Evaluation method of thermal aging status of cast main pipe based on single test temperature
By using a accelerated thermal aging method with a single test temperature in the main pipeline of a nuclear power plant, normalized energy parameters are calculated and relational equations are fitted, the accuracy of the evaluation of thermal aging status of cast stainless steel materials is solved, and scientific maintenance and life extension basis is provided. .
Patent Information
- Application Number
- CN202011560983.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-12-25
AI Technical Summary
After the existing cast stainless steel materials are thermally aged in high-temperature operating environment, the material becomes brittle and the tensile strength and toughness are reduced. The predicted values of the existing models are different and there is no data support, making it difficult to effectively evaluate the thermal aging status of the main pipeline of the nuclear power plant. .
Using accelerating thermal aging method based on a single test temperature, through cutting and processing test blocks, mechanical performance tests and Shabi pendulum impact tests, normalized energy parameters are calculated, relational equations are fitted, and materials are predicted at different temperatures and times. aging state.
A method is provided that can effectively evaluate the thermal aging status of stainless steel materials in casting main pipelines, overcomes the problems of insufficient data in the prior art and inconsistent models, improves prediction accuracy, and provides a scientific basis for component maintenance and life extension.
Smart Images

Figure CN114689489B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to a method for evaluating the thermal aging state of a material, and in particular relates to a method for evaluating the thermal aging state of a stainless steel material for a cast main pipeline of a nuclear power plant. Background Art
[0002] Cast stainless steel will experience thermal aging embrittlement after long-term service in the high temperature operating environment of 280-320℃ in the reactor, causing the stainless steel material to become brittle, the tensile strength of the stainless steel to increase, and the toughness, impact energy and fracture toughness to decrease. At present, there are at least four models for predicting the change of the toughness curve of cast stainless steel after thermal aging. One is a proprietary model for a specific component, and the other three are the American Argonne model, the French / EDF model and the Japanese model. The above four models are empirical relationships established based on the experimental data of the development stage of each model. For the change of the toughness value of different cast stainless steel materials, different prediction values will appear in the models established based on their respective databases. Moreover, with the increase of data and further in-depth analysis and mining, the model is also constantly improving and developing. Therefore, studying the thermal aging status evaluation method of stainless steel materials for cast main pipelines in nuclear power plants can prevent brittle failure of the main pipelines and provide a basis for component maintenance or replacement and license renewal application during life extension. Summary of the invention
[0003] The object of the present invention is to provide a method for evaluating the thermal aging state of stainless steel of a cast main pipeline based on a single test temperature, which can overcome the shortcomings of the prior art.
[0004] The technical solution of the present invention is as follows: A method for evaluating the thermal aging state of stainless steel in a cast main pipeline based on a single test temperature comprises the following steps:
[0005] Step A: cutting the selected cast main pipe to make a heat aging test block;
[0006] Step B: Select a test block for heat aging test in step A, and sample and process the mechanical properties test piece;
[0007] Step C: placing the remaining heat aging test pieces in step A into a high temperature box, and conducting accelerated heat aging tests at a single test temperature for different time periods;
[0008] Step D: Sampling and processing mechanical property specimens for the test blocks that have been subjected to accelerated thermal aging tests at a single test temperature for different time periods in step C;
[0009] Step E: performing Charpy pendulum impact tests on the mechanical property samples in steps B and D respectively;
[0010] Step F: Normalize the absorbed energy obtained from the Charpy pendulum impact test in step E, and calculate the thermal aging parameters at a single test temperature.
[0011] Step G, fitting the data to obtain the curve of the normalized energy parameter of the casting main pipeline material changing with the thermal aging parameter:
[0012] Step H: The aging state index (impact absorption energy) of the casting main pipeline material at different temperatures and different time points can be predicted according to the above normalized relationship equation.
[0013] The single test temperature in step D is 350°C.
[0014] In the step D, an accelerated heat aging test is performed at a single test temperature of 350° C. for different time periods of 0 h, 100 h, 500 h, 1000 h, 2000 h, 5000 h, 8000 h, and 10000 h.
[0015] In the step F,
[0016] Normalized energy parameter α i :
[0017] α i =C Vi / C V0 , where i = 1, 2, ..., n
[0018] Thermal aging parameters P i :
[0019]
[0020] where i = 1, 2, ..., n
[0021] Among them, Si, Cr, Mn, N, and C are element contents;
[0022] In the step F, for CF-3, CF-8 stainless steel I 1 =0,I 2 =1.
