A method for preparing a thin layer of carbon-based material and its use as a battery material

By using a combination of melamine, asphalt and ammonium chloride to prepare ultra-thin wrinkled carbon-based materials, the volume expansion effect and conductivity problems of carbon-based materials in potassium-ion batteries are solved, and efficient battery material performance improvements are achieved.

CN114715875BActive Publication Date: 2024-10-01JINMA ENERGY TECH (HUAINAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210353650.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-10-01
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

Carbon-based materials have volume expansion effects, conductivity and safety issues in potassium-ion battery applications, which limit their application prospects.

Method used

Using melamine, asphalt and ammonium chloride as the main raw materials, the N,N-dimethylformamide solvent was evaporated to dryness in a 90°C water bath and then sintering and annealed at 1100°C under argon protection to prepare an ultra-thin wrinkled graphene layer. Like carbon-based materials, the thickness and wrinkle degree of the material are controlled to suppress the volume expansion effect.

Benefits of technology

At a current density of 1000mA g-1, the prepared thin-layer carbon-based material has a specific discharge capacity of more than 147.6mAh g-1 after 1800 charge and discharge cycles, and a Coulombic efficiency of more than 99.6%, which significantly improves the performance of the battery material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003576044770000011
    Figure HDA0003576044770000011
  • Figure HDA0003576044770000012
    Figure HDA0003576044770000012
  • Figure HDA0003576044770000021
    Figure HDA0003576044770000021
Patent Text Reader

Abstract

The present application provides a method for preparing a thin layer of carbon-based materials and their use as negative electrode materials for potassium ion batteries. In the present invention, a certain amount of melamine and ammonium chloride are fully ground and dispersed in a certain volume of N, N-dimethylformamide, an appropriate amount of asphalt is added, and magnetic stirring is performed to obtain a yellowish-brown mixed solution, and then N, N-dimethylformamide is evaporated in a water bath, and asphalt-coated melamine and ammonium chloride powders are obtained by grinding; the obtained powder is transferred to a corundum crucible, and then transferred to a tubular furnace for sintering, annealing and carbonization under argon protection, and naturally cooled to room temperature to obtain a black ultra-thin wrinkled thin layer of carbon-based material. Electrochemical experiments have shown that the carbon-based material prepared by the present invention has application prospects as a negative electrode material for potassium ion batteries. The preparation process of the material of the present invention is simple, easy to operate, low in raw material cost, low in equipment investment, and suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of material chemical energy technology, and in particular to a method for preparing a thin-layer carbon-based material and its use as a battery material. Background Art

[0002] Among the numerous negative electrode materials, carbon-based materials have always attracted much attention in the application of alkaline ion batteries. The main advantages of carbon-based materials are their large abundance, adjustable interlayer spacing and structural characteristics. However, volume expansion effect, conductivity, safety, etc. have always been the fatal shortcomings of carbon-based materials in potassium ion battery applications. Therefore, the traditional modification methods of carbon-based materials include: 1. Carbon-carbon atomic structure regulation (Advanced Materials, 2018, 30 (48): 1802104); 2. Carbon micro-nanostructure regulation (Advanced Energy Materials, 2020: 2000808); 3. Heterojunction coupling regulation, etc. (ACS Energy Letters, 2020). It has been proved that carbon and its allotropes are a class of materials with great application value, especially the application of graphitized carbon materials in lithium-ion batteries is hailed as one of the most important inventions since the 20th century. However, the production process of graphene is complicated and expensive. Current research shows that the morphology of the product can be controlled by solid-phase reaction and with the help of the material's own composition structure, and the thickness and wrinkle degree of the material can be regulated by controlling the mass ratio of the material precursor to the product material precursor. The ultra-thin graphene-like layered structure can inhibit the volume expansion effect caused by the potassium ion insertion and extraction process of the material, while also increasing the contact area between the electrode material and the electrolyte and shortening the migration distance of the electrolyte. These characteristics make it have great application prospects in battery materials. Summary of the invention

[0003] In view of this, the purpose of the present application is to propose a method for preparing a thin layer of carbon-based material and its use as a battery material.

