Aluminum bag film for secondary battery and method for manufacturing the same
By using a copolymer of polyamide and polyimide as the outer resin layer in the secondary battery aluminum bag film, which is directly bonded to the aluminum layer, the aluminum bag film is prevented from being damaged in high temperature, high salt, and high humidity environments. solve the problem, achieve efficient chemical resistance and heat resistance, reduce the risk of battery expansion and explosion, and improve the safety of large-capacity batteries.
Patent Information
- Application Number
- CN202080070102.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-06
- Filing Date
- 2020-08-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-08-06
AI Technical Summary
The aluminum pouch film of existing secondary batteries is easily damaged in high-temperature, high-salt, high-humidity and ultraviolet environments, resulting in exposure of the aluminum layer, causing corrosion reactions and the risk of battery expansion and explosion, and the adhesive strength of the polyimide film is reduced. , difficult to maintain stability under harsh conditions.
A copolymer of polyamide and polyimide is used as the outer resin layer, which is directly bonded to the aluminum layer to form a structure of aluminum layer, inner resin layer and adhesive layer. The copolymer molar ratio is 1:9 to 9:1 , manufactured through dry lamination or extrusion lamination, ensuring that bonding strength and molding properties are maintained in high temperature, high salt and UV environments.
It improves the chemical resistance, heat resistance and salt resistance of the aluminum bag film, prevents chemical reactions caused by contact between the aluminum layer and the electrolyte, reduces the risk of battery expansion and explosion, and improves safety in large-capacity batteries.
Smart Images

Figure CN114651362B_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0095787 filed on August 6, 2019, the entire contents of which are incorporated into this specification by reference.
[0002] The present invention relates to an aluminum bag film for a secondary battery and a method for manufacturing the aluminum bag film, and more particularly, to an aluminum bag film for a secondary battery having significantly improved chemical resistance, heat resistance and electrolyte resistance compared to packaging films used in the art, and a method for manufacturing the aluminum bag film. Background Art
[0003] Secondary batteries are electrochemical devices that are recently used to power various electronic and electrical products, generally referring to lithium secondary batteries, and refer to batteries having polymer electrolytes and generating current by lithium ion migration. As an external material for packaging to protect such secondary batteries, a bag-shaped film in which polymers and metals are laminated is used. This bag-shaped film for secondary batteries has the form of an aluminum film disposed therebetween, so as to protect a battery cell formed by an electrode assembly and an electrolyte filled therein by a subsequent process, and stably maintain the electrochemical properties of the battery, etc., and in order to protect the battery cell from external impacts, a polyethylene terephthalate (PET) resin, a nylon film, etc. are formed on the aluminum film as an external resin layer.
[0004] In the bag film, the upper bag film and the lower bag film are bonded on the outer peripheral surface by thermal bonding, etc., and an adhesive layer made of thermoplastic polyolefin such as polyethylene (PE) or polypropylene (PP) or their copolymers is formed between the lower surface of the upper bag film and the upper surface of the lower bag film.
[0005] The bag-shaped film is generally formed into a predetermined layered structure having, in order, an inner resin layer in direct contact with the electrolyte, a second adhesive layer, an aluminum layer, a first adhesive layer, and an outer resin layer in direct contact with the outside.
[0006] The pouch-type secondary battery formed in the above structure may be damaged due to various reasons in various cases. For example, during the storage of the electrode assembly inside the pouch, a protruding portion such as an electrode tap or an electrode lead causes damage such as cracks on the inner layer of the pouch, and the aluminum layer may be exposed due to such damage.
[0007] In addition, when the bag-shaped film is heat-sealed, heat is applied from the outside, and pinholes are generated or damage is caused due to the heat, resulting in cracks on the inner adhesive layer, and the aluminum layer is exposed to the electrolyte, etc.
[0008] In addition to the above reasons, the adhesive layer formed in a thin film form may be damaged by dropping, impact, pressure, compression, etc., and the aluminum layer is exposed to an electrolyte, etc. through the damaged portion.
[0009] The aluminum layer exposed to the electrolyte as above may be corroded because the electrolyte infiltrated or diffused into the battery causes a chemical reaction with oxygen or moisture, which causes a problem of generating corrosive gas and thereby causing expansion that expands inside the battery.
