Polymer electrolyte membrane, membrane-electrode assembly including the same, and method for measuring durability thereof

By adopting a porous carrier and ionomer composite layer structure in the polymer electrolyte membrane, the mechanical properties and durability of the membrane are improved, and a testing method without manufacturing the actual membrane-electrode assembly is proposed to solve the polymerization problems in the existing technology. The problem of insufficient mechanical durability of bioelectrolyte membranes under high cycle times has significantly reduced the cost and time of fuel cell research and development.

CN114730901BActive Publication Date: 2024-10-15KOLON INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080079510.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-26
Filing Date
2020-12-23
Publication Date
2024-10-15
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Existing polymer electrolyte membranes have insufficient mechanical durability under high cycle times, and existing testing methods are time-consuming and costly, making it difficult to effectively evaluate the long-term operating performance of membrane-electrode assemblies.

Method used

A polymer electrolyte membrane with a composite layer structure of porous carrier and ionomer is used to improve the tear strength and puncture resistance of the membrane by adjusting the thickness of the porous carrier and ionomer distribution, and proposes a method that does not require the manufacture of actual membrane-electrodes A measurement method used to evaluate the durability of a component.

Benefits of technology

Achieving high durability of the polymer electrolyte membrane over 30,000 wet/dry cycles and significantly reducing the time and cost of fuel cell research and development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114730901B_ABST
    Figure CN114730901B_ABST
Patent Text Reader

Abstract

The present disclosure relates to: a polymer electrolyte membrane that can ensure the manufacture of a membrane-electrode assembly with excellent mechanical properties without deteriorating properties such as ionic conductivity, and thus the membrane-electrode assembly has a sufficiently high durability to achieve at least 30,000 wet / dry cycles measured according to the NEDO scheme; a membrane-electrode assembly including the polymer electrolyte membrane; and a method for measuring the durability of the membrane-electrode assembly. The polymer electrolyte membrane according to the present invention includes a composite layer, the composite layer including: a porous support having a plurality of pores; and an ionomer filling the pores, and the polymer electrolyte membrane has an MD internal tear strength of 150N / mm or more, a TD internal tear strength of 150N / mm or more, a puncture initial strain of 8% or less, and a puncture final strain of 10% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a polymer electrolyte membrane, a membrane-electrode assembly including the polymer electrolyte membrane, and a method for measuring the durability of the polymer electrolyte membrane, and more specifically to a polymer electrolyte membrane having excellent mechanical properties without deterioration in properties such as ionic conductivity, thereby ensuring the manufacture of a membrane-electrode assembly with high durability of more than 30,000 wet / dry cycles measured according to the NEDO scheme; a membrane-electrode assembly including the polymer electrolyte membrane; and a method for measuring the durability of the polymer electrolyte membrane. Background Art

[0002] A fuel cell is a battery that includes a power generation system that directly converts chemical reaction energy into electrical energy through an oxidation / reduction reaction of hydrogen and oxygen contained in hydrocarbon fuel materials such as methanol, ethanol or natural gas. Due to its environmentally friendly characteristics such as high energy efficiency and low pollutant emissions, it has attracted attention as a next-generation clean energy that can replace fossil energy.

[0003] The advantage of this fuel cell is that the unit cells are stacked to form a stack, thereby providing various levels of power. In addition, the energy density of the fuel cell is 4 to 10 times that of a small lithium battery, so the fuel cell is attracting attention as a small power source or mobile power source.

[0004] The stack of fuel cells that actually generate electricity has a structure in which several to dozens of unit cells are stacked, each unit cell includes a membrane-electrode assembly (MEA) and a diaphragm (also called a bipolar plate), and the membrane-electrode assembly is generally constructed to have a structure in which an anode and a cathode are formed on opposite sides of an electrolyte membrane in a state in which the electrolyte membrane is arranged between an anode (also called a "fuel electrode") and a cathode (also called an "air electrode").

[0005] Fuel cells can be classified into alkaline electrolyte membrane fuel cells or polymer electrolyte membrane fuel cells (PEMFC) according to the state and type of electrolyte. Polymer electrolyte membrane fuel cells have attracted attention as mobile power sources, vehicle power sources, and household power sources due to their low operating temperature of less than 100°C, fast startup and response characteristics, and excellent durability.

[0006] Typical examples of polymer electrolyte membrane fuel cells may include a proton exchange membrane fuel cell (PEMFC) using hydrogen as fuel and a direct methanol fuel cell (DMFC) using liquid methanol as fuel.

[0007] The reactions occurring in a polymer electrolyte membrane fuel cell will be briefly described. First, when a fuel such as hydrogen is supplied to the anode, hydrogen ions (H 2 O ) are generated at the anode due to an oxidation reaction of the hydrogen. +) and electron (e - ). The generated hydrogen ions are transferred to the cathode through the polymer electrolyte membrane, and the generated electrons are transferred to the cathode through an external circuit. At the cathode supplied with oxygen, oxygen combines with the hydrogen ions and the electrons, and water is generated due to the reduction reaction of the oxygen.

[0008] At the same time, in order to realize the commercial use of polymer electrolyte membrane fuel cells, there are many technical problems that need to be overcome, and it is essentially necessary to achieve high performance, long life and cost reduction of polymer electrolyte membrane fuel cells. The element that has the greatest impact on it is the membrane-electrode assembly, and the polymer electrolyte membrane is one of the core factors that have the greatest impact on the performance and cost of the membrane-electrode assembly.

[0009] In particular, for membrane-electrode assemblies used in transportation fuel cells, it is most important to ensure the mechanical durability of the membrane-electrode assembly for long-term operation. Generally, the mechanical durability of the membrane-electrode assembly mainly depends on the durability of the polymer electrolyte membrane that repeatedly expands and contracts during the driving process of the fuel cell.

[0010] In order to improve the mechanical durability of the polymer electrolyte membrane, a reinforced composite membrane type polymer electrolyte membrane manufactured by impregnating a porous support with an ionomer dispersion has been proposed. However, as the thickness of the porous support increases, the electrical properties of the polymer electrolyte membrane, such as ionic conductivity, decrease. For this reason, the thickness of the porous support cannot be increased indefinitely, and therefore, there is a limit to improving the mechanical durability of the polymer electrolyte membrane by adjusting the thickness of the porous support.