[0023] In the step F, for CF-8M stainless steel I 1 =1,I 2 =0, when the Mn content in the material is >1.2%, take 1.2%, the Q value range is 65 to 250 kJ / mole, when the Q value is less than 65 kJ / mole, take 65 kJ / mole, when the Q value is greater than 250 kJ / mole, take 250 kJ / mole.
[0024] In the step G,
[0025] The normalized fitting formula is:
[0026] log 10 α i =A+B[1-tanh(P i -C)]
[0027] Among them, A, B, C are the energy parameters α mentioned above i Thermal aging parameters P i The fitting constant of the variation curve.
[0028] The beneficial effects of the present invention are as follows: compared with those abroad, the current domestic thermal aging database and model of main pipelines are very short of data, and the model development lacks a large amount of data support. In addition, it is difficult to obtain a domestic material database and model development level of the same scale abroad in a short period of time. The present invention formally proposes an aging test based on a single temperature based on the above background, and at the same time draws on some foreign research results to evaluate the thermal aging status of cast main pipeline materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a flow chart;
[0030] Figure 2 This is the variation curve of normalized energy parameter with thermal aging parameter. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0032] The method for evaluating the thermal aging state of a cast main pipe based on a single test temperature includes the following steps:
[0033] Step A, cutting the selected cast main pipe to form a heat aging test block;
[0034] Step B, selecting a test block for heat aging test in step A, and sampling and processing a mechanical property test piece;
[0035] Step C, placing the remaining heat aging test pieces in step A into a high temperature box, and conducting accelerated heat aging tests at a single test temperature for different time periods;
[0036] Step D, sampling and processing mechanical property specimens of the test blocks subjected to accelerated thermal aging tests at a single test temperature for different time periods in step C;
[0037] Step E, performing Charpy pendulum impact tests on the mechanical property samples in steps B and D respectively;
[0038] Step F, normalizing the absorbed energy obtained from the Charpy pendulum impact test in step E, and calculating the thermal aging parameters at a single test temperature;
[0039] Step G, fitting the data to obtain the curve of the normalized energy parameter of the casting main pipeline material changing with the thermal aging parameter:
[0040] Step H: The aging state index (impact absorption energy) of the casting main pipeline material at different temperatures and different time points can be predicted according to the above normalized relationship equation.
[0041] Specifically, a method for evaluating the thermal aging state of a cast main pipeline based on a single test temperature comprises the following steps:
[0042] Step A, cutting the selected cast main pipe and processing it into test blocks for thermal aging test ( Figure 1 ), the reference size of the test block is length ≥100mm (recommended value), width ≥70mm, thickness is the original thickness of the selected main pipeline (such as 76mm), and the number is ≥8;
[0043] Step B, selecting a test block for heat aging test in step A, sampling and processing a mechanical property test piece (impact test piece: Charpy V-notch, 10 mm×10 mm×55 mm);
[0044] Step C, put the remaining heat aging test pieces in step A into a high temperature box (the highest operating temperature of the high temperature box is ≥400°C, the temperature fluctuation is ≤2°C, and the temperature uniformity is ≤8°C), and test them at a single test temperature T (such as T=350°C) with a maximum temperature not higher than 400°C for different time periods t i (such as t 1 =100h, t 2 =500h, t 3 =1000h, t 4 =2000h, t 5 =5000h, t 6 =8000h, t 7 =10000h,…,t n Accelerated thermal aging test at n time points in total, where i = 1, 2, ..., n);
[0045] Step D, the test samples in step C are subjected to different time periods t at a single test temperature T (e.g., T = 350°C). i (such as t 1 =100h, t 2 =500h, t 3 =1000h, t 4 =2000h, t 5 =5000h, t6 =8000h, t 7 =10000h,…, t n A total of n time points, where i = 1, 2, ..., n) were used for the test blocks of the accelerated thermal aging test, and mechanical properties specimens (impact specimens: Charpy V-notch, 10 mm × 10 mm × 55 mm) were sampled and processed;
[0046] Step E: Perform Charpy pendulum impact tests on the mechanical property samples (impact samples) in steps B and D, respectively. Place the impact sample between two supports of the pendulum impact tester with the notch facing away from the impact surface. Use the pendulum to strike the impact sample once, and measure the absorbed energy of the impact sample. The absorbed energy of the impact sample obtained in step B is recorded as C. V0 The absorbed energy obtained by impacting the sample in step D is recorded as C Vi , where i = 1, 2, 3, ..., n;