[0010] More specifically, LiPF 6 It can react with water and oxygen to generate hydrofluoric acid (HF), which is a corrosive gas. This hydrofluoric acid can react with aluminum to cause a rapid exothermic reaction, and, as a second reaction, the hydrofluoric acid is adsorbed on the aluminum surface and penetrates into the system. This increases the fragility of the system, causing cracks in the bag film even under micro-impacts, and here, due to electrolyte leakage, lithium and the atmosphere react to cause fire.
[0011] Therefore, various aluminum surface modification techniques have been studied to prevent contact with the aluminum of the central portion even when corrosive hydrofluoric acid is generated as described above. As aluminum surface modification techniques, heat treatment or other conversion treatments; sol-gel coating; primer treatment; treatment with corona, plasma, etc. may be included.
[0012] However, with the recent trend of gradually increasing the capacity of secondary batteries, aluminum surface modification alone has limitations in solving these problems, and there has been a continuous demand for an aluminum pouch film for secondary batteries having excellent chemical resistance, durability, electrolyte resistance, and moldability.
[0013] Furthermore, not only the electric vehicle industry, which has been conducting research for some time, but also as the application range of secondary batteries is expanded to the shipbuilding industry, the aviation industry, etc., research and development using high-capacity secondary batteries has been actively conducted.
[0014] However, when a nylon film susceptible to harsh environments such as high temperature, high salt, high humidity and ultraviolet rays is used as an outer resin layer in a bag-shaped film of a high-capacity secondary battery, problems of weak chemical resistance and electrolyte resistance have been raised. For example, when exposed to moisture containing high salt due to cracks in the bag-shaped film, there are problems such as degradation of the performance of the nylon film, generation of corrosive gases, or the possibility that the aluminum in the inner center portion contacts and reacts with the salt and moisture. It is also raised that the use of a polyurethane adhesive under the above conditions cannot prevent peeling or delamination.
[0015] Therefore, a method of laminating a polyimide film having excellent chemical resistance and heat resistance as an outer resin layer instead of the existing nylon film has been proposed, however, when the polyimide film is laminated as the outer resin layer, there is a problem of reduced adhesive strength. In order to overcome this problem, it is necessary to study a method of laminating a polyimide film on an aluminum layer without reducing adhesive strength under conditions of high temperature, high salt, high humidity and ultraviolet rays.
[0016] [Prior art literature]
[0017] [Patent Document]
[0018] (Patent Document 1) Korean Patent Publication No. 10-2001-7010231 (November 15, 2001) “Packaging material for polymer battery and method for manufacturing the same” Summary of the invention
[0019] Technical issues
[0020] The present invention is made in view of the above problems, and aims to provide an aluminum bag film for a secondary battery, which maintains excellent chemical resistance, heat resistance, salt resistance and electrolyte resistance even when the secondary battery is used in an environment of high temperature, high salt, high humidity and ultraviolet light; and a method for manufacturing the aluminum bag film.
[0021] Technical Solution
[0022] According to a first aspect of the present invention, there is provided an aluminum bag film for a secondary battery, the aluminum bag film comprising: an aluminum layer; an external resin layer formed on a first surface of the aluminum layer; an internal resin layer formed on a second surface of the aluminum layer; and an adhesive layer for bonding the aluminum layer to the internal resin layer, wherein the external resin layer comprises a copolymer of polyamide and polyimide.
[0023] In one embodiment of the present invention, polyamide and polyimide are copolymerized in a molar ratio of 1:9 to 9:1 in the outer resin layer.
[0024] In one embodiment of the present invention, the outer resin layer is directly bonded to the aluminum layer without an adhesive layer between the two layers.
[0025] In one embodiment of the present invention, after a 5 cm×5 cm sample of the outer resin layer is immersed in seawater having a salt concentration of 3.5% and a temperature of 85° C. for 24 hours, the adhesive strength between the outer resin layer and the aluminum layer is 2 N / 15 mm or more.
[0026] According to a second aspect of the present invention, there is provided a method for manufacturing an aluminum bag film for a secondary battery, the method comprising: a) preparing an aluminum layer; b) forming an external resin layer on a first surface of the aluminum layer; and c) bonding an internal resin layer to a second surface of the aluminum layer, wherein the external resin layer comprises a copolymer of polyamide and polyimide.