[0011] Meanwhile, the mechanical durability of the membrane-electrode assembly is usually evaluated by measuring the number of wet / dry cycles according to the NEDO scheme. However, there is a problem that this evaluation takes a long time (more than 50 days). In addition, in order to evaluate the durability of the membrane-electrode assembly, the membrane-electrode assembly sample must be actually manufactured, so (i) it also takes a lot of time to manufacture the membrane-electrode assembly sample for durability evaluation, and (ii) since precious metals are used to form electrodes, the cost of manufacturing the membrane-electrode assembly sample is too high. Summary of the invention

[0012] Technical issues

[0013] An object of the present disclosure is to provide a polymer electrolyte membrane having excellent mechanical properties without deterioration in properties such as ion conductivity, thereby ensuring the manufacture of a membrane-electrode assembly having high durability of more than 30,000 wet / dry cycles measured according to the NEDO scheme.

[0014] Another object of the present disclosure is to provide a membrane-electrode assembly including a polymer electrolyte membrane having excellent mechanical properties without deteriorating properties such as ion conductivity, so that the membrane-electrode assembly has high durability of more than 30,000 wet / dry cycles measured according to the NEDO scheme.

[0015] Another object of the present disclosure is to provide a method for measuring the durability of a polymer electrolyte membrane, which is capable of checking the mechanical durability of the polymer electrolyte membrane without actually manufacturing the membrane-electrode assembly, thereby significantly reducing the time and cost required for the research and development of the membrane-electrode assembly and the fuel cell.

[0016] Technical Solution

[0017] According to one aspect of the present disclosure, a polymer electrolyte membrane is provided, comprising a composite layer, the composite layer comprising: a porous support having a plurality of pores; and an ionomer filling the pores, wherein the polymer electrolyte membrane has an MD tear strength of greater than 150 N / mm, a TD tear strength of greater than 150 N / mm, a stab initial strain of less than 8%, and a stab final strain of less than 10%.

[0018] The polymer electrolyte membrane may have an in-plane ionic conductivity of 0.03 S / cm to 0.1 S / cm and a through-plane ionic conductivity of 0.03 S / cm to 0.1 S / cm under conditions of 80° C. and 50% RH.

[0019] The polymer electrolyte membrane may have an MD tear strength of 170 N / mm to 320 N / mm, a TD tear strength of 160 N / mm to 320 N / mm, a puncture initial strain of 1% to 6%, and a puncture final strain of 2% to 8%.

[0020] The composite layer may have a first surface and a second surface opposite to the first surface, and the polymer electrolyte membrane may also include: a first resin layer arranged on the first surface, the first resin layer containing a first ionomer; and a second resin layer arranged on the second surface, the second resin layer containing a second ionomer, and at least a portion of the ionomers in the composite layer may be the same ionomer as at least one of the first ionomer and the second ionomer.

[0021] The thickness of the polymer electrolyte membrane may be 10 μm to 50 μm, and the thickness of the composite layer may be 30% to 90% of the thickness of the polymer electrolyte membrane.

[0022] The porous support may include a first porous sub-support having a first surface and a second porous sub-support having a second surface, the first porous sub-support may have first pores filled with an ionomer identical to the first ionomer, the second porous sub-support may have second pores, portions of the second pores adjacent to the first porous sub-support are filled with an ionomer identical to the first ionomer, and the remaining portions of the second pores adjacent to the second resin layer are filled with an ionomer identical to the second ionomer.

[0023] The first porous sub-support and the second porous sub-support may be in contact with each other.

[0024] The porous carrier may include: a first porous sub-carrier having a first surface; a second porous sub-carrier having a second surface; and at least one third porous sub-carrier disposed between the first porous sub-carrier and the second porous sub-carrier, and the first porous sub-carrier, the second porous sub-carrier and the third porous sub-carrier may be in contact with each other.

[0025] The first ionomer may be the same as or different from the second ionomer.

[0026] According to another aspect of the present disclosure, there is provided a membrane-electrode assembly including: an anode, a cathode, and the polymer electrolyte membrane according to claim 1, the polymer electrolyte membrane being disposed between the anode and the cathode.

[0027] According to another aspect of the present disclosure, a method for measuring the durability of a polymer electrolyte membrane is provided, the method comprising: taking a sample having a predetermined size and shape from the polymer electrolyte membrane, fixing the sample to a bracket for a breakdown test according to ASTM F1342, repeatedly puncturing the sample at a predetermined load and a predetermined speed using a probe for a breakdown test according to ASTM F1342, measuring the displacement of the sample after each puncture, and calculating the puncture strain using at least one of the measured displacements.

[0028] Calculating the puncture strain may include: calculating the puncture initial strain according to the following equation 1 and calculating the puncture final strain according to the following equation 2:

[0029] [Equation 1]: IS (%) = [(D2-D1) / D1] x 100

[0030] [Equation 2]: FS (%) = [(D 20 -D1) / D1]×100

[0031] Where IS represents the initial strain of puncture, FS represents the final strain of puncture, D1 represents the displacement caused by the first puncture (mm), D2 represents the displacement caused by the second puncture (mm), and D 20 represents the displacement (mm) caused by the twentieth puncture.

[0032] The sample may have a square shape of 50 mm×50 mm, the predetermined load may be 10 N, and the predetermined speed may be 100 mm / min.

[0033] The method may be performed at a temperature of 23±2° C. and a relative humidity of 50±5%.

[0034] The initial load applied to the sample may be 0.2N.

[0035] Beneficial Effects

[0036] According to the present disclosure, a polymer electrolyte membrane having improved impregnation performance of ionomer in a porous support can be provided. Therefore, the polymer electrolyte membrane according to the present disclosure not only has excellent electrical properties such as ionic conductivity, but also has high tear strength and puncture resistance, thereby showing improved mechanical durability.

[0037] Specifically, the polymer electrolyte membrane according to the present disclosure has a tear strength and a puncture strain within the range defined by the present disclosure, and thus, it is possible to ensure the manufacture of a membrane-electrode assembly having high durability of more than 30,000 wet / dry cycles measured according to the NEDO scheme.

[0038] In addition, according to the present disclosure, it has been found that the tear strength and puncture strain of the polymer electrolyte membrane are directly related to the wet / dry cycle according to the NEDO scheme, which is usually measured to evaluate the mechanical durability of the membrane-electrode assembly. Therefore, by measuring the tear strength and puncture strain of the prepared polymer electrolyte membrane, the mechanical durability of the membrane-electrode assembly manufactured using the polymer electrolyte membrane can be easily predicted even before actual manufacturing. Therefore, the time and cost required for the research and development of membrane-electrode assemblies and fuel cells can be significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a cross-sectional view of a polymer electrolyte membrane according to one embodiment of the present disclosure. DETAILED DESCRIPTION

[0040] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings.

