Perovskite film modified by organic small molecule compound interface, preparation method thereof and solar cell
By spin-coating an acetophenone solution on a CH3NH3PbI3 film for annealing, the problem of insufficient surface lead atom coordination and moisture sensitivity in perovskite solar cells is solved, the photoelectric conversion efficiency and stability are improved, and a more efficient calcium Titanium solar cell performance.
Patent Information
- Application Number
- CN202210343297.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-03-31
AI Technical Summary
During the preparation and use of CH3NH3PbI3 films, there are problems such as insufficient coordination of lead atoms on the surface and sensitivity to moisture, resulting in poor photoelectric conversion efficiency and stability of perovskite solar cells.
The organic small molecule compound acetophenone is used to modify the perovskite film, and the acetophenone solution is spin-coated on the CH3NH3PbI3 film for annealing treatment to passivate uncoordinated Pb2+ and block moisture penetration, improving the structure and stability of the film.
It improves the photoelectric conversion efficiency and stability of perovskite solar cells, enhances the crystallinity and chemical stability of the film, and extends the service life of the battery.
Smart Images

Figure CN114784191B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cell preparation, and specifically relates to a method for preparing a perovskite light absorption layer modified with an organic small molecule compound interface, and in particular to the interface engineering of a light absorption layer / hole transport layer of a perovskite solar cell. Background Art
[0002] Solar energy is an excellent new type of renewable energy. Solar energy is widely distributed, inexhaustible, easy to obtain, low in pollution, and sustainable. It is believed that it will replace traditional fossil energy in the future, alleviate serious energy crises and environmental pollution problems, and has great potential in promoting the transformation of the energy structure of human society and achieving sustainable development of human society. Solar cells can directly convert solar energy into electrical energy and realize the effective utilization of solar energy, becoming a new energy conversion technology that has attracted much attention in recent years. Since the advent of solar cells in the 1950s, current solar cells can be divided into three generations: the first generation of solar cells represented by crystalline silicon solar cells, a series of second generation solar cells represented by cadmium telluride (CdTe) and copper indium gallium selenide (CIGS) thin film solar cells, and the third generation of solar cells represented by dye-sensitized solar cells, perovskite solar cells, and organic solar cells. At present, the highest photoelectric conversion efficiency of perovskite solar cells has reached 25.5%. Perovskite solar cells have attracted much attention for their high photoelectric conversion efficiency, simple and diverse preparation methods, relatively low preparation costs, and wide range of applications, and have broad development prospects. CH3NH3PbI3 perovskite material is a direct bandgap semiconductor material with a bandgap of about 1.55eV. It has the characteristics of high absorption coefficient, small exciton binding energy, high carrier mobility, long carrier diffusion length, and bipolar carrier transmission. It is widely used in the preparation of light absorption layer of perovskite solar cells. However, there are the following problems in the preparation and use of CH3NH3PbI3 film: ① The methylamine ions and iodine ions on the surface of CH3NH3PbI3 film will volatilize during the annealing process, resulting in insufficient coordination of surface lead atoms on the surface of CH3NH3PbI3 film, forming uncoordinated Pb 2+ The uncoordinated Pb on the film surface 2+ It is a deep energy level defect that acts as a non-radiative recombination center at the interface of the perovskite light absorption layer / hole transport layer in perovskite solar cells to capture photogenerated carriers. The carriers captured by the defect will cause charge accumulation at the interface, leading to charge recombination and band bending at the interface, thereby changing the energy level arrangement at the interface, affecting the extraction and transmission of carriers at the interface, and making the photoelectric conversion efficiency and stability of the device worse. ②CH3NH3PbI3 film is very sensitive to moisture in the environment. Moisture infiltrates into the CH3NH3PbI3 film and reacts with methylamine ions CH3NH3+ The formation of hydrogen bonds interrupts the bonding between the methylamine ion and the [PbI6] octahedron, destroys the perovskite structure, accelerates the deprotonation process of CH3NH3PbI3, causes the degradation of the CH3NH3PbI3 film, and affects the stability of the CH3NH3PbI3-based perovskite solar cells. Summary of the invention
[0003] The purpose of the present invention is to provide a perovskite film modified with an organic small molecule compound surface, a preparation method thereof and a solar cell, which can improve the quality of the perovskite film and improve the performance of the perovskite solar cell. The core of the method is a preparation method of a perovskite film modified with an organic small molecule compound surface and based on SnO2. The perovskite film prepared by the method can be applied to solar cells to effectively improve the efficiency and stability of the device and promote its commercialization process.