[0027] Beneficial Effects
[0028] The use of the aluminum bag film for secondary batteries according to the present invention can prevent the aluminum layer from chemically reacting when in contact with water containing an electrolyte or salt, and from deforming the bag film when exposed to harsh environments such as high temperature and ultraviolet rays, thereby reducing the risk of internal expansion of the battery due to gas generation inside the battery or explosion due to high temperature. In addition, microcracks are prevented from being generated, which is preferred for increasing the battery size for mass production of large-capacity batteries used in electric vehicles, marine electric ships, etc., and can improve the safety of the battery environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The structure of an aluminum bag film for a secondary battery according to a preferred embodiment of the present invention is shown. DETAILED DESCRIPTION
[0030] The embodiments provided according to the present invention can all be realized through the following description. The following description needs to be understood as describing the preferred embodiments of the present invention, and it should be understood that the present invention is not necessarily limited thereto.
[0031] The present invention provides an aluminum bag film for a secondary battery, the aluminum bag film comprising: an aluminum layer; an external resin layer formed on a first surface of the aluminum layer; an internal resin layer formed on a second surface of the aluminum layer; and an adhesive layer for bonding the aluminum layer to the internal resin layer, wherein the external resin layer comprises a copolymer of polyamide and polyimide.
[0032] Hereinafter, each configuration of the aluminum pouch film for a secondary battery of the present invention will be described in detail.
[0033] Aluminum layer
[0034] In the film for secondary battery packaging material of the present invention, aluminum or aluminum alloy is suitable as a material for a metal film used as a barrier layer for preventing oxygen, moisture, etc. from penetrating from the outside. As an aluminum alloy, an alloy obtained by adding various metals and non-metals to pure aluminum, or a stainless steel alloy can be used. As an aluminum layer, a soft aluminum foil can be preferably used, and more preferably, an aluminum foil containing iron is used to provide molding properties for the aluminum foil. For aluminum foil, a series with high purity has excellent processing properties, and therefore, an aluminum alloy foil of the No. 1000 series or the No. 8000 series is preferred. In addition, the aluminum base can optionally be an alloy containing atoms selected from silicon, boron, germanium, arsenic, antimony, copper, magnesium, manganese, zinc, lithium, iron, chromium, vanadium, titanium, bismuth, potassium, tin, lead, zirconium, nickel, cobalt and combinations thereof. In the iron-containing aluminum foil, the content of iron can be preferably 0.1% by mass to 9.0% by mass, more preferably 0.5% by mass to 2.0% by mass, relative to the total mass of 100% of the aluminum foil. When the iron content in the aluminum foil is less than 0.1% by mass, the softness of the aluminum layer is reduced, and the iron content greater than 9.0% by mass causes the problem of reduced forming performance. The aluminum foil used in the aluminum layer can have an etched or degreased surface to improve the adhesion to the internal resin layer, however, the treatment can be skipped to reduce the process speed. The aluminum layer is used to prevent gas and water vapor from penetrating into the battery from the outside, and the aluminum film is required to have no pinholes and have processing suitability (bag packaging, embossing molding). Considering processing performance, oxygen and moisture barrier properties, etc., the thickness is preferably 10μm to 100μm, more preferably 30μm to 50μm. Not meeting the above range has the following problems, when the thickness is less than 10μm, the aluminum layer is easily torn and the electrolytic resistance and insulation performance are reduced, and when the thickness is greater than 50μm, the forming performance is reduced.
[0035] External resin layer
[0036] In the aluminum bag film for secondary batteries of the present invention, the outer resin layer corresponds to the part in direct contact with the equipment, and therefore, it is preferred that the resin has insulating properties. Therefore, as the resin used as the outer resin layer, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, copolyester and polycarbonate may be included, or polyamide resin, polyimide resin or copolymer of polyamide and polyimide may be included. Preferably, copolymer of polyamide and polyimide may be included.