[0041] Figure 1 is a cross-sectional view of a polymer electrolyte membrane 100 according to one embodiment of the present disclosure.

[0042] like Figure 1 As shown in , a polymer electrolyte membrane 100 according to the present disclosure includes a composite layer 110 including a porous support 10 having a plurality of pores and an ionomer 21 / 22 filling the pores.

[0043] The porous support 10 may include a perfluorinated polymer (e.g., polytetrafluoroethylene (PTFE) or polytetrafluoroethylene and CF2=CFC) having high resistance to heat and chemical decomposition. n F 2n+1 (n is a real number from 1 to 5) or CF2=CFO-(CF2CF(CF3)O) m C n F 2n+1 (m is a real number of 0 to 15, and n is a real number of 1 to 15). As a non-exclusive example, a commercially available expanded polytetrafluoroethylene membrane (e-PTFE membrane) can be used as the porous support 10 .

[0044] Or, porous carrier 10 can be a nonwoven web made of hydrocarbon polymer. For example, porous carrier 10 can be a nanonet in which the nanofiber with an average diameter of 40nm to 5000nm is randomly arranged. The hydrocarbon polymer can be a polymer with excellent chemical resistance and no risk of deformation due to moisture in a high humidity environment, such as aliphatic polyamide, aromatic polyamide, polyimide, polyetherimide, polyacrylonitrile, polyaniline, polyethylene oxide, polyethylene naphthalate, polybutylene terephthalate, styrene butadiene rubber, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyvinylidene fluoride, polyvinyl butene, polyurethane, polybenzoxazole, polybenzimidazole, polyamide-imide, polyethylene terephthalate, polyphenylene sulfide, polyethylene, polypropylene, a copolymer of two or more thereof or a mixture of two or more thereof. In particular, polyimide is one of the preferred candidate materials for forming the porous support 10 because it has excellent heat resistance, chemical resistance, and dimensional stability.

[0045] The porosity of the porous support 10 may be 45% or more, preferably 50% or more, and more preferably 60% to 90%. If the porosity of the porous support 10 is less than 45%, the amount of ionomer in the porous support 10 is too small, and thus the ionic conductivity of the polymer electrolyte membrane 100 is reduced. On the other hand, if the porosity of the porous support 10 is greater than 90%, the intended reinforcing function of the porous support is deteriorated, and the dimensional stability of the porous support is reduced, and therefore, the subsequent process cannot be smoothly performed.

[0046] The ionomer 21 / 22 is a cation conductor having cation exchange groups or an anion conductor having anion exchange groups.

[0047] The cation conductor may be a fluorine-based polymer containing at least one cation exchange group selected from the group consisting of sulfonic acid group, carboxyl group, boric acid group, phosphoric acid group, imide group, sulfonimide group, sulfonamide group, fluorinated sulfonic acid group, and derivatives thereof. For example, the cation conductor may be, but is not limited to, poly(perfluorosulfonic acid), poly(perfluorocarboxylic acid), a copolymer of tetrafluoroethylene and fluorovinyl ether containing a sulfonic acid group, defluorinated polyetherketonesulfide, or a mixture of two or more thereof.

[0048] Alternatively, the cation conductor may be a hydrocarbon polymer comprising at least one cation exchange group selected from the group consisting of sulfonic acid group, carboxyl group, boric acid group, phosphoric acid group, imide group, sulfonimide group, sulfonamide group, fluorinated sulfonic acid group and derivatives thereof. For example, the cation conductor may be, but is not limited to, sulfonated polyimide (S-PI), sulfonated polyarylethersulfone (S-PAES), sulfonated polyetheretherketone (SPEEK), sulfonated polybenzimidazole (SPBI), sulfonated polysulfone (S-PSU), sulfonated polystyrene (S-PS), sulfonated polyphosphazene, sulfonated polyquinoxaline, sulfonated polyketone, sulfonated polyphenylene oxide, sulfonated polyethersulfone, sulfonated polyetherketone, sulfonated polyphenylene sulfone, sulfonated polyphenylene sulfide, sulfonated polyphenylene sulfide sulfone, sulfonated polyphenylene sulfide sulfone nitrile, sulfonated polyarylether, sulfonated polyarylether nitrile, sulfonated polyarylether ether nitrile, sulfonated polyarylether sulfone ketone, or a mixture of two or more thereof.

[0049] The anion conductor is a polymer capable of transferring anions such as hydroxide ions, carbonate or bicarbonate. Polymers doped with metal hydroxides can generally be used as anion conductors. Specifically, poly(ether sulfone), polystyrene, vinyl polymers, poly(vinyl chloride), poly(vinylidene fluoride), poly(tetrafluoroethylene), poly(benzimidazole) or poly(ethylene glycol) doped with metal hydroxides can be used as anion conductors.

[0050] The polymer electrolyte membrane 100 according to the present disclosure has an MD tear strength of 150 N / mm or more (eg, 170 N / mm to 320 N / mm), and a TD tear strength of 150 N / mm or more (eg, 160 N / mm to 320 N / mm).

[0051] The terms “MD” and “TD” used in this specification refer to “machine direction” and “transverse direction”, respectively. The “machine direction” is the direction in which the polymer electrolyte membrane 100 moves during manufacture, and the “transverse direction” is a direction perpendicular to the “machine direction”.

[0052] In the present disclosure, the “tear strength” of the polymer electrolyte membrane 100 is measured as follows.

[0053] [Tear strength]

[0054] A sample of 50 mm×50 mm was taken, and the maximum force applied to the sample until the sample was torn was measured under the following conditions according to ASTM D624 using a universal testing machine (UTM) (Instron 5966).

[0055] -Temperature: 23±2℃

[0056] -Relative humidity: 50±5%

[0057] -Test speed: 500±50mm / min

[0058] Subsequently, the tear strength of the sample was calculated using the following Equation 3.

[0059] [Equation 3]: TS = F / d

[0060] Wherein, TS represents the tear strength of the sample (N / mm), F represents the maximum force applied to the sample (N), and d represents the median thickness (mm), which is the arithmetic mean of the thickness of the sample measured at three points of the central part of the sample.

[0061] According to the above manner, the tear strengths of five samples were measured respectively, and the arithmetic mean value thereof was calculated, thereby obtaining the tear strength of the polymer electrolyte membrane 100 .