[0004] Based on the above purpose, the first aspect of the present application provides a method for preparing a thin layer of carbon-based material, using melamine and asphalt as main raw materials, adding an appropriate amount of ammonium chloride (NH 4 Cl) as a regulator, N,N-dimethylformamide (DMF) as a solvent, evaporated to dryness in a 90°C water bath, and then sintered, annealed and carbonized at 1100°C to obtain a thin layer of carbon-based material, which specifically includes the following steps:

[0005] 1) Weigh a certain amount of melamine (C 3 H 6 N 6 ) and ammonium chloride (NH 4C1) grind for 1 h to make it fully mixed, then disperse it into DMF solution and stir for 30 min to obtain a milky white mixed solution;

[0006] 2) Weigh a certain amount of asphalt and add it to the above mixture, stir it magnetically for 6 hours, then evaporate the DMF in a 90°C water bath, and then grind to obtain asphalt-coated melamine and ammonium chloride powder;

[0007] 3) placing the obtained powder into a corundum crucible, and then transferring it into a tube furnace for programmed temperature controlled sintering, annealing and carbonization under argon protection, and naturally cooling it to room temperature to obtain a black ultra-thin wrinkled thin layer carbon-based material, namely the thin layer carbon-based material.

[0008] Furthermore, the mass ratio of substances in the powder material is melamine: ammonium chloride = 4:1, and melamine+ammonium chloride: asphalt = 10-50:1.

[0009] Furthermore, the melamine and ammonium chloride substances are both chemically pure.

[0010] Furthermore, the asphalt is petroleum asphalt purchased on the market.

[0011] Based on the same inventive concept, the second aspect of the present application provides a thin layer of carbon-based material prepared using the preparation method described in the first aspect above.

[0012] Based on the same inventive concept, the third aspect of the present application provides a use of a thin layer of carbon-based material as a negative electrode material for a potassium ion battery. The material is used as a negative electrode material for a potassium ion battery. -1 At a current density of 1.5 2000, the discharge capacity remained at 147.6 mAh g after 1800 charge and discharge cycles. -1 The coulombic efficiency is above 99.6%.

[0013] From the above, it can be seen that the preparation method of the thin-layer carbon-based material provided by the present application and its use as a battery material, the specific combination of melamine, asphalt, ammonium chloride and DMF used in the present invention and the preparation process parameters play a key role in the morphology and composition structure of the prepared thin-layer carbon-based material, so that the prepared material has a unique Raman absorption spectrum, and the prepared thin-layer carbon-based material has specific electrochemical parameters. The specific surface area of ​​the prepared thin-layer carbon-based material is 141.23m 2 g -1 The morphology of the material is ultra-thin wrinkled graphene sheets. The prepared thin-layer carbon-based material has a high conductivity at 1000 mA g -1 At a current density of 1.5 2000, the discharge capacity remained at 147.6 mAh g after 1800 charge and discharge cycles. -1 The coulombic efficiency is above 99.6%. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions in the present application or related technologies, the drawings required for use in the embodiments or related technical descriptions are briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0015] Figure 1 N is a thin layer of carbon-based material prepared in the embodiment of the present application. 2 Adsorption-desorption curve diagram;

[0016] Figure 2 This is a SEM image of a thin layer of carbon-based material prepared in an embodiment of the present application;

[0017] Figure 3 TEM image of a thin layer of carbon-based material prepared in an embodiment of the present application;

[0018] Figure 4 Another TEM image of a thin layer of carbon-based material prepared in an embodiment of the present application;

[0019] Figure 5 XRD diagram of the thin-layer carbon-based material prepared in the embodiment of the present application;

[0020] Figure 6 Raman spectrum of the thin layer carbon-based material prepared in the embodiment of the present application;

[0021] Figure 7 Schematic diagram of the charge and discharge cycle performance of the thin layer carbon-based material prepared in the embodiment of the present application as the negative electrode of a potassium ion battery. DETAILED DESCRIPTION