[0037] Specific examples of polyester resins may include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), copolyesters, polycarbonate (PC), etc. Specific examples of polyesters may include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, polycarbonate, copolyesters using ethylene terephthalate as a main body of a repeating unit, copolyesters using butylene terephthalate as a main body of a repeating unit, etc. In addition, specific examples of copolymer polyesters using ethylene terephthalate as the main body of repeating units may include: copolymer polyesters using ethylene terephthalate as the main body of repeating units polymerized with ethylene isophthalate, poly(ethylene terephthalate / ethylene isophthalate), poly(ethylene terephthalate / ethylene adipate), poly(ethylene terephthalate / sodium sulfoisophthalate), poly(ethylene terephthalate / sodium ethylene isophthalate), poly(ethylene terephthalate / ethylene phenyl dicarboxylate), poly(ethylene terephthalate / ethylene decanedicarboxylate), and the like. In addition, examples of the copolyester using butylene terephthalate as a main body of a repeating unit may include: a copolymer polyester using butylene terephthalate as a main body of a repeating unit polymerized with butylene isophthalate, poly(butylene terephthalate / adipate), poly(butylene terephthalate / sebacate), poly(butylene terephthalate / decanedicarboxylate), polybutylene naphthalate, etc. These polymers may be used alone as one type, or as a combination of two or more types.
[0038] Specific examples of the polyamide resin may include: aliphatic polyamides, such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; aromatic polyamides, such as hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides, such as nylon 6I, nylon 6T, nylon 6IT and nylon 6I6T (I represents isophthalic acid) containing structural units from terephthalic acid and / or isophthalic acid. , T represents terephthalic acid), and poly-m-xylene adipamide (MXD6); alicyclic polyamides such as polyaminomethylcyclohexyl adipamide (PACM6); or polyamides obtained by copolymerizing a lactam component and an isocyanate component such as 4,4'-diphenylmethane-diisocyanate; polyesteramide copolymers or polyetheresteramide copolymers, which are copolymers of copolymerized polyamide and polyester or polyalkylene ether glycol; copolymers thereof, etc. These polyamides may be used alone as one type or in combination of two or more types.
[0039] Nylon film is mainly used as packaging film by having excellent heat resistance, cold resistance and mechanical strength and having excellent breaking strength, anti-pinhole property, gas barrier property etc. The specific example of nylon film can include polyamide resin, that is, copolymer of nylon 6, nylon 66, nylon 6 and nylon 66, nylon 610, poly-m-xylene adipamide (MXD6) etc. When laminating external resin layer, the thickness of the laminated external resin layer is preferably 10 μm to 30 μm or more, and thickness is particularly preferably 12 μm to 25 μm. Not meeting the above range has the following problem, when thickness is less than 10 μm, external resin layer is easy to tear due to physical property reduction, and when thickness is greater than 30 μm, molding performance is reduced.
[0040] The above-mentioned external resin layer may preferably include a copolymer of polyamide and polyimide as a packaging film of a secondary battery.
[0041] Polyimide is classified as a general engineering plastic and has excellent heat resistance, insulation performance, flexibility and non-flammability, and its performance does not change in a wide temperature range from 273 degrees below zero to 400 degrees above zero. Due to these characteristics, polyimide is used as a material in various fields such as space suits, mobile phones, fuel cell housings, displays and military equipment. However, when polyimide is used alone in the outer resin layer, the bonding strength is reduced under the environment of high temperature, high salt, high humidity and ultraviolet rays, and polyurethane adhesives cannot prevent peeling or delamination. Therefore, in order to solve the problem of bonding strength of polyimide film, a copolymer of polyamide and polyimide can be included as the outer resin layer.
[0042] In the external resin layer, polyamide and polyimide can be copolymerized with a molar ratio of 1:9 to 9:1, preferably 3:7 to 9:1, more preferably 5:5 to 9:1, and more preferably 6:4 to 8:2. In addition, the external resin layer and the aluminum layer can be directly bonded, without an adhesive layer between the two layers. When polyimide is used alone as the external resin layer, the bonding strength is low, causing delamination under harsh environments such as high temperature, high salt and high humidity, but the copolymer of polyamide and polyimide can keep the bonding strength between the external resin layer and the aluminum layer without delamination without a separate adhesive, and has excellent heat resistance, chemical resistance, molding performance and salt resistance.
[0043] After a 5 cm×5 cm sample of the external resin layer is immersed in seawater at 85° C. with a salt concentration of 3.5% for 24 hours, the bonding strength between the external resin layer and the aluminum layer can be 2N / 15mm or more, preferably 3N / 15mm or more, and more preferably 5N / 15mm or more. Since the external resin layer has better salt resistance, the bonding strength between the external resin layer and the aluminum layer can be maintained without being reduced.