[0062] Even if the polymer electrolyte membrane 100 has the MD tear strength and TD tear strength within the above-specified ranges, the membrane-electrode assembly manufactured according to a conventional method using the polymer electrolyte membrane 100 does not always meet the high durability required by the industry (i.e., wet / dry cycles>30,000 times measured according to the NEDO scheme). In other words, the MD tear strength of 150 N / mm or more and the TD tear strength of 150 N / mm or more are necessary conditions for meeting 30,000 wet / dry cycles or more, but are not sufficient conditions.

[0063] Although the MD tear strength of the polymer electrolyte membrane 100 is 150 N / mm or more and the TD tear strength is 150 N / mm or more, therefore, it is necessary to actually manufacture a membrane-electrode assembly sample and perform a durability test according to the NEDO scheme in order to check whether a membrane-electrode assembly manufactured according to a conventional method using the polymer electrolyte membrane has sufficient durability. This requires a lot of time and leads to increased costs.

[0064] According to the present disclosure, it has been found that when the polymer electrolyte membrane 100 having a tear strength of 150 N / mm or more in MD and a tear strength of 150 N / mm or more in TD has a certain degree of puncture resistance, the membrane-electrode assembly manufactured by conventional methods using the polymer electrolyte membrane always meets more than 30,000 wet / dry cycles. Therefore, according to the present disclosure, the puncture resistance and tear strength of the polymer electrolyte membrane 100 are measured, thereby checking whether the membrane-electrode assembly meets the mechanical durability required by the industry without actual manufacturing. Therefore, the time and cost required for the research and development of membrane-electrode assemblies and fuel cells can be significantly reduced.

[0065] The method for measuring the durability of the polymer electrolyte membrane 100 according to the present disclosure includes: a step of taking a sample having a predetermined size and shape from the polymer electrolyte membrane 100; a step of fixing the sample to a bracket for a breakdown test according to ASTM F1342; a step of repeatedly puncturing the sample at a predetermined load and a predetermined speed using a probe for a breakdown test according to ASTM F1342; a step of measuring the displacement of the sample after each puncture; and a step of calculating the puncture strain using at least one of the measured displacements.

[0066] In an embodiment of the present disclosure, the puncture strain calculation step may include a step of calculating an initial puncture strain and a step of calculating a final puncture strain.

[0067] More specifically, in the present disclosure, the “puncture initial strain” and the “puncture final strain” of the polymer electrolyte membrane 100 are measured as follows.

[0068] [Puncture initial strain and puncture final strain]

[0069] Take a 50mm×50mm sample and use a universal testing machine (UTM) (Instron 5966) to measure the puncture resistance of the sample. According to ASTM F1342, a fixture (sample holder and probe) provided by Instron Company for the breakdown test is used as an accessory for repeated puncture. Specifically, the probe is used to repeatedly puncture (load: 10N) under the following conditions when the sample is fixed to the bracket (distance from the base to the sample: 100mm), and the distance shortened by each puncture (i.e., "displacement") is measured respectively. At this time, the displacement when a load of 0.2N is applied is considered to be zero.

[0070] -Temperature: 23±2℃

[0071] -Relative humidity: 50±5%

[0072] -Mode: Compressed mode

[0073] - Cycle period: 20 times

[0074] -Test speed: 100mm / min

[0075] The strain when the probe is punctured twice (load: 10 N) (i.e., “puncture initial strain”) and the strain when the probe is punctured 20 times (load: 10 N) (i.e., “puncture final strain”) are calculated by the following equations 1 and 2, respectively.

[0076] [Equation 1]: IS (%) = [(D2-D1) / D1] x 100

[0077] [Equation 2]: FS (%) = [(D 20 -D1) / D1]×100

[0078] Where IS represents the initial strain of puncture, FS represents the final strain of puncture, D1 represents the displacement caused by the first puncture (mm), D2 represents the displacement caused by the second puncture (mm), and D 20 represents the displacement (mm) caused by the twentieth puncture.

[0079] The polymer electrolyte membrane 100 according to the present disclosure has the MD / TD tear strength and puncture initial / final strains in the above ranges, and thus will ensure a membrane-electrode assembly with high durability of more than 30,000 wet / dry cycles measured according to the NEDO scheme.

[0080] That is, the present disclosure has found that the MD / TD tear strength and puncture initial / final strain of the polymer electrolyte membrane 100 are directly related to the wet / dry cycle according to the NEDO scheme, which is generally measured to evaluate the mechanical durability of the membrane-electrode assembly. Therefore, by measuring the tear strength and puncture strain of the prepared polymer electrolyte membrane 100, the mechanical durability of the membrane-electrode assembly to be manufactured using the polymer electrolyte membrane 100 can be easily predicted even before actual manufacturing. Therefore, the time and cost required for the research and development of membrane-electrode assemblies and fuel cells can be significantly reduced.

[0081] In an embodiment of the present disclosure, the in-plane ionic conductivity of the polymer electrolyte membrane 100 under the conditions of 80° C. and 50% RH may be 0.03 S / cm to 0.1 S / cm, for example, 0.046 S / cm to 0.1 S / cm, and the through-plane ionic conductivity may be 0.03 S / cm to 0.1 S / cm, for example, 0.042 S / cm to 0.1 S / cm. The detailed reasons why the polymer electrolyte membrane 100 according to the present disclosure has high ionic conductivity and excellent mechanical properties will be described later.

[0082] That is, the polymer electrolyte membrane 100 according to the embodiment of the present disclosure has excellent mechanical properties (i.e., MD tear strength of more than 150 N / mm, TD tear strength of more than 150 N / mm, puncture initial strain of less than 8% and puncture final strain of less than 10%) without deterioration of properties such as ionic conductivity, thereby ensuring the manufacture of a membrane-electrode assembly having excellent electrical properties and high durability of more than 30,000 wet / dry cycles.

[0083] In the present disclosure, the in-plane ionic conductivity and the through-plane ionic conductivity are measured using the following method.

[0084] [In-plane ionic conductivity]

[0085] The in-plane ionic conductivity of the polymer electrolyte membrane 100 was measured using a magnetic suspension balance apparatus (Bell Japan Company) at 80° C. and 50% RH.

[0086] [Through-surface ionic conductivity]

[0087] The through-plane ionic conductivity of the polymer electrolyte membrane 100 was measured using a through-plane membrane test system (Scribner Associates, MTS 740) according to the constant current four-terminal method. Specifically, the AC potential difference generated in the sample (10 mm × 30 mm) was measured while applying an AC current to both sides of the sample under the conditions of 80°C and 50% RH to obtain the membrane resistance R (Ω). Subsequently, the through-plane ionic conductivity of the polymer electrolyte membrane 100 was calculated using the following equation 4.

