrochemical activity to a rock salt phase structure with no electrochemical activity appears at its grain boundary.

[0190] Fig.11 The results of the chemical reaction theory calculation of the interdiffusion reaction between LPO-NMC-10nm and sulfur-rich phase P4S16 or non-sulfur-rich phase P2S5 in Application Example 1 and Comparative Example 3 are shown in FIG. It can be found that Li3PO4 and sulfur-rich phase P4S16 can spontaneously undergo chemical reactions to achieve the process of element interdiffusion; for Li3PO4 and non-sulfur-rich phase P2S5, the calculation shows that the two cannot undergo chemical reactions, and it is difficult to achieve the construction of a coating layer with a component gradient distribution.

[0191] The results show that, compared with the positive electrode active material without a coating layer and the positive electrode material without a component gradient distribution, the positive electrode provided by the present invention, especially the coating layer with a component gradient distribution with a nanometer-level thickness, has obvious effects in at least 1) stabilizing the surface and grain boundaries of the positive electrode active material and reducing structural decay; 2) improving the activity of the positive electrode active material; 3) improving the long-cycle stability of the all-solid-state battery; and 4) improving the battery rate performance.

[0192] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A lithium-ion battery composite positive electrode material, comprising: Composite materials, positive electrode active materials, and a coating layer located on the surface of the positive electrode active material, The coating layer is a coating layer with a component gradient distribution with a nanometer-level thickness, and the coating layer is a mixture of one or more of an amorphous phase, a crystalline phase, and a glass ceramic phase; the coating layer has a thickness between 5 nanometers and 200 nanometers; The coating layer with gradient distribution of components is composed of nanometer-level amorphous phase Li3PO4 and sulfur-rich phase phosphorus-sulfur molecules P4S 10+x Obtained through interdiffusion reaction, expressed as formula 1: Formula 1 aLi3PO4·bP4S10+x In formula 1 30≥x≥2; a≤5wt.%; b<5wt.%, Where a is the mass percentage of Li3PO4 in the entire positive electrode active material, b is P4S 10+x The mass percentage of the entire positive electrode active material; wherein the coating layer with a gradient distribution of components is obtained by multi-step epitaxial growth on the surface of the positive electrode active material; The component gradient distribution means that the coating layer has a high O content at the end close to the positive electrode active material and a high S content at the end away from the positive electrode active material; the S and O element contents in the coating layer are distributed gradiently from the end close to the positive electrode active material to the outside; the amorphous phase Li3PO4 and the sulfur-rich phase phosphorus-sulfur molecules P4S 10+x Through interdiffusion reaction, it means that the amorphous phase Li3PO4 with a thickness of nanometers is directly epitaxially deposited and grown on the surface of the positive electrode active material using atomic layer deposition technology, with a thickness between 2 nanometers and 50 nanometers. The sulfur-rich phase phosphorus-sulfur molecules P4S 10+x It is prepared by eutectic reaction of elemental P and elemental S according to the stoichiometric ratio; in order to realize the sulfur-rich phase phosphorus-sulfur molecule P4S 10+x The quantitative preparation of the eutectic reaction is replaced by ball milling-sintering and reaction in an organic solution; wherein the process of the interdiffusion reaction is as follows: an ester, ether or ketone organic solvent is used to dissolve the sulfur-rich phase phosphorus sulfur molecules P4S 10+x , to obtain a certain concentration of P4S 10+x In the solution phase, the positive electrode material with amorphous phase Li3PO4 epitaxially grown on the surface with a nanometer thickness obtained by atomic layer deposition is immersed in the P4S 10+x The reaction is carried out in a solution, the mass ratio between the two, the reaction time and the reaction temperature conditions are optimized, and then the nano-thick amorphous phase Li3PO4 and the sulfur-rich phase phosphorus-sulfur molecule P4S are achieved by heating, drying and vacuum annealing. 10+x The interdiffusion reaction between the two is carried out in a glove box with an inert atmosphere; the multi-step epitaxial growth on the surface of the positive electrode active material is as follows: 1) multi-step atomic layer deposition is carried out on the surface of the positive electrode active material to obtain an amorphous phase Li3PO4 with different thicknesses; 2) the amorphous phase Li3PO4 is then sulfurized by a liquid phase immersion reaction method, and the amorphous phase Li3PO4 is reacted with the sulfur-rich phase phosphorus-sulfur molecules P4S 10+x The chemical reaction between the two and the mutual diffusion of P, S, O and Li realize the preparation of the coating layer with component gradient distribution; the component gradient distribution refers to the use of X-ray fluorescence spectroscopy (XPS), electron energy spectrum (EDS), time-of-flight-secondary ion mass spectrometry (Tof-SIMS), X-ray absorption spectroscopy (XAS) testing methods to detect the element composition and content at different depths of the coating layer, and the characteristic of the element composition having a content gradient distribution with different detection depths can be obtained.

2. The lithium-ion battery composite positive electrode material of claim 1, wherein the positive electrode active material comprises lithium nickel manganese oxide, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxide, lithiated layered sulfide, or a combination thereof; the surface of the lithium-ion battery composite positive electrode material comprises the surface of primary particles and secondary particles.

3. The lithium-ion battery composite positive electrode material according to claim 1 or 2, wherein the amorphous phase Li3PO4 is completely or partially replaced by a C metal element, and the C metal element is one or more of Ta, Ge, Ti, Zr, Al, Hf, Nb, V, Zn, Sn, Mo, Ru, Co, Mn, and Fe, and the substitution refers to partial or complete substitution of the P element by adding a precursor containing the C metal element during the atomic layer deposition process.

4. The lithium-ion battery composite positive electrode material according to claim 1, further comprising an ion conductive additive and a conductive additive; the ion conductive additive comprises a sulfide electrolyte, an oxide electrolyte, a halide electrolyte, or a combination thereof; the conductive additive comprises carbon nanofibers, graphite, carbon black, graphene, carbon nanotubes, a conductive polymer mainly formed by polymerization of 3,4-ethylenedioxythiophene monomers, or a combination thereof.

5. A lithium ion battery comprising: Positive electrode; the positive electrode comprises the lithium ion battery composite positive electrode material according to any one of claims 1 to 4; negative electrode; and an electrolyte interposed between the positive electrode and the negative electrode and including a sulfide solid electrolyte, an oxide solid electrolyte, a halide electrolyte, a nitride electrolyte, a polymer electrolyte, an organic electrolyte, or a combination thereof.

6. The lithium ion battery of claim 5, wherein the lithium ion battery comprises an all-solid battery, a semi-solid battery, and a liquid battery.

7. Application of the lithium-ion battery composite positive electrode material according to claim 1 to improve the capacity, initial efficiency and long cycle performance of positive electrode active materials.

8. Application of the lithium-ion battery composite positive electrode material according to claim 1 to improve the commercial application value of lithium-ion batteries including all-solid-state secondary batteries; the commercial application value refers to improving the structural stability of the positive electrode active material and reducing the surface impedance of the material.

Citation Information

Patent Citations

  • Anode active material, preparation method of anode active material, high-performance anode slurry containing anode active material, and all-solid-state lithium ion battery

    CN106784798A

  • Lithium-rich antiperovskite-coated LCO-based lithium composite, method for preparing same, and positive electrode active material and lithium secondary battery comprising same

    CN109155411A

  • Lithium ion battery electrode material and preparation method thereof

    CN112909224A

  • Cathode, all-solid secondary battery including cathode, and method of preparing all-solid secondary battery

    US20210280873A1

  • Composite material, preparation method therefor, and negative electrode

    WO2022016374A1