[0004] The technical solution of the present invention is:
[0005] A perovskite film modified with an organic small molecule compound surface, wherein the film is based on a planar structure SnO2, a CH3NH3PbI3 film is prepared on the substrate, and then acetophenone is spin-coated on the CH3NH3PbI3 film.
[0006] The preparation method thereof comprises:
[0007] (1) The conductive glass is ultrasonically treated with acetone, anhydrous ethanol, and deionized water, respectively, and then dried and treated with ultraviolet ozone, and then a SnO2 colloidal dispersion is spin-coated onto the treated conductive glass, and annealed to obtain a conductive glass / SnO2 film;
[0008] (2) preparing a CH3NH3PbI3 thin film on a conductive glass / SnO2 thin film by a two-step method to obtain a conductive glass / SnO2 / CH3NH3PbI3 thin film;
[0009] (3) dissolving acetophenone in isopropanol and stirring at room temperature until completely dissolved to obtain an acetophenone solution; spin coating the acetophenone solution on the conductive glass / SnO2 / CH3NH3PbI3 film prepared in step (2), and annealing at a certain temperature to obtain a conductive glass / SnO2 / CH3NH3PbI3 / acetophenone film.
[0010] In the above technical solution, the mass concentration of the acetophenone solution is 2-10 mg / mL.
[0011] Furthermore, the acetophenone solution in step (3) is spin-coated at a speed of 2000 to 5000 rpm, and the spin-coating time is 20 to 40 s.
[0012] Furthermore, in step (3), the annealing temperature is 90-120° C., and the annealing time is 1-3 min.
[0013] Furthermore, the mass percentage concentration of the SnO2 colloidal dispersion described in step (1) is 1wt% to 5wt%, the spin coating speed is 2000 to 5000 r / min, the spin coating time is 10s to 60s, the process is repeated 4 to 8 times, the annealing temperature is 100 to 200°C, and the annealing time is 20 to 60min.
[0014] Furthermore, the two-step method for preparing CH3NH3PbI3 thin film is as follows:
[0015] 1) PbI2 is dissolved in a mixed solvent of dimethyl sulfoxide (DMSO) and N,N-dimethylformamide (DMF), and heated and stirred until completely dissolved. The solution is then filtered with a polytetrafluoroethylene filter to obtain a PbI2 precursor solution. The PbI2 precursor solution is spin-coated onto a conductive glass / SnO2 film treated with UV ozone, and a conductive glass / SnO2 / PbI2 film is obtained after annealing;
[0016] 2) Weigh methylammonium iodide and dissolve it in isopropanol, stir until completely dissolved, and obtain a methylammonium iodide solution with a mass concentration of 5-10 mg / mL. Immerse the obtained conductive glass / SnO2 / PbI2 film in the methylammonium iodide solution for 1-5 minutes. Take out the immersed film, wash it in isopropanol, take out the film, remove the excess isopropanol, and anneal it at 80-110°C for 1-10 minutes to obtain a conductive glass / SnO2 / CH3NH3PbI3 film.
[0017] Furthermore, in step 1), the concentration of the PbI2 precursor solution is 0.5-1.5 mol / L, the volume ratio of dimethyl sulfoxide and N,N-dimethylformamide is 1:7-1:11, the stirring heating temperature is 50°C-100°C, the stirring time is 10-60 min, the spin coating volume of the PbI2 precursor solution is 130-180 μL, the spin coating speed is 2000-5000 rpm, and the spin coating time is 20-60 s; the annealing temperature is 50-80°C, and the annealing time is 10-60 min.