[0088] [Equation 4]: σ = L / [R × A]

[0089] (Where σ represents the ionic conductivity (S / cm), L represents the distance between the electrodes (cm), R represents the membrane resistance (Ω), and A represents the effective area of ​​the membrane (cm 2 ). )

[0090] like Figure 1 As shown in , according to an embodiment of the present disclosure, the composite layer 110 may have a first surface and a second surface opposite to the first surface, and the polymer electrolyte membrane 100 may further include a first resin layer 120 disposed on the first surface and a second resin layer 130 disposed on the second surface.

[0091] The first resin layer 120 may include a first ionomer 21 , and the second resin layer 130 may include a second ionomer 22 .

[0092] At least a portion of the ionomer in the composite layer 110 may be the same ionomer as at least one of the first ionomer 21 and the second ionomer 22 .

[0093] The thickness of the polymer electrolyte membrane 100 may be 10 μm to 50 μm, and the thickness of the composite layer 110 may be 30% to 90%, preferably 35% to 85%, and more preferably 40% to 80% of the thickness of the polymer electrolyte membrane 100. If the thickness percentage of the composite layer 110 is less than 30%, the effect of improving the mechanical durability and dimensional stability of the polymer electrolyte membrane 100 due to the use of the porous support 10 is not significant. On the other hand, if the thickness percentage of the composite layer 110 is greater than 90%, the thicknesses of the first resin layer 120 and the second resin layer 130 are too small, and therefore, the ionic conductivity of the polymer electrolyte membrane 100 is reduced.

[0094] like Figure 1 As shown in , the porous support 10 according to an embodiment of the present disclosure includes a first porous sub-support 11 and a second porous sub-support 12 .

[0095] The first porous sub-carrier 11 has a first surface of the composite layer 110. That is, one surface of the first porous sub-carrier 11 constitutes the first surface of the composite layer 110. Similarly, the second porous sub-carrier 12 has a second surface of the composite layer 110. That is, one surface of the second porous sub-carrier 12 constitutes the second surface of the composite layer 110.

[0096] The first porous sub-carrier 11 and the second porous sub-carrier 12 may be the same type of carrier or different types of carriers. For example, both the first porous sub-carrier 11 and the second porous sub-carrier 12 may be e-PTFE membranes or nonwoven webs. When both the first porous sub-carrier 11 and the second porous sub-carrier 12 are e-PTFE membranes, the sub-carriers may be stacked in such a manner that their extension directions are perpendicular to each other.

[0097] like Figure 1 As shown in , the first porous sub-carrier 11 and the second porous sub-carrier 12 may be in contact with each other. Since the first porous sub-carrier 11 and the second porous sub-carrier 12 are in close contact with each other, the interface between them cannot be visually inspected unless the sub-carriers are different kinds of porous carriers that can be distinguished from each other. That is, the porous carrier 10 may be an apparently single porous carrier.

[0098] Compared to a polymer electrolyte membrane reinforced by an actual single porous support having the same thickness as the porous support 10 (i.e., an actual single porous support providing the same or similar mechanical properties as the porous support 10), the polymer electrolyte membrane 100 having a first porous sub-carrier 11 and a second porous sub-carrier 12 according to an embodiment of the present disclosure provides many advantages in several aspects. For example, according to an embodiment of the present disclosure, compared with the case where an actual single porous support having the same thickness as the porous support 10 is impregnated with an ionomer, (i) since the surface area of ​​the porous support 10 in direct contact with the ionomer is large during the ionomer impregnation process, the porous support 10 is well wetted by the ionomer solution or dispersion, thereby minimizing the reduction in ionic conductivity of the polymer electrolyte membrane 100 due to the use of the support (i.e., the air in the pores of the support is better discharged and the voids are filled with ionomer, thereby preventing the remaining microbubbles from adversely affecting the ionic conductivity in the final polymer electrolyte membrane, and thus, a water channel as a movement path of hydrogen ions can be well formed in the through-surface direction of the support), and (ii) since the area where deformation of the polymer electrolyte membrane can be reduced is increased, the puncture strain of the polymer electrolyte membrane can be further reduced (i.e., the puncture resistance can be improved).

[0099] Therefore, the polymer electrolyte membrane 100 having the first porous sub-carrier 11 and the second porous sub-carrier 12 according to an embodiment of the present disclosure may have excellent mechanical properties without deterioration of properties such as ion conductivity.

[0100] The first porous sub-carrier 11 may have a plurality of first pores, wherein the first pores may be filled with the same ionomer as the first ionomer 21 of the first resin layer 120 .

[0101] The second porous sub-carrier 12 may have a plurality of second pores, wherein a portion of the second pores adjacent to the first porous sub-carrier 11 may be filled with an ionomer identical to the first ionomer 21 of the first resin layer 120 , and a remaining portion of the second pores adjacent to the second resin layer 130 may be filled with an ionomer identical to the second ionomer 22 of the second resin layer 130 .

[0102] That is, in the embodiment of the present disclosure, since the interface between the first ionomer 21 and the second ionomer 22 exists in the second porous sub-carrier 12 (that is, since the first ionomer 21 present in the second porous sub-carrier 12 functions as an anchor), the bonding force between the first porous sub-carrier 11 and the second porous sub-carrier 12 can be ensured, and the bonding force is as strong as the bonding force of the stacked structure having porous carriers bonded to each other by an adhesive and / or hot pressing, thereby preventing any degradation of ion conductivity that may be caused by using an adhesive and / or hot pressing for bonding the carriers. Therefore, the polymer electrolyte membrane 100 according to the embodiment of the present disclosure can have excellent mechanical properties without deteriorating properties such as ion conductivity.

[0103] The first ionomer 21 may be the same as or different from the second ionomer 22 .

[0104] In the following, the following will be described in detail Figure 1 Detailed Description of the Preferred Embodiments of the Invention A method for manufacturing a polymer electrolyte membrane 100 according to an embodiment of the present disclosure is shown in FIG.

[0105] The method according to an embodiment of the present disclosure includes: (i) casting a first mixed liquid containing a first ionomer 21; (ii) placing a first porous sub-carrier 11 in a dry state on the first mixed liquid, so that the first porous sub-carrier 11 becomes a completely wet state; (iii) adding a second porous sub-carrier 12 in a dry state on the first porous sub-carrier 11 immediately after the first porous sub-carrier 11 becomes a completely wet state, so that the first porous sub-carrier 11 and the second porous sub-carrier 12 are in contact with each other; (iv) applying a second mixed liquid containing a second ionomer 22 to the second porous sub-carrier 12, so that the second porous sub-carrier 12 becomes a completely wet state; and (v) drying the first porous sub-carrier 11 and the second porous sub-carrier 12 in a wet state.

[0106] The second porous sub-carrier 12 can be added to the first porous sub-carrier 11 while the first porous sub-carrier is kept in a completely wet state by the first mixed liquid, whereby a portion of the second pores of the second porous sub-carrier 12 can be filled with the first mixed liquid. Therefore, as described above, the first ionomer 21 present in a portion of the second pores of the second porous sub-carrier 12 acts as an anchor, whereby a strong adhesive force between the first porous sub-carrier 11 and the second porous sub-carrier 12 can be ensured, and the mechanical properties of the polymer electrolyte membrane 100 can be significantly improved.

[0107] In addition, according to the present disclosure, since such high bonding force between the first porous sub-carrier 11 and the second porous sub-carrier 12 is obtained without using a separate adhesive and / or hot pressing process, any degradation of ionic conductivity that may be caused by using an adhesive and / or hot pressing for bonding the carriers can be prevented. Therefore, the polymer electrolyte membrane 100 according to an embodiment of the present disclosure can have excellent mechanical properties without degradation of properties such as ionic conductivity.

[0108] That is, the polymer electrolyte membrane 100 according to the present disclosure is different from a stacked polymer electrolyte membrane manufactured by preparing two or more polymer electrolyte membranes and bonding them to each other by an adhesive and / or heat pressing in that a resin layer formed only of an ionomer is not included between the first porous sub-carrier 11 and the second porous sub-carrier 12. Unlike the present disclosure, in the stacked polymer electrolyte membrane, (i) as described above, deterioration of ion conductivity is inevitably caused due to the adhesive and / or heat pressing, and (ii) there is a resin layer formed only of an ionomer between the porous carriers, whereby resistance to hydrogen movement is relatively reduced, and therefore, chemical durability is significantly reduced due to relatively high hydrogen permeation.

[0109] As described above, the first porous sub-carrier 11 and the second porous sub-carrier 12 may be the same type of carrier or different types of carriers. For example, both the first porous sub-carrier 11 and the second porous sub-carrier 12 may be e-PTFE membranes or nonwoven webs.

[0110] Generally, an e-PTFE membrane is an anisotropic membrane, and there is a non-negligible difference between its mechanical properties (e.g., tensile strength and elongation) in the expansion direction and its mechanical properties (e.g., tensile strength and elongation) in the direction perpendicular to the expansion direction. For this reason, when both the first porous sub-carrier 11 and the second porous sub-carrier 12 are e-PTFE membranes, the second porous sub-carrier 12 can be added to the first porous sub-carrier 11 so that their expansion directions are perpendicular to each other, thereby further improving the mechanical properties of the polymer electrolyte membrane 100.

[0111] The step of applying the second mixed liquid containing the second ionomer 22 to the second porous sub-carrier 12 so that the second porous sub-carrier 12 becomes a completely wetted state may include: (i) when the first ionomer 21 and the second ionomer 22 are the same as each other, the step of adding the second porous sub-carrier 12 to the first porous sub-carrier 11 and immersing the first porous sub-carrier 11 and the second porous sub-carrier 12 in the second mixed liquid, or (ii) the step of applying the second mixed liquid to the exposed surface of the second porous sub-carrier 12 using a method such as rod coating, comma coating, slot die coating, screen printing, spray coating, doctor blade coating, etc.

[0112] The first mixed liquid and the second mixed liquid each may be a solution or dispersion in which the first ionomer 21 or the second ionomer 22 is dissolved or dispersed in water, a hydrophilic solvent, an organic solvent, or a mixed solvent of two or more thereof.

[0113] The hydrophilic solvent may have at least one functional group selected from alcohol, isopropanol, ketone, aldehyde, carbonate, carboxylate, carboxylic acid, ether and amide, each of which includes as its main chain a linear or branched saturated or unsaturated hydrocarbon having carbon atoms in the range of 1 to 12. Each of them may include an alicyclic or aromatic ring compound as at least a part of its main chain.

[0114] The organic solvent may be N-methylpyrrolidone, dimethyl sulfoxide, tetrahydrofuran or a mixture of two or more thereof.

[0115] In order to completely fill the pores of the first porous sub-carrier 11 and the second porous sub-carrier 12 with the first ionomer 21 or the second ionomer 22, various factors such as temperature and time may be appropriately adjusted. For example, at least one of the thickness of the first porous sub-carrier 11 and the second porous sub-carrier 12, the concentration of the first mixed liquid and the second mixed liquid, and the type of the solvent / dispersion medium may be appropriately adjusted.

[0116] The step of drying the joined first porous sub-carrier 11 and second porous sub-carrier 12 may include: first drying at 60°C to 150°C for 15 minutes to 1 hour, and second drying at 150°C to 190°C for 3 minutes to 1 hour. Specifically, the first drying may be performed at 60°C to 120°C for 15 minutes to 1 hour, and the second drying may be performed at 170°C to 190°C for 3 minutes to 1 hour. If the first drying temperature is lower than 60°C or the first drying time is shorter than 15 minutes, the solvent / dispersion medium cannot be first discharged, and a high-density membrane cannot be obtained. If the second drying temperature is higher than 190°C or the second drying time is longer than 1 hour, the ion exchange group (e.g., sulfonic acid group) will decompose and the performance of the membrane will deteriorate.

[0117] Optionally, although Figure 1 The polymer electrolyte membrane 100 shown in FIG. 1 includes only two porous sub-carriers 11 and 12 , but the polymer electrolyte membrane 100 according to the present disclosure may include more than two porous sub-carriers in consideration of required specific physical properties.

[0118] In another embodiment of the present disclosure, the polymer electrolyte membrane 100 may include a single porous support 10 instead of a plurality of porous sub-supports 11 and 12, and an ionomer dispersion to fill the pores of the single porous support 10 may be prepared by adding an ionomer to a solvent and mixing them using a resonant acoustic wave method. The ionomer dispersion thus obtained has high dispersion stability.

[0119] High pressure may be applied to the mixture obtained using resonant acoustic wave mixing in order to further improve the dispersion stability of the ionomer dispersion.

[0120] In the present disclosure, an ionomer dispersion having high dispersion stability refers to an ionomer dispersion having a viscosity ratio defined by the following equation 5 of 1.7 or less and a shear stress ratio defined by the following equation 6 of 1.5 or less, wherein the viscosity and shear stress of the ionomer dispersion are measured using a rheometer at a shear rate of 0.001 s -1 Increase to 1000s -1 , then from 1000s -1 Reduced to 0.001s -1 Simultaneous measurement.

[0121] [Equation 5]: Viscosity ratio = η2 / η1

[0122] (where η1 represents the shear rate of the ionomer dispersion measured at 1s -1 The first viscosity at a shear rate of 1s is represented by η2, which is the viscosity of the ionomer dispersion measured at 1s when the shear rate is reduced. -1 The second viscosity at the shear rate.

[0123] [Equation 6]: Shear stress ratio = σ2 / σ1

[0124] (where σ1 represents the first shear stress, which is measured at 1s when the shear rate increases. -1 The shear stress at the shear rate of 1s is σ2, which is the second shear stress measured when the shear rate decreases. -1 Shear stress at a shear rate of .

[0125] An ionomer dispersion having sufficiently high dispersion stability while containing a high content of ionomer solids can optimize the morphology of the ionomer in the polymer electrolyte membrane 100, thereby improving both the ionic conductivity and durability of the polymer electrolyte membrane 100. That is, the polymer electrolyte membrane 100 can have excellent mechanical durability, such as MD tear strength of 150 N / mm or more, TD tear strength of 150 N / mm or more, puncture initial strain of 8% or less, and puncture final strain of 10% or less, and can have an in-plane ionic conductivity of 0.03 S / cm to 0.1 S / cm and a through-plane ionic conductivity of 0.03 S / cm to 0.1 S / cm under the conditions of 80° C. and 50% RH.

[0126] Specifically, the ionomer dispersion with high dispersion stability has excellent impregnation performance and small and uniform particle size. Thus, when the porous support 10 is impregnated or coated with the ionomer dispersion to form the reinforced composite membrane type polymer electrolyte membrane 100, water channels that provide a movement path for hydrogen ions are well formed in the through-plane direction and the in-plane direction, thereby improving the ionic conductivity of the polymer electrolyte membrane 100 in both the in-plane direction and the through-plane direction.

[0127] Obviously, the ionomer dispersion having high dispersion stability may also be applied to the polymer electrolyte membrane 100 having a plurality of porous sub-carriers 11 and porous sub-carriers 12 .

[0128] The membrane-electrode assembly according to the present disclosure includes: an anode; a cathode; and a polymer electrolyte membrane 100 disposed between the anode and the cathode. The membrane-electrode assembly is the same as a conventional membrane-electrode assembly for a fuel cell, except that the polymer electrolyte membrane 100 according to the present disclosure is used as the polymer electrolyte membrane, and therefore, a detailed description thereof will be omitted in this specification.

[0129] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the embodiments of the present disclosure. However, the present disclosure can be implemented in various different forms and is not limited to the embodiments described herein.

[0130] [Manufacturing Example: Manufacturing of Polymer Electrolyte Membrane]

[0131] (Example 1)

[0132] The first porous sub-support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.1) was wetted with a first ionomer dispersion ("resonant acoustic mixing + high pressure dispersion", viscosity ratio: 1.01, shear stress ratio: 1.01) containing 20 wt% of a highly fluorinated polymer with an equivalent weight (EW) of 800 g / eq.

[0133] A second porous sub-carrier (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.1) was added to the first porous sub-carrier in a wet state so that their extension directions crossed each other.

[0134] A second ionomer dispersion ("resonance acoustic mixing + high pressure dispersion", viscosity ratio: 1.01, shear stress ratio: 1.01) containing 20 wt% of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq was additionally coated on the second porous sub-support added on the first porous sub-support.

[0135] Subsequently, the first porous sub-support and the second porous sub-support were dried at 60° C. for 1 hour and then at 150° C. for 30 minutes to obtain a polymer electrolyte membrane.

[0136] (Example 2)

[0137] A first porous sub-support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.2) was wetted with a first ionomer dispersion (resonant acoustic mixing, viscosity ratio: 1.26, shear stress ratio: 1.09) comprising 20 wt% of a highly fluorinated polymer with an equivalent weight (EW) of 800 g / eq.

[0138] A second porous sub-carrier (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.2) was added to the first porous sub-carrier in a wet state so that their extension directions intersected each other. At this time, the first porous sub-carrier and the second porous sub-carrier were stacked so that the extension direction of the first porous sub-carrier and the extension direction of the second porous sub-carrier were perpendicular to each other.

[0139] A second ionomer dispersion (resonant acoustic mixing, viscosity ratio: 1.26, shear stress ratio: 1.09) containing 20 wt% of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq was additionally coated onto the second porous sub-support added onto the first porous sub-support.

[0140] Subsequently, the first porous sub-support and the second porous sub-support were dried at 60° C. for 1 hour and then at 150° C. for 30 minutes to manufacture a polymer electrolyte membrane.

[0141] [Measurement of physical properties of polymer electrolyte membrane]

[0142] The MD tear strength, TD tear strength, puncture initial strain, puncture final strain, in-plane ionic conductivity and through-plane ionic conductivity of each polymer electrolyte membrane according to the above examples were measured using the following methods and the results are shown in Table 1 below.

[0143] *MD / TD tear strength

[0144] A sample of 50 mm×50 mm was taken, and the maximum force applied to the sample in the MD / TD directions until the sample was torn was measured using a universal testing machine (UTM) (Instron 5966) according to ASTM D624 under the following conditions.

[0145] -Temperature: 23±2℃

[0146] -Relative humidity: 50±5%

[0147] -Test speed: 500±50mm / min

[0148] Subsequently, the MD / TD tear strength of the sample was calculated using Equation 3 below.

[0149] [Equation 3]: TS = F / d

[0150] Wherein, TS represents the MD / TD tear strength of the sample (N / mm), F represents the maximum force applied to the sample (N), and d represents the median thickness (mm), which is the arithmetic mean of the thickness of the sample measured at three points in the central part of the sample.

[0151] According to the above method, the MD / TD tear strengths of five samples were measured respectively, and the arithmetic mean value thereof was calculated, thereby obtaining the MD / TD tear strength of the polymer electrolyte membrane.

