Wide bandgap perovskite solar cell with high stability and preparation method thereof
By heating the DMF solvent to flush the PTAA layer and using halogen-like anions instead of halogen ions, the problem of holes and halogen separation in the perovskite film in perovskite solar cells is solved, the conversion efficiency and stability of the device are improved, and efficient perovskite is achieved Mineral solar cell preparation.
Patent Information
- Application Number
- CN202210414778.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-04-20
AI Technical Summary
Wide-bandgap perovskite solar cells have problems such as large deviations between open circuit voltage and band gap, low photoelectric conversion efficiency, and poor stability. Especially in humid environments, ion defects in perovskite materials lead to insufficient charge extraction and halogen separation, affecting the device. performance.
By heating the N,N-dimethylformamide (DMF) solvent to rinse the hole transport layer (PTAA) film, improve its contact with the perovskite precursor solution, and use halogen-like anions (such as BF4-, PF6-) replaces part of the halide ions, increases the stability of the perovskite film, and prepares devices by combining spin coating and thermal evaporation methods.
It improves the conversion efficiency and stability of perovskite solar cells, reduces halogen decomposition, enhances device repeatability and performance, and achieves efficient perovskite film deposition and charge transport.
Smart Images

Figure CN114784192B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silicon-perovskite stacked solar cell, in particular to a wide bandgap perovskite solar cell with high stability and a preparation method thereof. Background Art
[0002] At present, the conversion efficiency of single-junction perovskite solar cells has reached 25.7%. The flexible and adjustable bandgap width of perovskite materials and the simple low-temperature solution preparation process make them ideal candidate materials for manufacturing multi-junction stacked solar cells. The development of wide-bandgap perovskite solar cells (PSCs) is imperative.
[0003] At present, wide bandgap perovskite cells generally have problems such as large deviation between open circuit voltage (Voc) and bandgap (Eg) and low photoelectric conversion efficiency. In addition, perovskite cells also face stability challenges. Halogen separation is prone to occur under light, heat, water, oxygen, etc., especially the phase instability of wide bandgap perovskite cells is particularly prominent. Perovskite materials have some ion defects, which can be transferred to the interface between perovskite and other contact layers, inhibiting the effective extraction of charge. Moreover, these ion defects are also very sensitive to humidity. In a humid environment, the performance of PSCs decays quickly.
[0004] In inverted PSCs, the hole transport layer (HTL) not only acts as a charge carrier extraction layer, but also has a significant impact on the crystallization and film formation of perovskite. It is crucial to optimize the HTL to improve its contact with the perovskite layer. Currently, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine](PTAA) has become one of the most widely used hole transport materials (HTMs) in inverted devices due to its high hole mobility, good corrosion resistance to precursor solvents (such as N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO)), and energy level matching with the perovskite layer.
[0005] Due to the non-wettability of the PTAA film surface, the adhesion of the perovskite precursor solution during the deposition process is small, and the contact between the PTAA film and the perovskite precursor solution is very poor, so that the perovskite precursor solution cannot completely cover the PTAA film during the spin coating process. At the same time, the perovskite film produces more holes, wasting a large amount of perovskite precursor solution. These factors directly affect the conversion efficiency and stability of perovskite solar devices. In order to solve this problem, researchers have adopted various methods. It is currently known to directly treat the PTAA film with ultraviolet ozone (UVO) to change its chemical structure. However, this method has many influencing factors (such as plasma power and processing time), which reduces the repeatability of the device and increases the manufacturing difficulty of the perovskite solar cell industry. In addition, washing the PTAA film with chlorobenzene (CB) solution is also a method to reduce the non-wettability of PTAA. Although this method solves the hole problem of the perovskite film, the PTAA solution is dissolved in CB as a solvent. Using CB for washing reduces the effective adhesion of PTAA on ITO conductive glass and affects its hole mobility.
[0006] Therefore, it is urgent to explore a facile and cost-effective method to optimize PTAA to achieve both high efficiency and reproducibility of PSCs. It is also necessary to find an efficient and feasible additive to reduce the halogen decomposition of perovskite and increase device efficiency. Summary of the invention
[0007] The purpose of the present invention is to provide a wide bandgap perovskite solar cell with high stability and a preparation method thereof, so as to optimize PTAA and improve the hole problem of the perovskite film; at the same time, it can effectively reduce the decomposition of perovskite halogen and improve the battery conversion efficiency.
[0008] The present invention is implemented as follows: the present invention improves the problem of poor contact between the PTAA layer and the perovskite precursor solution by washing the PTAA film with heated DMF solvent, and solves the problem of halogen instability in wide-bandgap perovskite by adding halogen-like additives, thereby preparing an efficient, stable and repeatable perovskite solar cell device.