[0018] A perovskite solar cell is prepared by spin coating a spiro-OMeTAD solution on a conductive glass / SnO2 / CH3NH3PbI3 / acetophenone film prepared by the above method to prepare a hole transport layer, thereby obtaining a conductive glass / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD film, and finally vacuum evaporating a layer of Au counter electrode on the conductive glass / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD film to obtain a perovskite solar cell device.
[0019] According to a specific example of the present invention, a method for preparing a solar cell of the present invention may include the following steps:
[0020] (1) The FTO conductive glass was ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 20 minutes, dried in a vacuum drying oven, and then treated in a UV ozone cleaning machine for 30 minutes. A SnO2 colloidal dispersion with a volume of 100 to 200 μL and a mass percentage concentration of 1wt% to 5wt% was spin-coated on the FTO conductive glass treated with UV ozone, and the spin coating was performed at a speed of 2000 to 5000 rpm for 10 to 60 seconds. The process was repeated 4 to 8 times. Then, it was placed on a constant temperature heating table and annealed at 100 to 200°C for 20 to 60 minutes to obtain a SnO2 film (FTO / SnO2 film) with the FTO conductive glass as the substrate.
[0021] (2) Weigh an appropriate amount of PbI2 and dissolve it in a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide in a volume ratio of 1:7 to 1:11, and use a constant temperature heating magnetic stirrer to heat and stir at 50 to 100°C for 10 to 60 minutes until it is completely dissolved. Then filter the solution with a polytetrafluoroethylene filter to obtain a PbI2 precursor solution with a molar concentration of 0.5 to 1.5 mol / L. Treat the FTO / SnO2 film prepared in step (1) in a UV ozone cleaning machine for 30 minutes. Spin-coat a volume of 130 to 180 μL of PbI2 solution onto the FTO / SnO2 film treated with UV ozone at a spin-coating speed of 2000 to 5000 rpm and a spin-coating time of 20 to 60 seconds. Then anneal at 50 to 80°C for 10 to 60 minutes to obtain a FTO / SnO2 / PbI2 film. Weigh an appropriate amount of methylammonium iodide and dissolve it in isopropanol. Stir it with a magnetic stirrer at 20-40°C for 20-60 minutes until it is completely dissolved to obtain a methylammonium iodide solution with a mass concentration of 5-10 mg / mL. Immerse the FTO / SnO2 / PbI2 film in the methylammonium iodide solution for 1-5 minutes. Take out the immersed film and wash it in isopropanol for 10-60 seconds. After washing, take out the film and dry the excess isopropanol. Then use a constant temperature heating table to anneal the film at 80-110°C for 1-10 minutes to obtain a FTO / SnO2 / CH3NH3PbI3 film.
[0022] (3) Dissolve an appropriate amount of acetophenone liquid in a certain volume of isopropanol, stir with a magnetic stirrer at 20-30°C for 20-60 min until completely dissolved, and obtain an acetophenone solution with a concentration of 2-10 mg / mL. Use a pipette to transfer 100-200 μL of acetophenone solution to the FTO / SnO2 / CH3NH3PbI3 film prepared in step (2) at a spin coating speed of 2000-5000 rpm and a spin coating time of 20-40 s. Subsequently, place the film on a constant temperature heating table and anneal at 90-120°C for 1-3 min to obtain a FTO / SnO2 / CH3NH3PbI3 / acetophenone film.
[0023] (4) Spin coat 50 μL of spiro-OMeTAD cobalt-based spin coating liquid on the FTO / SnO2 / CH3NH3PbI3 / acetophenone film prepared in step (3) at a spin coating speed of 3000 rpm for 30 s to obtain a cobalt-doped spiro-OMeTAD hole transport layer with the FTO / SnO2 / CH3NH3PbI3 / acetophenone film as the substrate.
[0024] (5) In high vacuum (5×10 -5 Under conditions of 240 Pa, a 80 nm thick layer of gold (Au) was evaporated on the FTO / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD substrate as a counter electrode to obtain a perovskite solar cell with a FTO / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD / Au structure.
[0025] In step (2) of the present invention, the acetophenone, Standard for GC, is ≥99.5% (GC).