[0047] Step F, normalizing the absorbed energy obtained from the Charpy pendulum impact test in step E to obtain a normalized energy parameter α i , and calculate the thermal aging parameter P at a single test temperature T i , the normalized energy parameter α i and thermal aging parameters P i The calculation formula is as follows:
[0048] Normalized energy parameter α i :
[0049] α i =C Vi / C V0 , where i = 1, 2, ..., n
[0050] Thermal aging parameters P i :
[0051]
[0052] where i = 1, 2, ..., n
[0053] Among them, Si, Cr, Mn, N, and C are element contents; for CF-3 and CF-8 stainless steels, 1 =0,I 2 =1; for CF-8M stainless steel I 1 =1,I 2=0. When the Mn content in the material is >1.2%, take 1.2%. The Q value range is 65 to 250 kJ / mole. When the Q value is less than 65 kJ / mole, take 65 kJ / mole. When the Q value is greater than 250 kJ / mole, take 250 kJ / mole. When the heat aging temperature T is between 280-400°C, the θ value is 2.9.
[0054] Step G, using the thermal aging parameter P in step F i is the horizontal axis, the normalized energy parameter α i As the ordinate, the normalized energy parameter α of the casting main pipe material is obtained by fitting the data. i Thermal aging parameters P i The change curve of , the normalized relationship equation is:
[0055] log 10 α i =A+B[1-tanh(P i -C)]
[0056] Where A, B, C are the energy parameters α mentioned above i Thermal aging parameters P i The fitting constant of the variation curve.
[0057] Step H: The aging state index (impact absorption energy) of the casting main pipeline material at different temperatures T and different time points t can be predicted according to the above normalized relationship equation.
Claims
1. A method for evaluating the thermal aging state of a cast main pipeline based on a single test temperature, characterized in that: The steps include: Step A: cutting the selected cast main pipe to make a heat aging test block; Step B: Select a test block for heat aging test in step A, and sample and process the mechanical properties test piece; Step C: placing the remaining heat aging test pieces in step A into a high temperature box, and conducting accelerated heat aging tests at a single test temperature for different time periods; Step D: Sampling and processing mechanical property specimens for the test blocks that have been subjected to accelerated thermal aging tests at a single test temperature for different time periods in step C; Step E: performing Charpy pendulum impact tests on the mechanical property samples in steps B and D respectively; Step F: normalizing the absorbed energy obtained from the Charpy pendulum impact test in step E, and calculating the thermal aging parameters at a single test temperature; Step G, fitting the data to obtain the curve of the normalized energy parameter of the casting main pipeline material changing with the thermal aging parameter: Step H: The aging status index of the casting main pipeline material at different temperatures and time points can be predicted according to the above normalized relationship equation.
2. The method for evaluating the thermal aging state of a casting main pipeline based on a single test temperature according to claim 1, characterized in that: The single test temperature in step C described above.
3. The method for evaluating the thermal aging state of a casting main pipeline based on a single test temperature according to claim 1, characterized in that: In step C, an accelerated heat aging test is performed at a single test temperature for different time periods.
4. The method for evaluating the thermal aging state of a casting main pipeline based on a single test temperature according to claim 1, characterized in that: In the step F, the absorbed energy obtained from the Charpy pendulum impact test is normalized, and the thermal aging parameters at a single test temperature are calculated.
5. The method for evaluating the thermal aging state of stainless steel of a cast main pipeline based on a single test temperature as claimed in claim 4, characterized in that: The data were fitted to obtain the variation curve of the normalized energy parameters of the casting main pipe material with the thermal aging parameters.
6. The method for evaluating the thermal aging state of stainless steel of a cast main pipeline based on a single test temperature according to claim 1, characterized in that: The single test temperature in step D is 350°C.
7. The method for evaluating the thermal aging state of stainless steel in a cast main pipeline based on a single test temperature according to claim 1, characterized in that: In the step D, an accelerated heat aging test is carried out at a single test temperature of 350°C for different time periods of 0h, 100h, 500h, 1000h, 2000h, 5000h, 8000h, and 10000h.