[0044] Internal resin layer
[0045] In the aluminum bag-shaped film for secondary batteries of the present invention, polyolefins such as polyethylene (PE) or polypropylene (PP), or their copolymers can be used as internal resin layers. The internal resin layer is not particularly limited thereto, and is formed by a resin layer selected from ethylene copolymers, propylene copolymers, polyesters, polyamides, polycarbonates, fluorines, silicones, acrylics, ethylene-propylene-diene-monomer rubber (EPDM) and mixtures thereof, in addition to polyolefins such as polyethylene, polypropylene and polybutene. Preferably, a polyolefin resin layer, or a composite resin layer of polybutadiene and polyolefin can be used.
[0046] Specific examples of the polyolefin used above may include polyethylene, such as low-density polyethylene, medium-density polyethylene, high-density polyethylene or linear low-density polyethylene; polypropylene, such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene) and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); terpolymers of ethylene-butene-propylene; etc. Among these polyolefins, polyethylene and polypropylene are preferably included.
[0047] It is preferred to use a polyolefin such as polyethylene or polypropylene or a copolymer thereof in the inner resin layer because the processing properties such as lamination are good and it has the properties required as a packaging material for a secondary battery such as good heat sealing properties, moisture resistance and heat resistance. Considering the molding properties, insulation properties, electrolyte resistance, etc., the thickness of the polymer layer of the inner resin layer is preferably 20 μm to 100 μm, more preferably 30 μm to 80 μm. Failure to meet the above range may cause problems such as reduced molding properties, insulation properties and electrolyte resistance.
[0048] Adhesive layer
[0049] The adhesive layer is a layer that increases the adhesion between the inner resin layer and the aluminum foil layer.
[0050] The adhesive layer may include one or more types of compounds selected from polyurethane resins, polyolefin resins, and epoxy resins, or a mixture of modified products thereof. Specific examples of the adhesive may include maleic anhydride polypropylene (MAHPP) and the like.
[0051] Examples of thermally adhesive olefin resins may include polyethylene, ethylene-α-olefin copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-acrylate copolymers, ethylene-methacrylate copolymers, ethylene-vinyl acetate copolymers, ionomers, polypropylene, maleic anhydride-modified polypropylene, ethylene-propylene copolymers, propylene-1-butene-ethylene copolymers, and the like, and may preferably include one or more types of olefin resins selected from polypropylene, ethylene-propylene copolymers, and propylene-1-butene-ethylene copolymers.
[0052] The polyolefin used to form the adhesive layer can be an acid-modified polyolefin. The acid-modified polyolefin used to form the second adhesive layer is a polymer modified by grafting polyolefin with unsaturated carboxylic acid. Specific examples of acid-modified polyolefins may include polyethylene, such as low-density polyethylene, medium-density polyethylene, high-density polyethylene or linear low-density polyethylene; crystalline or amorphous polypropylene, such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene) and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); terpolymers of ethylene-butene-propylene, etc. Among these polyolefins, it is preferred to include polyolefins having at least propylene as a forming monomer, and in terms of heat resistance, it is more preferred to include terpolymers of ethylene-butene-propylene and random copolymers of propylene-ethylene. Examples of unsaturated carboxylic acids used for modification may include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. Among these unsaturated carboxylic acids, it is preferred to include maleic acid and maleic anhydride. The acid-modified polyolefin may be used alone as one type or in combination of two or more types.
[0053] Considering the adhesion to the inner resin layer and the thickness after molding, the thickness of the adhesive layer is preferably 2 μm to 10 μm, more preferably 3 μm to 5 μm. Failure to meet the above range may cause the following problems: when the thickness is less than 2 μm, the adhesion is reduced, and when the thickness is greater than 5 μm, cracks may occur.
[0054] When the inner resin layer and the aluminum layer are laminated on the adhesive layer, the method is not particularly limited, however, dry lamination, heat lamination, or extrusion lamination may be preferably used for lamination.
[0055] Method for manufacturing aluminum bag film for secondary battery
[0056] The present invention provides a method for manufacturing an aluminum bag film for a secondary battery, the method comprising: a) preparing an aluminum layer; b) forming an outer resin layer on a first surface of the aluminum layer; and c) bonding an inner resin layer to a second surface of the aluminum layer, wherein the outer resin layer comprises a copolymer of polyamide and polyimide.