[0022] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0023] It should be noted that, unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0024] Example 1

[0025] Weigh melamine (8.0 g) and ammonium chloride (2.0 g) and grind for 1 h to fully mix them, then disperse them in 100 mL of N,N-dimethylformamide and stir for 30 min to obtain a milky white mixed solution; weigh asphalt (1.0 g) and add it to the above mixed solution, stir it magnetically for 6 h, then evaporate N,N-dimethylformamide in a 90°C water bath, grind to obtain asphalt-coated melamine and ammonium chloride powders; transfer the obtained powders to a corundum crucible, and then transfer them to a tubular furnace and heat them at 2°C min under argon protection. -1 Heat to 600℃ and keep warm for 2h, then at 4℃min -1 Heat to 800℃ and keep for 2h, then at 5℃min -1 The temperature is raised to 1100°C and kept for 3 hours for annealing and carbonization, and then naturally cooled to room temperature to obtain a black ultra-thin wrinkled carbon-based material.

[0026] Example 2

[0027] Weigh melamine (16.0 g) and ammonium chloride (4.0 g) and grind for 1 h to fully mix them, then disperse them in 200 mL of N,N-dimethylformamide and stir for 30 min to obtain a milky white mixed solution; weigh asphalt (1.0 g) and add it to the above mixed solution, stir it magnetically for 6 h, then evaporate N,N-dimethylformamide in a 90°C water bath, grind to obtain asphalt-coated melamine and ammonium chloride powders; transfer the obtained powders to a corundum crucible, and then transfer them to a tubular furnace and precipitate them at 2°C min under argon protection. -1 Heat to 600℃ and keep warm for 2h, then at 4℃min -1 Heat to 800℃ and keep for 2h, then at 5℃min -1 The temperature was raised to 1100°C and kept for 3 hours for annealing and carbonization, and then naturally cooled to room temperature to obtain a black ultra-thin wrinkled carbon-based material.

[0028] Example 3

[0029] Weigh melamine (24.0 g) and ammonium chloride (6.0 g) and grind for 1 h to fully mix them, then disperse them in 300 ml N, N-dimethylformamide and stir for 30 min to obtain a milky white mixed solution; weigh asphalt (1.0 g) and add it to the above mixed solution, stir magnetically for 6 h, then evaporate N, N-dimethylformamide in a 90°C water bath, grind to obtain asphalt-coated melamine and ammonium chloride powders; transfer the obtained powders to a corundum crucible, and then transfer them to a tubular furnace and precipitate them at 2°C min under argon protection. -1 Heat to 600℃ and keep warm for 2h, then at 4℃min -1 Heat to 800℃ and keep for 2h, then at 5℃min -1The temperature was raised to 1100°C and kept for 3 hours for annealing and carbonization, and then naturally cooled to room temperature to obtain a black ultra-thin wrinkled carbon-based material.

[0030] Example 4

[0031] Weigh melamine (32.0 g) and ammonium chloride (8.0 g) and grind them for 1 h to fully mix them, then disperse them in 300 ml N, N-dimethylformamide and stir for 30 min to obtain a milky white mixed solution; weigh asphalt (1.0 g) and add it to the above mixed solution, stir it magnetically for 6 h, then evaporate N, N-dimethylformamide in a 90°C water bath, grind to obtain asphalt-coated melamine and ammonium chloride powders; transfer the obtained powders to a corundum crucible, and then transfer them to a tubular furnace and condense them at 2°C min under argon protection. -1 Heat to 600℃ and keep warm for 2h, then at 4℃min -1 Heat to 800℃ and keep for 2h, then at 5℃min -1 The temperature is raised to 1100°C and kept for 3 hours for annealing and carbonization, and then naturally cooled to room temperature to obtain an ultra-black, thin-layer carbon-based material with thin wrinkles.