[0009] When optimizing the PTAA layer, DMF is used for washing. Since the polarity of the DMF solution is relatively large, the perovskite film obtained by washing the PTAA film at room temperature and spin coating the perovskite film on this basis still has many problems. Therefore, the present invention uses a heating method to improve the polarity of the DMF solution, thereby solving the wettability of the PTAA film and the hole problem on the surface of the perovskite film.
[0010] Halide-like elements have similar chemical properties and ionic radius to halides, and can effectively replace some halogen ions, thereby increasing the stability of wide-bandgap perovskite films, effectively reducing the halogen separation of perovskite devices, and greatly improving the performance and stability of the devices, providing a more ideal upper absorption material for perovskite-silicon tandem solar cells.
[0011] The final device includes, from bottom to top, ITO conductive glass, a washed hole transport layer (i.e., the hole transport layer is washed with DMF), a perovskite film, an electron transport layer, a blocking layer, and a metal electrode.
[0012] The hole transport layer, DMF washing, perovskite film, electron transport layer and barrier layer were all prepared by spin coating.
[0013] The metal electrodes were prepared by thermal evaporation.
[0014] The selected system is FA with a band gap of 1.67 eV 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 Wide bandgap perovskite, the specific preparation process of each layer is as follows:
[0015] a. Hole transport layer: Dissolve poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) powder in chlorobenzene solution, and use spin coating to spin coat the completely dissolved PTAA solution on the conductive glass ITO, and anneal on a heating table. The selection of hole transport layer materials must meet the band gap matching of the perovskite film.
[0016] b. DMF washing: Since the polarity of DMF solution is relatively high, DMF is placed on a heating table for heating. The sample obtained in step a is placed on a spin coater for one-step dynamic spin coating.
[0017] c. Perovskite film: Spin-coat the wide bandgap perovskite precursor solution on the sample obtained in step b by spin coating. During spin coating: low speed 1100 rpm, spin coating time 2 s, acceleration 1000 rpm / s; high speed 6000 rpm, spin coating time 30 s, acceleration 2000 rpm / s. Add anti-solvent chlorobenzene solution at high speed 20-25 s, and anneal the perovskite film obtained by spin coating. Annealing obtains a crystallized perovskite film with a thickness of about 400 nm.
[0018] d. Electron transport layer: Dissolve 3'-phenyl-3'H-cyclopropyl[1,9][5,6]fullerene-C60-Ih-3'-butyric acid methyl ester (PCBM) powder in chlorobenzene solution, and filter with a 0.22 μm filter head after fully dissolved. Place the perovskite film sample obtained in step c on a spin coater and statically spin coat the PCBM solution at a speed of 1500 rpm, a spin coating time of 30 s, and an acceleration of 1000 rpm / s.
[0019] e. Barrier layer: Dissolve BCP powder in anhydrous ethanol. Let the sample obtained in step d stand for about 10 minutes, and spin-coat BCP to prevent the metal electrode from reacting with the underlying perovskite film and affecting the device performance.
[0020] f. Metal electrode: A silver metal electrode with a thickness of about 150 nm was prepared by thermal evaporation.
[0021] The present invention provides a method for solving the problems of PTAA wettability and perovskite film holes by heating and washing with a DMF solution, which has the advantages of being simple and easy to implement, having high conversion efficiency, and having good contact with the perovskite precursor solution.
[0022] Halogen-like anion BF4 - PF6 - Acting on this system can greatly improve the conversion efficiency of the basic devices of this system. In addition, the halogen separation and tensile strain of perovskite have been improved.
[0023] The present invention relates to a top cell light-absorbing layer in a silicon-perovskite stacked solar cell, and first solves the non-wetting problem of a hole transport layer in a perovskite device. The present invention selects an N,N-dimethylformamide (DMF) solution to heat and rinse a PTAA film, thereby improving the hole problem of the perovskite film without affecting its hole transport, and achieving high efficiency and repeatability of PSCs. This method is simple, economical, and efficient, and achieves optimization of the PTAA film. A wide-bandgap perovskite precursor solution is deposited on the PTAA film after DMF optimization and rinsing, and the two have good contact, and the holes on the surface of the deposited perovskite film disappear.
[0024] At the same time, in the formed wide bandgap perovskite solar cell device, a halogen-like element with similar chemical properties and ionic radius to the halogen element is found to partially replace the halogen element to solve the problems of halogen separation, tensile strain inside the film, low conversion efficiency, etc. of the existing wide bandgap perovskite solar cells, while providing an ideal upper absorption material for the stacked solar cells.
[0025] The present invention effectively solves the non-wettability of the hole transport layer PTAA film and improves the hole problem of the perovskite film; in addition, the use of halogen-like additives solves the problems of easy decomposition of perovskite halogens, tensile strain inside the film, low conversion efficiency, etc. with the effective action of halogen-like additives. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the device structure of the present invention.
[0027] Figure 2 For the halogen-like anion BF4 - PF6 - structure and working process.
[0028] Figure 3 Field emission scanning electron microscope (SEM) surface morphology and cross-sectional comparison of the basic perovskite film in comparative example 1 and the improved film after adding halogen-like additives in Examples 1 and 2.
[0029] Figure 4 Atomic force microscope (AFM) images of the basic perovskite film in Comparative Example 1 and the improved films after adding halogen-like additives in Examples 1 and 2.
[0030] Figure 5 This is a comparison chart of the changes in PL spectra measured for the basic perovskite film in Comparative Example 1 and the improved films after adding halogen-like additives in Examples 1 and 2 under continuous irradiation of one sun.
[0031] Figure 6 (a) shows the JV curve of the basic device and the device with halogen-like additives, and (b) shows the EQE curve of the basic device and the device with halogen-like additives.
[0032] Figure 7 Water contact angle diagram measured for the base perovskite film and the perovskite film with added halogen-like additives. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0034] Example 1, using halogen-like anion BF4 - Partially replace halogen ions.
[0035] In this example, a high-efficiency and stable wide bandgap perovskite solar cell device was prepared according to the following steps. The selected system was FA with a bandgap of 1.67 eV. 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2)3 Wide bandgap perovskite.
[0036] (1) Cleaning the substrate: The ITO conductive glass was placed in a cleaning solution (commercially available, produced by Liaoning Youxuan New Energy Technology Co., Ltd.), deionized water, acetone, isopropanol and anhydrous ethanol in sequence and ultrasonically cleaned for 20 minutes each, then blown dry with nitrogen, and then placed in an ultraviolet ozone (UVO) instrument for 30 minutes of ultraviolet ozone treatment.
[0037] (2) The ITO conductive glass treated with UV ozone was transferred to a glove box filled with nitrogen. A PTAA solution with a concentration of 5 mg / mL was spin-coated at a speed of 5000 rpm (accelerated at an acceleration of 2500 rpm / s) for 25 s (the 25 s includes the acceleration time, the same below), and the spin-coated film was annealed on a heating table at 100°C for 10 min. After annealing, the film was allowed to stand at room temperature before starting the next step.
[0038] (3) Since the PTAA film is relatively hydrophobic and is not conducive to perovskite spin coating, the sample obtained in step (2) is rinsed with DMF: the DMF solution is heated on a heating table at 100°C for 5 min, 40 μL of the heated DMF solution is aspirated with a pipette, and spin-coated at a speed of 4000 rpm (accelerated at an acceleration of 2000 rpm / s) for 25 s. The DMF solution is dripped at 8 s, thus realizing dynamic spin coating of the DMF solution. This dynamic spin coating process is called DMF rinsing.
[0039] (4) Before starting to spin-coat the perovskite, the glove box was cleaned and the prepared MABF4 wide bandgap perovskite precursor solution was fully dissolved for 12 hours.
[0040] The preparation process of MABF4 wide band gap perovskite precursor solution is as follows: 167.7 mg FAI, 553.2 mg PbI2, 33.6 mg MABr, 110.1 mg PbBr2, 58.5 mg CsI, 24 mg MACl, and 2 mg MABF4 are dissolved in 1 mL of a mixed solution of DMF and DMSO with a volume ratio of 4:1.
[0041] Place the prepared MABF4 wide bandgap perovskite precursor solution with a concentration of 2 mg / mL in a glove box. Pipette 30 μL of the precursor solution onto the sample obtained in step (3), and spin coat it at a low speed of 1100 rpm (accelerated at 1000 rpm / s) for 2 seconds; then spin coat it at a high speed of 6000 rpm (accelerated at 2000 rpm / s) for 30 seconds. At a high speed of 20-25 seconds, add 110 μL of the anti-solvent chlorobenzene solution, and immediately place the spin-coated perovskite film on a 100°C heating table for annealing for 45 minutes to obtain a crystallized perovskite film. After annealing, let it stand at room temperature before starting the next step.
[0042] (5) The filtered PCBM solution was spin-coated on the sample obtained in step (4). The concentration of the solution was 20 mg / mL. The solution was spin-coated at a rotation speed of 1500 rpm (accelerated at an acceleration of 1000 rpm / s) for 30 seconds. The solution was statically spin-coated and then allowed to stand for about 15 minutes.
[0043] (6) Then, the sample obtained in step (5) was spin-coated at 5000 rpm (accelerated at 2000 rpm / s) for 30 s, and 40 μL of BCP solution with anhydrous ethanol as solvent was dynamically spin-coated at 8 s, wherein the concentration of the BCP solution was 0.5 mg / mL.
[0044] (7) Place the sample obtained in step (6) in a vapor deposition mold and perform thermal evaporation of metal electrode Ag in the vapor deposition chamber. Place the Ag particles on a thermal evaporation boat, close the door, and pump the vacuum of the chamber to 6×10 -4 Pa. