A method for preparing quantum dot patterns based on surface pretreatment
By using hydrophilic and hydrophobic substances in pretreatment and template imprinting processes in quantum dot display technology, the problem of pattern deformation caused by the fluidity of the quantum dot solution is solved, a more regular and neat color conversion layer is achieved, and the Display quality.
Patent Information
- Application Number
- CN202210295814.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-03-24
AI Technical Summary
In the field of quantum dot display, it is difficult to effectively prepare regular and neat color conversion layer patterns with existing technology, resulting in problems such as pattern deformation and poor quality caused by the fluidity of the quantum dot solution.
By pretreating the substrate surface before depositing the quantum dot solution, using hydrophilic and hydrophobic substances to form a specific pattern, and combining the template imprinting process to prepare a pattern composed of hydrophilic and hydrophobic substances, limiting the quantum dot solution. Deposit areas, thereby improving pattern regularity and controllability.
It effectively alleviates the difference between the design pattern and the actual pattern, improves the shape regularity and high controllability of the quantum dot color conversion layer, and improves the light emission effect of narrow half-width and high color quality.
Smart Images

Figure CN114744100B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of quantum dot display, and in particular to a method for preparing a quantum dot pattern based on surface pretreatment. Background Art
[0002] Compared with LCD, OLED and other technologies, Micro LED has attracted more and more interest due to its many advantages such as self-luminescence, low power consumption, high brightness and high reliability. Micro LED display technology is also called "next-generation display technology". More and more researchers and manufacturers are investing in the research of Micro LED.
[0003] There are two main technical routes for full-colorization of Micro LED: ① RGB method, that is, to achieve full colorization by controlling the light emission of three chips, R, G, and B, respectively. However, this technical route faces the technical barrier of mass transfer, which is difficult and expensive. ② Color conversion method, that is, to achieve full color by exciting long-wavelength red and green light with short-wavelength blue-violet light. Compared with the RGB method, this method has great advantages in terms of technical difficulty and cost, and is currently the easiest method to achieve full colorization. In the color conversion method, a color conversion layer needs to be prepared on the device surface or substrate. Factors such as the shape and thickness of the color conversion layer have an important relationship with the quality of the excitation light.
[0004] In the process of applying quantum dots to the display field, the patterning of the quantum dot color conversion layer plays a pivotal role. Quantum dot solutions can be made into various patterns to meet different needs through masking, photolithography, inkjet printing and other technologies. However, due to the fluidity of the quantum dot solution itself, the prepared pattern will deform, and the pattern shape will be irregular, uneven, and highly uncontrollable, resulting in a large difference between the actual quantum dot pattern and the designed pattern, such as Figure 1 As shown, (the dotted line frame is the design pattern, and the solid line frame is the actual pattern). The existence of these phenomena will inevitably have an adverse effect on the light output quality of the color conversion layer. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing quantum dot patterns based on surface pretreatment. By pretreating the surface of the deposited quantum dots with hydrophilic and hydrophobic substances before the deposition of the quantum dot solution, the difference between the designed pattern and the actual pattern can be effectively alleviated.
[0006] In order to achieve the above purpose, the technical solution of the present invention is:
[0007] A method for preparing a quantum dot pattern based on surface pretreatment is to pretreat the surface of a substrate, to form a first pattern composed of a hydrophilic substance and a second pattern composed of a hydrophobic substance on the surface of the pretreated substrate, wherein the second pattern is arranged outside the first pattern and matches the edge of the first pattern, and a quantum dot solution is deposited on the first pattern; wherein at least one of the first pattern and the second pattern is prepared by the following process:
[0008] A template is provided, the template surface has a concave-convex structure, wherein the convex part forms a pattern surface; a hydrophilic substance or a hydrophobic substance is coated on the pattern surface, and a pattern composed of the hydrophilic substance or the hydrophobic substance corresponding to the pattern surface is formed on a substrate by an embossing process.
[0009] Optionally, include the following steps:
[0010] 1) Pre-treating the substrate surface;
[0011] 2) providing a first template, wherein the surface of the first template has a plurality of discrete columnar structures, the surfaces of the plurality of discrete columnar structures form a first pattern surface, a hydrophilic material is coated on the first pattern surface, and a first pattern is formed on the substrate by an imprinting process;
[0012] 3) providing a second template, wherein the surface of the second template has a plurality of discrete pits, the pits are opposite to the columnar structures in position and have a similar size, the surface outside the plurality of discrete pits forms a second pattern surface, a hydrophobic material is coated on the second pattern surface, and a second pattern is formed on the substrate by an imprinting process;
[0013] 4) depositing a quantum dot solution on the surface of the first pattern;
[0014] There is no particular order between step 2) and step 3).
[0015] Optionally, include the following steps:
[0016] 1) Pre-treating the substrate surface;
[0017] 2) coating a layer of hydrophobic material on the surface of the substrate;
[0018] 3) providing a first template, wherein the surface of the first template has a plurality of discrete columnar structures, the surfaces of the plurality of discrete columnar structures form a first pattern surface, a hydrophilic substance is coated on the first pattern surface, and a first pattern is formed on the substrate by an embossing process, and the hydrophobic substance outside the first pattern forms a second pattern;
[0019] 4) Depositing a quantum dot solution on the first pattern surface.
[0020] Optionally, include the following steps:
[0021] 1) Pre-treating the substrate surface;
[0022] 2) coating a layer of hydrophilic material on the surface of the substrate;
[0023] 3) providing a second template, wherein the surface of the second template has a plurality of discrete pits, the surface outside the plurality of discrete pits forms a second pattern surface, a hydrophobic substance is coated on the second pattern surface, and a second pattern is formed on the substrate by an imprinting process, and the hydrophilic substance outside the second pattern forms a first pattern;
[0024] 4) Depositing a quantum dot solution on the first pattern surface.
[0025] Optionally, the substrate surface is pretreated by placing the substrate in acetone and alcohol solutions in turn, ultrasonically cleaning each for 5-10 minutes, then rinsing with deionized water for 5-10 minutes, and drying with nitrogen; placing the dried substrate in the cavity of a plasma cleaning machine with a power of 50 to 300 W for 3 to 5 minutes.
[0026] Optionally, the quantum dots in the quantum dot solution have hydrophilic groups on their surfaces.
[0027] Optionally, the quantum dots in the quantum dot solution are red quantum dots or green quantum dots.
[0028] Optionally, the quantum dot solution is deposited on the first pattern by an inkjet printing process.
[0029] Optionally, the hydrophilic substance includes one of polyvinyl alcohol, polyether polyol and polyacrylic acid.
[0030] Optionally, the hydrophobic substance includes at least one of polycarbonate, polyolefin, polyacrylonitrile, polyester, fluorinated chloroethylene, polytetrafluoroethylene, and polyamide.
[0031] The beneficial effects of the present invention are:
[0032] By utilizing the relevant properties of hydrophilic and hydrophobic substances and patterning the area where the quantum dot solution is to be deposited, the shape of the deposited quantum dot color conversion layer can be made more regular and the height more controllable, and the color conversion layer pattern is not easily deformed due to the flow of the quantum dot solution. The regularity and neatness of the pattern of the quantum dot color conversion layer are conducive to the realization of narrow half-width and high color quality light output. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The quantum dot forming pattern is the prior art;
[0034] Figure 2 is a schematic top view of a quantum dot solution deposition pattern of an embodiment;
[0035] Figure 3 is a schematic structural diagram of a first template of an embodiment;
[0036] Figure 4 is a schematic structural diagram of a second template of the embodiment;
[0037] Figure 5 Schematic diagram of hydrophilic principle;
[0038] Figure 6 Schematic diagram of the hydrophobic principle;
[0039] Figure 7 is a schematic diagram of a first pattern of Example 1;
[0040] Figure 8 A schematic diagram of a quantum dot pattern to be deposited composed of a first pattern and a second pattern in Example 1;
[0041] Fig. 9 This is a schematic diagram of a red light color conversion layer array formed by depositing red quantum dots in Example 1;
[0042] Fig.10 Schematic diagram of a red light color conversion layer array and a green light color conversion layer array of Example 1;
[0043] Fig.11 Schematic diagram of the inkjet printing process;
[0044] Fig.12 is a schematic diagram of a whole layer of hydrophobic material in Example 2;
[0045] Fig.13 is a schematic diagram of a whole layer of hydrophilic material in Example 3;
[0046] Fig.14 This is the quantum dot forming pattern of the present invention. DETAILED DESCRIPTION
[0047] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.