[0026] The specifications of the above-mentioned FTO conductive glass are 20mm*25mm, the square resistance is 14Ω, and the transmittance is ≥90%.
[0027] Uncoordinated Pb in CH3NH3PbI3 thin films 2+ It can be regarded as a Lewis acid, which contains an unfilled p orbital and can be passivated by introducing Lewis base modifiers containing electron donor elements O, P, N, and S with lone pairs of electrons. Acetophenone contains a carbonyl group (C=O) and can be regarded as a Lewis base. Through the Lewis acid-base reaction, it can passivate the positive charge defects caused by insufficient coordination of Pb atoms, reduce the defect state density at the interface, inhibit the non-radiative recombination of the interface, improve the carrier transport kinetics at the interface, and obtain higher efficiency. In addition, acetophenone contains a benzene ring. The π-conjugated structure of the benzene ring can promote charge transfer inside the battery, and the hydrophobicity of the benzene ring can prevent moisture in the environment from penetrating into the perovskite, which is beneficial to improve the stability of the device.
[0028] The beneficial effects of the present invention are:
[0029] The present invention spin-coats acetophenone on the CH3NH3PbI3 / spiro-OMeTAD interface. The introduction of the organic small molecule compound acetophenone can give the uncoordinated Pb 2+ Provide lone pair electrons through acetophenone to uncoordinated Pb 2+ The Lewis acid-base reaction between the two can passivate the defects. The benzene ring in acetophenone can promote the charge transfer inside the battery and improve the device performance; at the same time, the hydrophobic benzene ring can block the water in the environment from penetrating into the perovskite, prevent the degradation of the perovskite, and improve the stability of the device. The research results show that the modification of the CH3NH3PbI3 / spiro-OMeTAD interface by acetophenone improves the morphology, structure, optical properties, stability of the CH3NH3PbI3 film and the performance of the corresponding solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Field emission scanning electron microscopy images of perovskite films: (a) unmodified CH3NH3PbI3 film; (b) acetophenone-modified CH3NH3PbI3 film.
[0031] Figure 2 X-ray diffraction patterns of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film.
[0032] Figure 3 UV-visible absorption spectra of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film.
[0033] Figure 4 Fluorescence spectra of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film.
[0034] Figure 5 The chemical stabilities of unmodified CH3NH3PbI3 perovskite films and acetophenone-modified CH3NH3PbI3 perovskite films stored in air for 0 to 300 h, respectively.
[0035] Figure 6 The efficiency changes of unmodified and acetophenone-modified perovskite solar cells placed in air conditions for 0-42 days.
[0036] Figure 7 JV characteristic curves of unmodified and acetophenone-modified perovskite solar cells.
[0037] Figure 8Figure 2 shows the monochromatic light conversion efficiency (IPCE) of unmodified and acetophenone-modified perovskite solar cells. DETAILED DESCRIPTION
[0038] The present invention will be described in detail below with reference to specific embodiments.
[0039] Example 1
[0040] (1) The FTO conductive glass was ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 20 minutes, then dried in a vacuum drying oven, and then treated in a UV-ozone cleaning machine for 30 minutes. A 120 μL SnO2 hydrocolloid dispersion with a mass percentage concentration of 1.5 wt% was spin-coated on the FTO conductive glass treated with UV-ozone at a speed of 2500 rpm for 20 seconds. The process was repeated 4 times, and then annealed at 100°C for 25 minutes to obtain a SnO2 film (FTO / SnO2 film) with the FTO conductive glass as the substrate.
[0041] (2) Dissolve an appropriate amount of PbI2 in a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide in a volume ratio of 1:9, heat and stir at 70°C for 25 minutes using a constant temperature heating magnetic stirrer until completely dissolved, and then filter the solution using a polytetrafluoroethylene filter to obtain a PbI2 precursor solution with a molar concentration of 0.5 mol / L. Treat the FTO / SnO2 film prepared in step (1) in a UV-ozone cleaning machine for 30 minutes. Spin coat 120 μL of the PbI2 precursor solution on the FTO / SnO2 film treated with UV-ozone at a spin coating speed of 2500 rpm for 40 seconds. Then anneal at 70°C for 30 minutes to obtain a FTO / SnO2 / PbI2 film. Weigh an appropriate amount of methylammonium iodide and dissolve it in a certain volume of isopropanol. Stir magnetically at 25°C for 25 minutes to obtain a methylammonium iodide solution with a mass concentration of 7 mg / mL. The FTO / SnO2 / PbI2 film was immersed in methylammonium iodide solution for 2 minutes, and the immersed film was taken out and washed in isopropanol for 20 seconds. After washing, the film was taken out and the excess isopropanol was dried. Then, the film was annealed at 95°C for 5 minutes using a constant temperature heating table to obtain a FTO / SnO2 / CH3NH3PbI3 film.
[0042] (3) Dissolve an appropriate amount of acetophenone in a certain volume of isopropanol, stir magnetically for 25 min at 25°C until completely dissolved, and prepare an acetophenone solution with a mass concentration of 4 mg / mL. Take 120 μL of the acetophenone solution and spin coat it on the FTO / SnO2 / CH3NH3PbI3 film at a spin coating speed of 2500 rpm for 30 s. Then anneal at 110°C on a constant temperature heating table for 3 min to obtain the FTO / SnO2 / CH3NH3PbI3 / acetophenone film.
[0043] (4) Spin coat 50 μL of spiro-OMeTAD cobalt-based spin coating liquid on the FTO / SnO2 / CH3NH3PbI3 / acetophenone film prepared in step (3) at a spin coating speed of 3000 rpm for 30 s to obtain a cobalt-doped spiro-OMeTAD hole transport layer with the FTO / SnO2 / CH3NH3PbI3 / acetophenone film as the substrate.
[0044] (5) In high vacuum (5×10 -5 Under conditions of 240 Pa, a 80 nm thick layer of gold (Au) was evaporated on the FTO / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD substrate as a counter electrode to obtain a perovskite solar cell with a FTO / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD / Au structure.
[0045] The present invention will be specifically described below in conjunction with the accompanying drawings:
[0046] Attached Figure 1 The following are field emission scanning electron microscope images of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film. As can be seen from the figure, the unmodified CH3NH3PbI3 perovskite film has many holes, poor film coverage, uneven grain size, an average grain size of about 185.60nm, and poor crystallinity; the acetophenone-modified CH3NH3PbI3 perovskite film has fewer pinholes on the surface, the film is more dense, the grain size is more uniform, the average grain size increases to 219.86nm, and the crystallinity is improved. The dense film with few pinholes can prevent the hole transport layer from directly contacting the electron transport layer, avoiding short circuits, which is beneficial to improving the performance of perovskite solar cells.
[0047] Attached Figure 2 The X-ray diffraction patterns of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film. Figure 2It can be seen that after acetophenone modification, the diffraction peak intensity corresponding to CH3NH3PbI3 increases slightly, and the position of the diffraction peak does not change, indicating that acetophenone modification does not change the structure of the CH3NH3PbI3 film, and the crystallinity of the CH3NH3PbI3 film is improved. In addition, after acetophenone modification, a very small PbI2 diffraction peak appears in the CH3NH3PbI3 / acetophenone film, indicating that a small amount of PbI2 appears, which is beneficial to passivate the defects on the surface of the CH3NH3PbI3 film. The above results show that the crystallization performance of the CH3NH3PbI3 film modified with acetophenone is improved, the film quality is improved, and it is beneficial to improve the optoelectronic performance of the device.
[0048] Attached Figure 3 The UV-visible absorption spectra of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film are shown in Figure 2. The results show that acetophenone modification can increase the absorbance of CH3NH3PbI3 perovskite film in the wavelength range of 600nm-900nm, and red-shift the absorption edge of the film, thereby improving the light absorption performance of CH3NH3PbI3 perovskite film.
[0049] Attached Figure 4 The fluorescence spectra (PL) of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film are shown in the figure. As can be seen from the figure, after acetophenone modification, the PL intensity of the CH3NH3PbI3 perovskite film is significantly enhanced, indicating that the defect concentration of the CH3NH3PbI3 perovskite film after acetophenone modification is reduced, and the film quality is improved, which is conducive to the preparation of stable and efficient perovskite solar cells.
[0050] Attached Figure 5 The X-ray diffraction patterns of unmodified CH3NH3PbI3 perovskite film and acetophenone-modified CH3NH3PbI3 perovskite film placed in air for 0h and 300h. Figure 5 It can be seen that at 0h, the diffraction peak intensity of the CH3NH3PbI3 perovskite film modified with acetophenone and the unmodified CH3NH3PbI3 perovskite film is comparable, but after being placed in the air for 300h, it can be clearly observed that the CH3NH3PbI3 diffraction peak intensity corresponding to the unmodified CH3NH3PbI3 perovskite film sample has decreased significantly, while the diffraction peak intensity of the CH3NH3PbI3 perovskite film sample modified with acetophenone remains basically unchanged. The above results show that acetophenone modification of CH3NH3PbI3 perovskite film can effectively prevent moisture in the air from penetrating into the perovskite, inhibit the degradation of the perovskite film, and improve the stability of the perovskite film.
[0051] Attached Figure 6The efficiency change diagram of unmodified CH3NH3PbI3 perovskite solar cells and acetophenone-modified CH3NH3PbI3 perovskite solar cells placed in air for 0-42 days. As can be seen from the figure, the efficiency of the unmodified CH3NH3PbI3 perovskite solar cell drops to 0 after 24 days in the air; while the CH3NH3PbI3 perovskite solar cell modified with acetophenone can still maintain about 72% of the initial efficiency after 45 days under the same conditions. The above results show that after acetophenone modification, the stability of CH3NH3PbI3 perovskite solar cells is significantly improved, indicating that acetophenone modification can effectively inhibit moisture infiltration, delay the perovskite degradation process caused by moisture, and improve the air stability of the device.
[0052] Attached Figure 7 The JV curves of unmodified CH3NH3PbI3 perovskite solar cells and acetophenone-modified CH3NH3PbI3 perovskite solar cells are shown in Table 1. Figure 7 Related perovskite solar cell performance parameter table. Figure 7 As shown in Table 1, after the perovskite light absorption layer / hole transport layer interface of the perovskite solar cell was modified with acetophenone, the performance parameters of the corresponding device were improved. After acetophenone modification, the photoelectric conversion efficiency of the perovskite solar cell increased from 8.13% to 11.85%, the open circuit voltage increased from 0.99V to 1.07V, and the short circuit current increased from 11.50mA·cm -2 Increased to 15.21 mA cm -2 , the filling factor is increased from 0.72 to 0.73. Compared with the unmodified CH3NH3PbI3 perovskite solar cell, the efficiency of the CH3NH3PbI3 perovskite solar cell modified with acetophenone is increased by 45.76%.
[0053] Table 1 Photovoltaic parameters of perovskite solar cells
[0054] sample <![CDATA[V OC (V)]]> <![CDATA[J SC (mA cm -2 )]]> FF(%) PCE(%) <![CDATA[SnO2 / CH3NH3PbI3]]> 0.99 11.50 0.72 8.13 <![CDATA[SnO2 / CH3NH3PbI3 / acetophenone]]> 1.07 15.21 0.73 11.85
[0055] Attached Figure 8 The monochromatic photoelectric conversion efficiency (IPCE) of unmodified CH3NH3PbI3 perovskite solar cells and acetophenone-modified CH3NH3PbI3 perovskite solar cells is shown in the figure. As can be seen from the figure, at 460nm, the unmodified CH3NH3PbI3 perovskite solar cells and acetophenone-modified CH3NH3PbI3 perovskite solar cells reach the maximum IPCE values of 68.21% and 77.66%, respectively, and the corresponding integrated currents are 13.74mA / cm 2 and 16.29mA / cm 2After acetophenone modification, the IPCE value of CH3NH3PbI3 perovskite solar cells increased significantly, indicating that the modified devices achieved more efficient photoelectric conversion. The results were consistent with the JV test results, indicating that acetophenone modification is conducive to the preparation of efficient perovskite solar cells.
[0056] The present invention modifies the CH3NH3PbI3 / spiro-OMeTAD interface by acetophenone to passivate the uncoordinated Pb generated in the preparation process of the CH3NH3PbI3 film. 2+ , reducing the defect density of CH3NH3PbI3 perovskite film and improving the film quality; and by modifying the surface of CH3NH3PbI3 film with acetophenone, it is possible to block the penetration of moisture in the air, inhibit the decomposition of the perovskite film, and improve the stability of the perovskite film, thereby preparing efficient and stable perovskite solar cells.
[0057] Example 2
[0058] (1) The FTO conductive glass was ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 20 minutes, then dried in a vacuum drying oven, and then treated in a UV ozone cleaning machine for 30 minutes. A 200 μL SnO2 hydrocolloid dispersion with a mass percentage concentration of 4wt% was spin-coated on the FTO conductive glass treated with UV ozone at a speed of 4000 rpm for 40 seconds. The process was repeated 6 times, and then annealed at 170°C for 45 minutes to obtain a SnO2 film (FTO / SnO2 film) with FTO conductive glass as the substrate. (2) An appropriate amount of PbI2 was dissolved in a mixed solvent of dimethyl sulfoxide (DMSO) and N,N-dimethylformamide (DMF) with a volume ratio of 1:11, and heated and stirred at 80°C for 50 minutes using a constant temperature heating magnetic stirrer until completely dissolved, and then the solution was filtered using a polytetrafluoroethylene filter to obtain a PbI2 precursor solution with a molar concentration of 1.2 mol / L. Treat the FTO / SnO2 film prepared in step (1) in a UV-ozone cleaning machine for 30 minutes. Spin-coat 160 μL of PbI2 precursor solution on the UV-ozone treated FTO / SnO2 film at a speed of 3500 rpm for 30 seconds. Then anneal at 80°C for 20 minutes to obtain a FTO / SnO2 / PbI2 film. Weigh an appropriate amount of methylammonium iodide and dissolve it in a certain volume of isopropanol. Stir magnetically at 20°C for 25 minutes to obtain a methylammonium iodide solution with a mass concentration of 10 mg / mL. The FTO / SnO2 / PbI2 film was immersed in methylammonium iodide solution for 5 minutes, and the immersed film was taken out and washed in isopropanol for 40 seconds. After washing, the film was taken out and the excess isopropanol was dried. Then, the film was annealed at 100°C for 10 minutes using a constant temperature heating table to obtain a FTO / SnO2 / CH3NH3PbI3 film.
[0059] (3) Dissolve an appropriate amount of acetophenone in a certain volume of isopropanol, stir magnetically at 30°C for 45 min until completely dissolved, and prepare an acetophenone solution with a mass concentration of 8 mg / mL. Take 180 μL of the acetophenone solution and spin coat it on the FTO / SnO2 / CH3NH3PbI3 film at a spin coating speed of 5000 rpm for 35 s. Then anneal at 120°C on a constant temperature heating table for 2 min to obtain the FTO / SnO2 / CH3NH3PbI3 / acetophenone film.
[0060] (4) Spin coat 50 μL of spiro-OMeTAD cobalt-based spin coating liquid on the FTO / SnO2 / CH3NH3PbI3 / acetophenone film prepared in step (3) at a spin coating speed of 3000 rpm for 30 s to obtain a cobalt-doped spiro-OMeTAD hole transport layer with the FTO / SnO2 / CH3NH3PbI3 / acetophenone film as the substrate.
[0061] (5) In high vacuum (5×10 -5 Under conditions of 240 Pa, a 80 nm thick layer of gold (Au) was evaporated on the FTO / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD substrate as a counter electrode to obtain a perovskite solar cell with a FTO / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD / Au structure.
Claims
1. A perovskite film modified with an organic small molecule compound interface, characterized in that: The film is based on a planar structure SnO2, a CH3NH3PbI3 film is prepared on the substrate, and then acetophenone is spin-coated on the CH3NH3PbI3 film.
2. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 1, characterized in that: include: (1) The conductive glass is ultrasonically treated with acetone, anhydrous ethanol, and deionized water, respectively, and then dried and cleaned with ultraviolet ozone, and then a SnO2 colloidal dispersion is spin-coated onto the treated conductive glass, and annealed to obtain a conductive glass / SnO2 film; (2) preparing a CH3NH3PbI3 thin film on a conductive glass / SnO2 thin film by a two-step method to obtain a conductive glass / SnO2 / CH3NH3PbI3 thin film; (3) dissolving acetophenone in isopropanol and stirring at room temperature until completely dissolved to obtain an acetophenone solution; spin coating the acetophenone solution on the conductive glass / SnO2 / CH3NH3PbI3 film prepared in step (2), and annealing at a certain temperature to obtain a conductive glass / SnO2 / CH3NH3PbI3 / acetophenone film.
3. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 2, characterized in that: The mass concentration of the acetophenone solution described in step (3) is 2-10 mg / mL.
4. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 2, characterized in that: The acetophenone solution described in step (3) is spin-coated at a speed of 2000 to 5000 rpm, and the spin-coating time is 20 to 40 seconds.
5. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 2, characterized in that: In step (3), the annealing temperature is 90-120° C. and the annealing time is 1-3 min.
6. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 2, characterized in that: The mass percentage concentration of the SnO2 colloidal dispersion described in step (1) is 1wt% to 5wt%, the spin coating speed is 2000 to 5000r / min, the spin coating time is 10s to 60s, the spin coating process is repeated 4 to 8 times, the annealing temperature is 100 to 200°C, and the annealing time is 20 to 60min.
7. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 2, characterized in that: The two-step method for preparing CH3NH3PbI3 thin film is as follows: 1) PbI2 is dissolved in a mixed solvent of dimethyl sulfoxide (DMSO) and N,N-dimethylformamide (DMF), heated and stirred until completely dissolved, and then the solution is filtered through a polytetrafluoroethylene filter to obtain a PbI2 precursor solution, and the PbI2 precursor solution is spin-coated onto a conductive glass / SnO2 film treated with ultraviolet ozone, and annealed to obtain a conductive glass / SnO2 / PbI2 film; 2) Weigh methylammonium iodide and dissolve it in isopropanol, stir until completely dissolved, and obtain a mass concentration of 5-10 The conductive glass / SnO2 / PbI2 film is immersed in the methylammonium iodide solution of 1 mg / mL for 1 to 5 minutes, the immersed film is taken out and washed in isopropanol, the excess isopropanol is removed, and the film is annealed at 80 to 110°C for 1 to 10 minutes to obtain a conductive glass / SnO2 / CH3NH3PbI3 film.
8. The method for preparing a perovskite film modified with an organic small molecule compound interface according to claim 7, characterized in that: In step 1), the concentration of the PbI2 precursor solution is 0.5-1.5 mol / L, the volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 1:7-1:11, and the stirring and heating temperature is 50°C- 100°C, stirring time is 10-60min, the spin coating volume of PbI2 precursor solution is 130-180μL, the spin coating speed is 2000-5000rpm, and the spin coating time is 20-60s; the annealing temperature is 50-80°C, and the annealing time is 10-60min.
9. A perovskite solar cell, characterized in that: A hole transport layer is prepared by spin coating a spiro-OMeTAD solution on the conductive glass / SnO2 / CH3NH3PbI3 / acetophenone film prepared by the method as described in any one of claims 2 to 8 to obtain a conductive glass / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD film, and finally a layer of Au counter electrode is vacuum evaporated on the conductive glass / SnO2 / CH3NH3PbI3 / acetophenone / spiro-OMeTAD film to obtain a perovskite solar cell device.
10. A perovskite solar cell according to claim 9, characterized in that: In the solar cell, acetophenone modification is used to reduce the defect state density at the CH3NH3PbI3 / spiro-OMeTAD interface, inhibiting interface non-radiative recombination, while utilizing the π-conjugated structure of the benzene ring in acetophenone to promote charge transfer within the battery, and the hydrophobicity of the benzene ring blocks the penetration of moisture in the environment into the perovskite CH3NH3PbI3, thereby improving stability.