[0032] Example 5

[0033] Weigh melamine (40.0 g) and ammonium chloride (10.0 g) and grind for 1 h to fully mix them, then disperse them in 300 ml N, N-dimethylformamide and stir for 30 min to obtain a milky white mixed solution; weigh asphalt (1.0 g) and add it to the above mixed solution, stir magnetically for 6 h, then evaporate N, N-dimethylformamide in a 90°C water bath, grind to obtain asphalt-coated melamine and ammonium chloride powders; transfer the obtained powders to a corundum crucible, and then transfer them to a tubular furnace and condense them at 2°C min under argon protection. -1 Heat to 600℃ and keep warm for 2h, then at 4℃min -1 Heat to 800℃ and keep for 2h, then at 5℃min -1 The temperature was raised to 1100°C and kept for 3 hours for annealing and carbonization, and then naturally cooled to room temperature to obtain a black ultra-thin wrinkled carbon-based material.

[0034] The following are the appearance and electrochemical performance parameter tests of the materials:

[0035] The thin-layer carbon-based materials prepared in Examples 1-5 were tested for their specific surface area and pore structure using a specific surface adsorption instrument ( Figure 1 ); scanning electron microscopy (SEM, Figure 2 ) and transmission electron microscopy (TEM, Figure 3 and Figure 4) observed the morphology of the material, and the results showed that the material presented an ultra-thin wrinkled graphene sheet structure with a sheet thickness of about 60nm; the composition structure of the material tested by a powder X-ray diffraction (XRD) instrument showed a strong absorption peak at 25.63 degrees ( Figure 5 ); Raman spectroscopy test shows that at 1350cm -1 and 1585cm -1 There are two strong absorption peaks ( Figure 6 );

[0036] The prepared thin-layer carbon-based material was used as the negative electrode material for potassium ion battery to carry out electrochemical performance test. The electrochemical performance test showed that the -1 At a current density of 1.5 2000, the discharge capacity remained at 147.6 mAh g after 1800 charge and discharge cycles. -1 Above, the Coulomb efficiency is above 99.6% ( Figure 7 ).

[0037] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present disclosure (including the claims) is limited to these examples. Based on the concept of the present disclosure, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the embodiments of the present disclosure as described above, which are not provided in detail for the sake of simplicity.

[0038] The embodiments of the present disclosure are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present disclosure should be included in the scope of protection of the present disclosure.

Claims

1. A method for preparing a thin layer of carbon-based material, characterized in that: include: 1) Weigh a certain amount of melamine and ammonium chloride, grind for 1 hour to fully mix them, then disperse them into a certain volume of N,N-dimethylformamide solution, stir for 30 minutes to obtain a milky white mixed solution; 2) Weigh a certain amount of asphalt and add it to the mixed solution, stir it magnetically for 6 hours, then evaporate N,N-dimethylformamide in a 90°C water bath, and then grind to obtain powders of melamine and ammonium chloride coated with asphalt; 3) The obtained powder was placed in a corundum crucible and then transferred to a tube furnace under argon protection at 2°C min -1 Heat to 600℃ and keep warm for 2h, then at 4℃min -1 Heat to 800℃ and keep for 2h, then at 5℃min -1 Heating to 1100° C. and keeping the temperature for 3 hours for annealing and carbonization, and naturally cooling to room temperature to obtain a black ultra-thin wrinkled thin-layer carbon-based material, namely the thin-layer carbon-based material; The mass ratio of each substance in the powder is melamine: ammonium chloride = 4:1, melamine + ammonium chloride: asphalt = 10-50:1; The melamine and ammonium chloride are both chemically pure; The asphalt is petroleum asphalt purchased on the market.

2. A thin layer of carbon-based material, characterized in that: The preparation method according to claim 1 is used for preparation.

3. A use of a thin layer of carbon-based material, characterized in that: The thin-layer carbon-based material prepared in claim 1 is used as the negative electrode material of a potassium ion battery at 1000 mAg -1 At a current density of 1.5 2000, the discharge capacity remained at 147.6 mAh g after 1800 charge and discharge cycles. -1 The coulombic efficiency is above 99.6%.