[0048] The method for preparing a quantum dot pattern based on surface pretreatment of the embodiment mainly consists of three parts:
[0049] 1. Design of the deposition pattern of quantum dot solution. A pattern composed of hydrophilic material and hydrophobic material is set in the area where the quantum dot solution is to be deposited (a square is used as an example in the embodiment, and other patterns that meet the requirements are also acceptable), the first pattern A composed of the hydrophilic material is inside, and the second pattern B composed of the hydrophobic material is outside, such as Figure 2 The second pattern B matches the edge of the first pattern A, which means that at the junction of the two patterns, the hydrophilic substance and the hydrophobic substance can contact each other or there is a very small distance (≤5 microns) between the two.
[0050] 2. Template design. To meet the needs of mass production, two sets of templates are designed in this technical solution, which are used to form a first pattern A composed of hydrophilic substances and a second pattern B composed of hydrophobic substances. Figure 3 As shown, the surface of the first template 2 has a concave-convex structure, and the protruding part is a plurality of discrete columnar structures 21, which can be arranged at regular intervals, for example, and the top surfaces of the columnar structures 21 are combined to form a first pattern surface, and a hydrophilic material is coated on the top surfaces of the columnar structures. Figure 4 As shown, the upper surface of the second template 3 is distributed with many pits 31, the positions of the pits 31 are opposite to the columnar structures of the first template 2, and the sizes are similar. The surface outside the pits 21 forms a second pattern surface, and the hydrophobic material is coated on the surface of the second template except for the positions of the pits. Through the cooperation of the two sets of templates, the required pattern can be prepared on the surface of the substrate quickly and in large quantities.
[0051] 3. Deposition of quantum dot solution. Deposit the quantum dot solution on the hydrophilic material (i.e., the first pattern A), and use the "hydrophilic" properties of the relevant groups in the hydrophilic material to enhance the adhesion between the quantum dot solution and the substrate, such as Figure 5 The quantum dot solution is not deposited on the pattern composed of the hydrophobic material arranged outside the hydrophilic material pattern (i.e., the second pattern B). When the quantum dot solution diffuses onto the pattern composed of the hydrophobic material, the "hydrophobic" characteristics of the relevant groups in the hydrophobic material can limit the diffusion of the quantum dot solution. Figure 6 .
[0052] The surface of a hydrophilic substance has a higher surface energy, and its components generally include but are not limited to groups such as carboxyl, amino, and hydroxyl. The surface of a hydrophobic substance has a lower surface energy, and its components generally include but are not limited to fluorocarbon compounds, silicone resins, etc. The surface of quantum dots contains groups such as carboxyl, amino, and hydroxyl, and is soluble in aqueous solution. For example, the hydrophilic substance includes one of polyvinyl alcohol, polyether polyol, and polyacrylic acid; the hydrophobic substance includes at least one of polycarbonate, polyolefin, polyacrylonitrile, polyester, fluorinated chloroethylene, polytetrafluoroethylene, and polyamide.
[0053] Example 1
[0054] 1. Substrate cleaning. Place the substrate in acetone and alcohol solutions in turn, ultrasonically clean for 5-10 minutes, rinse with deionized water for 5-10 minutes, and blow dry with nitrogen. The substrate can be a hard substrate such as a glass substrate, a silicon substrate, etc., preferably a light-transmitting glass substrate.
[0055] 2. Plasma treatment: Place the dried substrate into the Asher chamber at 200W for 3-5 minutes, and use the high activity of oxygen plasma to further clean the substrate surface.
[0056] 3. Pattern preparation. Figure 3 The first template and Figure 4 First, the first template is used to prepare a first pattern A composed of a hydrophilic material in the region of the substrate 1 where the quantum dots are to be deposited by means of embossing, such as Figure 7 As shown, a second pattern B composed of a hydrophobic material is prepared on the periphery of the hydrophilic material pattern by a second template in the same manner. The first pattern A and the second pattern B together constitute a pattern of the quantum dot solution to be deposited, as shown in FIG. Figure 8 As shown, the inner circle pattern is composed of a hydrophilic substance, and the outer circle pattern is composed of a hydrophobic substance. At the junction of the inner and outer circles, the hydrophilic substance is in contact with the hydrophobic substance. The sizes of the inner circle pattern and the outer circle pattern can be designed according to needs. The specific process of pattern formation is as follows: ① The surface of the columnar structure 21 of the first template 2 is coated with a polyvinyl alcohol solution of a hydrophilic substance by smearing, immersing, etc. ② Under a certain pressure, the first template 2 coated with a hydrophilic substance is tightly attached to the plasma-treated substrate 1 and maintained for 3-5 minutes. After the two are separated and the solvent is evaporated, an array-like first pattern composed of a hydrophilic substance is prepared on the surface of the substrate 1, as shown Figure 8 As shown. ③ Use smearing, immersion and other methods to coat the surface of the second template 3 (except the pits 31) with a hydrophobic polycarbonate solution. ④ Use the alignment marks on the template to achieve precise alignment between the second template 3 and the first pattern A (specifically, the pits 31 and the first pattern A are aligned one by one). Under a certain pressure, the second template 3 coated with the hydrophobic substance is tightly attached to the substrate with the first pattern A and maintained for 3-5 minutes (the pits 31 of the hydrophobic template just surround the first pattern A). After the two are separated and the solvent evaporates, a hydrophobic second pattern B is formed. The first pattern A and the second pattern B together constitute the pattern of quantum dots to be deposited, as shown in FIG. Figure 8 shown.
[0057] 4. Deposition of red light quantum dot solution. Deposit the quantum dot solution in the pattern on the substrate by inkjet printing or other methods. The quantum dot solution is deposited only on a portion of the first pattern A composed of the hydrophilic material, such as Fig. 9 As shown, a red light color conversion layer array 4 is obtained. The red quantum dot material is CdSe / ZnS, and the hydrophilic group is a carboxyl group.
[0058] 5. Deposition of green quantum dot solution. In the same manner as the red quantum dot solution, a green quantum dot solution is deposited on another part of the first pattern A composed of the hydrophilic material to obtain a green light color conversion layer array 5, thereby completing the preparation of a color conversion layer that can achieve full colorization, such as Fig.10 As shown in the figure, the green quantum dot material is CdSe / CdS, and the hydrophilic group is carboxyl.
[0059] The inkjet printing process is completed by, for example, the instrument Super Inkjet Printer Model SIJ-S350, which can directly prepare high-precision quantum dot patterns on the substrate without a mask. The inkjet printing process is as follows Fig.11 shown.
[0060] Example 2
[0061] In order to quickly prepare a pattern composed of a hydrophilic substance and a hydrophobic substance on a substrate, this embodiment provides another simpler technical solution. Figure 3 The first template shown can realize the preparation of the pattern, as follows:
[0062] Steps 1-2 are the same as those in Example 1 and will not be repeated here.
[0063] 3. Pattern preparation. A layer of hydrophobic material B' is adhered to the surface of the cleaned and plasma-treated substrate by spin coating or the like. The hydrophobic material is evenly distributed on the surface of the substrate, such as Fig.12 Then, the first template 2 uses the aforementioned embossing method to directly prepare a first pattern A composed of a hydrophilic substance on the hydrophobic substance of the substrate, and the hydrophobic substance outside the first pattern A forms a second pattern B, thereby completing the preparation of the pattern to be deposited by the quantum dot solution. Figure 8 The method only needs to prepare one template, which is less expensive and does not need to consider the problem of pattern registration, and is more suitable for large-scale production.
[0064] Steps 4-5 are the same as those in Example 1 and will not be repeated here.
[0065] Example 3
[0066] This embodiment provides another technical solution. Figure 4 The second template shown can realize the preparation of the pattern, as follows:
[0067] Steps 1-2 are the same as those in Example 1 and will not be repeated here.
[0068] 3. Pattern preparation. A layer of hydrophilic material A' is adhered to the surface of the cleaned and plasma-treated substrate by spin coating or the like. The hydrophilic material is evenly distributed on the surface of the substrate, such as Fig.13 Then, the second template 3 uses the aforementioned embossing method to directly prepare a second pattern B composed of a hydrophobic substance on the hydrophilic substance of the substrate, and the exposed hydrophilic substance in the hollowed-out part outside the second pattern B forms the first pattern A, thereby completing the preparation of the pattern to be deposited by the quantum dot solution, and also referring to Figure 8 The method only needs to prepare one template, which is less expensive and does not need to consider the problem of pattern registration, and is more suitable for large-scale production.
[0069] Steps 4-5 are the same as those in Example 1 and will not be repeated here.
[0070] refer to Fig.14 , the dotted frame in the figure is the design pattern, and the solid frame is the actual pattern. The present invention can effectively alleviate the difference between the design pattern and the actual pattern by using hydrophilic substances and hydrophobic substances to pre-treat the surface of the deposited quantum dots before the quantum dot solution is deposited, so that the shape of the deposited quantum dot color conversion layer is more regular and the height is more controllable, and the color conversion layer pattern is not easily deformed due to the flow of the quantum dot solution. The regularity and neatness of the quantum dot color conversion layer pattern are conducive to the realization of narrow half-width and high color quality light output.
[0071] The above embodiments are only used to further illustrate a method for preparing a quantum dot pattern based on surface pretreatment of the present invention, but the present invention is not limited to the embodiments. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention fall within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a quantum dot pattern based on surface pretreatment, characterized in that: The following steps are involved: 1) Pre-treat the surface of the substrate by placing it in acetone and alcohol solutions in turn, ultrasonically cleaning it for 5-10 minutes, then rinsing it with deionized water for 5-10 minutes, and drying it with nitrogen; place the dried substrate in the chamber of a plasma cleaning machine with a power of 50~300W for 3-5 minutes; 2) providing a first template, wherein the surface of the first template has a plurality of discrete columnar structures, the surfaces of the plurality of discrete columnar structures form a first pattern surface, coating a solution of a hydrophilic substance on the first pattern surface, and forming a first pattern on the substrate by an imprinting process; 3) providing a second template, wherein the surface of the second template has a plurality of discrete pits, the pits are opposite to the columnar structures in position and have a similar size, the surface outside the plurality of discrete pits forms a second pattern surface, a solution of a hydrophobic substance is coated on the second pattern surface, and a second pattern is formed on the substrate by an imprinting process; The second pattern is located outside the first pattern and matches the edge of the first pattern; 4) depositing a quantum dot solution on the surface of the first pattern, wherein the surface of the quantum dots in the quantum dot solution has a hydrophilic group; There is no particular order between step 2) and step 3).
2. The method for preparing a quantum dot pattern based on surface pretreatment according to claim 1, characterized in that: The quantum dots in the quantum dot solution are red quantum dots or green quantum dots.
3. The method for preparing a quantum dot pattern based on surface pretreatment according to claim 1, characterized in that: The quantum dot solution is deposited on the first pattern by an inkjet printing process.
4. The method for preparing a quantum dot pattern based on surface pretreatment according to claim 1, characterized in that: The hydrophilic substance includes one of polyvinyl alcohol, polyether polyol and polyacrylic acid.