[0057] a) Preparation of aluminum layer
[0058] As the aluminum layer of the aluminum bag-shaped film for secondary batteries of the present invention, soft aluminum foil can be preferably used, and in order to further provide pinhole resistance and softness during cooling and forming, iron-containing aluminum foil can be more preferably used. In the iron-containing aluminum foil, the iron content relative to 100% by mass of the entire aluminum foil can be preferably 0.1% by mass to 9.0% by mass, more preferably 0.5% by mass to 2.0% by mass. When the iron content is less than 0.1% by mass relative to 100% by mass of the entire aluminum foil, the softness of the aluminum layer is reduced, and the inclusion of more than 9.0% by mass of iron has the problem of reduced forming performance.
[0059] The thickness of the aluminum layer is preferably 10 μm to 100 μm, more preferably 30 μm to 50 μm, in consideration of pinhole resistance, processing performance, oxygen and moisture barrier properties, etc. Failure to meet the above range may cause the following problems: when the thickness is less than 10 μm, the aluminum layer is easily torn and the electrolyte resistance and insulation performance are reduced; when the thickness is greater than 100 μm, the molding performance deteriorates.
[0060] As the aluminum foil used in the aluminum layer, an untreated aluminum foil may be used, however, a degreased aluminum foil is more preferably used in terms of providing electrolyte resistance, etc. As the degreasing treatment method, a wet treatment method or a dry treatment method may be included.
[0061] The example of wet degreasing can include acid degreasing or alkali degreasing. The example of the acid used in the acid degreasing can include mineral acid such as sulfuric acid, acetic acid, phosphoric acid and hydrofluoric acid, and the acid can be used alone as a type, or used in combination of two or more types. In addition, as required, various metal salts can be mixed therein to improve the etching effect of aluminum foil. The example of the alkali used in the alkali degreasing can include strong alkali such as sodium hydroxide, and weak base types or surfactants can also be mixed therein.
[0062] An example of dry degreasing treatment may include a degreasing method using an annealing process for aluminum at a high temperature.
[0063] b) forming an outer resin layer on the first surface of the aluminum layer
[0064] In the aluminum bag-shaped film for secondary batteries of the present invention, the outer resin layer corresponds to the part in direct contact with the equipment, and therefore, preferably a resin with insulating properties. Therefore, as a resin used as an outer resin layer, a polyester resin such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, copolyester and polycarbonate may be included, or a polyamide resin, a polyimide resin, or a copolymer of a polyamide resin and a polyimide resin may be included. Preferably, a copolymer of polyamide and polyimide may be included.
[0065] The above-mentioned external resin layer may preferably include a copolymer of polyamide and polyimide as a packaging film of the secondary battery.
[0066] Polyimide is classified as a general engineering plastic and has excellent heat resistance, insulation performance, flexibility and non-flammability, and its performance does not change in a wide temperature range from -273 degrees to 400 degrees. Due to these characteristics, polyimide is used as a material in various fields such as space suits, mobile phone fuel cell housings, displays and military equipment. However, when polyimide is used alone in the outer resin layer, the bonding strength is reduced under high temperature, high salt, high humidity and ultraviolet light, and polyurethane adhesives cannot prevent peeling or delamination. Therefore, in order to solve the problem of bonding strength of polyimide film, a copolymer of polyamide and polyimide can be included as the outer resin layer.
[0067] In the outer resin layer, polyamide and polyimide can be copolymerized with a molar ratio of 1:9 to 9:1, preferably 3:7 to 9:1, more preferably 5:5 to 9:1, and more preferably 6:4 to 8:2. In addition, the outer resin layer and the aluminum layer can be directly bonded, without an adhesive layer between the two layers. When polyimide is used alone as the outer resin layer, the bonding strength is low, causing delamination under harsh environments such as high temperature, high salt and high humidity, however, the copolymer of polyamide and polyimide can maintain the bonding strength between the outer resin layer and the aluminum layer without delamination without a separate adhesive, while having excellent heat resistance and chemical resistance.
[0068] When forming an external resin layer on the first surface of the aluminum layer of the aluminum bag-shaped film for a secondary battery of the present invention, a copolymer of polyamide and polyimide is laminated using a dry lamination method or an extrusion lamination method to form an external resin layer. When laminating the external resin layer, the thickness of the laminated external resin layer is preferably 10 μm to 30 μm or more, and the thickness is particularly preferably 12 μm to 25 μm. Not meeting the above range has the following problems, when the thickness is less than 10 μm, the external resin layer is easily torn due to reduced physical properties, and when the thickness is greater than 30 μm, the molding performance is reduced.
[0069] When the outer resin layer is laminated, although not particularly limited, the outer resin layer may be preferably laminated using a dry lamination method or an extrusion lamination method.
[0070] c) Bonding the inner resin layer to the second surface of the aluminum layer
[0071] When the inner resin layer is bonded to the second surface of the aluminum layer of the aluminum bag film for secondary batteries of the present invention, a compound of one or more types selected from polyurethane resins, polyolefin resins and epoxy resins, or a mixture of modified products thereof, may be included as an adhesive layer for bonding the aluminum layer to the inner resin layer. Specific examples of the adhesive may include maleic anhydride polypropylene (MAHPP) and the like.
[0072] Considering the adhesion to the inner resin layer and the thickness after molding, the thickness of the second adhesive layer is preferably 2 μm to 30 μm, more preferably 3 μm to 15 μm. Failure to meet the above range may cause the following problems: when the thickness is less than 2 μm, the adhesion is reduced, and when the thickness is greater than 30 μm, cracks may occur.
[0073] When the inner resin layer is laminated on the aluminum layer, although not particularly limited thereto, the inner resin layer may be preferably laminated using a dry lamination method or an extrusion lamination method.
[0074] Hereinafter, preferred examples are provided to illustrate the present invention, however, the following examples are provided only for easier understanding of the present invention, and the present invention is not limited thereto.
[0075] Example: Making a bag-shaped film
[0076] [Example 1 to Example 5]
[0077] In order to laminate the outer resin layer, polyamide-polyimide copolymer films (Vylomax, Toyobo Co., Ltd.) having a thickness of 25 μm and having different molar ratios as in Examples 1 to 5 of Table 1 below were first prepared.
[0078] Without a separate adhesive, a polyamide-polyimide copolymer film having a thickness of 25 μm was dry-laminated on the first surface of an aluminum foil having a thickness of 40 μm (a product of Dong-il Aluminum Co., Ltd.) and laminated as an outer resin layer. Thereafter, in order to laminate an inner resin layer on the second surface of the aluminum foil, a maleic anhydride-modified polyolefin adhesive (a product of HICHEM Co., Ltd.) was applied to a thickness of 4 μm, and a cast polypropylene having a thickness of 40 μm (a product of Lotte Chemical (formerly Homan Petrochemical)) was laminated on aluminum using a dry lamination method to prepare bag films of Examples 1 to 5.
[0079] [Table 1]
[0080] Copolymerization molar ratio (polyamide (PA): polyimide (PI)) Example 1 1:9 Example 2 3:7 Example 3 5:5 Example 4 7:3 Example 5 9:1 Comparative Example 10:0
[0081] [Comparative Example]
[0082] A polyurethane adhesive resin (product of HICHEM Co., Ltd.) having a thickness of 4 μm was coated on the first surface of an aluminum foil (product of Dong-il Aluminum Co., Ltd.) using a gravure roll coating method, and then a nylon 6 film (product of Hyosung) having a thickness of 25 μm was laminated as an outer resin layer by a dry lamination process, instead of a process in which a polyamide-polyimide copolymer film was laminated on aluminum as an outer resin layer without an adhesive.
[0083] Except for this, all processes were performed in the same manner under the same conditions as in Example 1 to Example 5 to produce a bag-shaped film of the comparative example.
[0084] Experimental example: Measurement of Young's modulus, and evaluation of adhesion, molding properties, and salt resistance
[0085] (Measurement of Young's modulus)
[0086] For the bag-shaped films produced in each of Examples 1 to 5 and Comparative Examples, Young's modulus was measured using a universal testing machine (Shimadzu AG-X), and the results are shown in Table 2 below.
[0087] [Table 2]
[0088] Young's modulus(GPa) Example 1 6.5 Example 2 6.2 Example 3 5.5 Example 4 5.0 Example 5 4.5 Comparative Example 4.2
[0089] It can be confirmed from the Young's modulus measurement results in Table 2 that, as the polymerization ratio of polyimide in the polyamide-polyimide copolymer increases, the copolymer becomes strong and difficult to compress, and the force required to deform the polymer increases.
[0090] (Adhesion Evaluation)
[0091] For the bag-shaped films manufactured in each of Examples 1 to 5 and Comparative Examples, the adhesion (N / 15 mm) between the polyamide-polyimide copolymer outer resin layer and the aluminum layer was measured using a UTM device (TESTONE Co., Ltd.) according to ASTM D882 to evaluate the adhesion, and the results are shown in Table 3 below.
[0092] [Table 3]
[0093] Adhesion strength (N / 15mm) Example 1 2 Example 2 2 Example 3 3 Example 4 5 Example 5 5.5 Comparative Example 6
[0094] (Evaluation of molding performance)
[0095] The bag-shaped films produced in each of Examples 1 to 5 and Comparative Examples were molded using a cold drawing punching method (die size: 5 cm×6 cm) while changing the molding depth by 0.1 mm, and crack generation was measured. The results are shown in Table 4 below.
[0096] The occurrence of cracks was confirmed by the generation of microcracks by flashing the molded product in a dark room and observing the leaked light using a microscope. Thus, the molding performance was evaluated by taking the molding depth when no cracks were generated as the limit molding depth.
[0097] [Table 4]
[0098] Limit forming depth (mm) Example 1 2.0 Example 2 3.0 Example 3 4.0 Example 4 6.0 Example 5 6.2 Comparative Example 6.5
[0099] (Salt tolerance evaluation)
[0100] The 5 cm×5 cm bag-shaped film samples manufactured in each of Examples 1 to 5 and Comparative Examples were immersed in seawater at 85° C. with a salt concentration of 3.5% (the composition ratio of the components is shown in Table 5) for 24 hours. After 24 hours, the bag-shaped film samples were taken out, and the adhesion strength (N / 15 mm) between the polyamide-polyimide copolymer outer resin layer and the aluminum layer was measured using a UTM device (TESTONE Co., Ltd.) according to ASTM D882 to evaluate the adhesion, and the results are shown in Table 6 below.
[0101] [Table 5]
[0102] Composition ratio of each component (mol / kg) <![CDATA[H 2 The]]> 53.6 <![CDATA[Na + ]]> 0.46 <![CDATA[Mg 2+ ]]> 0.053 <![CDATA[Ca 2+ ]]> 0.01 <![CDATA[K + ]]> 0.01
[0103] [Table 6]
[0104] Adhesion strength (N / 15mm) Example 1 2 Example 2 2 Example 3 3 Example 4 5 Example 5 2 Comparative Example 1
[0105] Through the evaluation of adhesion, molding properties and salt resistance according to Tables 3, 4 and 6, it can be determined that Example 4 in which the polymerization ratio of polyamide-polyimide is 7:3 can be used as an external resin layer in which adhesion is maintained even under harsh conditions of high temperature and high salt, while having excellent adhesion and molding properties.
[0106] Simple modifications and changes of the present invention all fall within the scope of the present invention, and the specific protection scope of the present invention will become apparent from the appended claims.
Claims
1. An aluminum bag film for a secondary battery, the aluminum bag film comprising: Aluminum layer; an outer resin layer formed on a first surface of the aluminum layer; an inner resin layer formed on the second surface of the aluminum layer; and an adhesive layer for bonding the aluminum layer to the inner resin layer, wherein the outer resin layer comprises a copolymer of polyamide and polyimide, Wherein, in the outer resin layer, polyamide and polyimide are copolymerized in a molar ratio of 1:9 to 9:1, Wherein, the outer resin layer is directly bonded to the aluminum layer without an adhesive layer between the two layers.
2. The aluminum bag film for a secondary battery according to claim 1, wherein After a 5 cm×5 cm sample of the outer resin layer was immersed in seawater having a salt concentration of 3.5% and a temperature of 85° C. for 24 hours, the adhesive strength between the outer resin layer and the aluminum layer was 2 N / 15 mm or more.
3. A method for manufacturing the aluminum bag film for a secondary battery according to claim 1, the method comprising: a) preparing an aluminum layer; b) forming an outer resin layer on the first surface of the aluminum layer; and c) bonding an inner resin layer to the second surface of the aluminum layer, Wherein, the outer resin layer comprises a copolymer of polyamide and polyimide.