[0152] * Initial puncture strain and final puncture strain

[0153] Take a 50mm×50mm sample and use a universal testing machine (UTM) (Instron 5966) to measure the puncture resistance of the sample. According to ASTM F1342, a fixture (sample holder and probe) for the breakdown test provided by Instron Company is used as an accessory for repeated puncture. Specifically, in a state where the sample is fixed to a bracket (distance from the base to the sample: 100mm), a probe is used for repeated puncture (load: 10N) under the following conditions, and the reduction in distance caused by each puncture (i.e., "displacement") is measured. At this time, the displacement when a load of 0.2N is applied is considered to be zero.

[0154] -Temperature: 23±2℃

[0155] -Relative humidity: 50±5%

[0156] -Mode: Compressed mode

[0157] - Cycle period: 20 times

[0158] -Test speed: 100mm / min

[0159] The strain when the probe is punctured twice (load: 10 N) (i.e., “puncture initial strain”) and the strain when the probe is punctured 20 times (load: 10 N) (i.e., “puncture final strain”) are calculated by the following equations 1 and 2, respectively.

[0160] [Equation 1]: IS (%) = [(D2-D1) / D1] x 100

[0161] [Equation 2]: FS (%) = [(D 20 -D1) / D1]×100

[0162] Where IS represents the initial strain of puncture, FS represents the final strain of puncture, D1 represents the displacement caused by the first puncture (mm), D2 represents the displacement caused by the second puncture (mm), and D 20 represents the displacement (mm) caused by the twentieth puncture.

[0163] * In-plane ionic conductivity

[0164] The in-plane ionic conductivity of the polymer electrolyte membrane 100 was measured at 80° C. and 50% RH using a magnetic suspension balance apparatus (Bell Japan Company).

[0165] *Through-surface ionic conductivity

[0166] The through-plane ionic conductivity of the polymer electrolyte membrane 100 was measured according to the constant current four-terminal method using a through-plane membrane test system (Scribner Associates, MTS 740). Specifically, the AC potential difference generated in the sample (10 mm×30 mm) was measured while applying an AC current to both sides of the sample under the conditions of 80° C. and 50% RH to obtain the membrane resistance R (Ω). Subsequently, the through-plane ionic conductivity of the polymer electrolyte membrane 100 was calculated using the following equation 4.

[0167] [Equation 4]: σ = L / [R × A]

[0168] (Where σ represents the ionic conductivity (S / cm), L represents the distance between the electrodes (cm), R represents the membrane resistance (Ω), and A represents the effective area of ​​the membrane (cm 2 ). )

[0169] [Measurement of wet / dry cycles of membrane-electrode assemblies (MEAs)]

[0170] A membrane-electrode assembly (MEA) was manufactured using a polymer electrolyte membrane, and the wet / dry cycle of the membrane-electrode assembly was measured according to the NEDO scheme. Specifically, while nitrogen was injected into the anode and cathode at a flow rate of 800 NmL / min, a wet / dry cycle consisting of humidification (150% RH, 2 minutes) and drying (0% RH, 2 minutes) was repeated. Hydrogen permeation (Hydrogen crossover) of MEA was measured every 1000 cycles using linear sweep voltammetry (LSV). Specifically, while hydrogen was injected into the anode at a flow rate of 200 NmL / min and nitrogen was injected into the cathode at a flow rate of 200 NmL / min at 80 ° C and 100% RH, 0.2V to 0.5V parts were scanned at a scan rate of 0.5mV / s to extract the current density data of 0.4V to 0.5V parts. Linear fitting of data was performed to obtain the current density value of the part where the voltage was 0. When the measured hydrogen permeation is 10 times or more of the initial hydrogen permeation, the evaluation is terminated, and the number of cycles performed until then is taken as the wet / dry cycle of the MEA. For example, when the measured hydrogen permeation after completing a total of 15,000 cycles is less than 10 times the initial hydrogen permeation, but the measured hydrogen permeation after completing a total of 16,000 cycles is more than 10 times the initial hydrogen permeation, the wet / dry cycle of the MEA is "more than 15,000 cycles".

[0171] [Table 1]

[0172] Example 1 Example 2 MD tear strength (N / mm) 225 171 TD tear strength (N / mm) 250 160 Initial puncture strain (%) 4.4 5.0 Final puncture strain (%) 5.5 6.3 MEA wet / dry cycles (number of cycles) 40,000 and above 30,000 and above In-plane ionic conductivity (S / cm) 0.046 0.048 Total ionic conductivity (S / cm) 0.042 0.038

Claims

1. A polymer electrolyte membrane, comprising a composite layer, the composite layer comprising: (i) a porous support; and (ii) first and second ionomers, Wherein, the porous carrier comprises: a first porous sub-support having first pores; and a second porous sub-support having second pores, wherein the first porous sub-carrier and the second porous sub-carrier are in contact with each other, wherein the first pores are filled with a first ionomer, wherein a portion of the second pores adjacent to the first porous sub-support is filled with the first ionomer and a remaining portion of the second pores is filled with the second ionomer such that an interface between the first and second ionomers exists in the second porous sub-support, Wherein, the thickness of the polymer electrolyte membrane is 10 to 50 μm, Wherein, the thickness of the composite layer is 40 to 80% of the thickness of the polymer electrolyte membrane. The polymer electrolyte membrane has an MD tear strength of 150 N / mm or more, a TD tear strength of 150 N / mm or more, an initial puncture strain of 8% or less, and a final puncture strain of 10% or less, and The polymer electrolyte membrane has an in-plane ionic conductivity of 0.03 S / cm to 0.1 S / cm and a through-plane ionic conductivity of 0.03 S / cm to 0.1 S / cm under conditions of 80° C. and 50% RH.

2. The polymer electrolyte membrane according to claim 1, wherein The polymer electrolyte membrane has an MD tear strength of 170 N / mm to 320 N / mm, a TD tear strength of 160 N / mm to 320 N / mm, an initial puncture strain of 1% to 6%, and a final puncture strain of 2% to 8%.

3. The polymer electrolyte membrane according to claim 1, wherein The polymer electrolyte membrane also includes: a first resin layer disposed on the first porous sub-support, the first resin layer comprising an ionomer that is the same as the first ionomer; and A second resin layer is disposed on the second porous sub-support, the second resin layer comprising an ionomer that is the same as the second ionomer.

4. The polymer electrolyte membrane according to claim 1, wherein The porous support also includes a third porous sub-support in contact with the second porous sub-support.

5. The polymer electrolyte membrane according to claim 1, wherein The first ionomer is the same as or different from the second ionomer.

6. A membrane-electrode assembly comprising: anode; cathode; and The polymer electrolyte membrane according to claim 1, wherein the polymer electrolyte membrane is provided between the anode and the cathode.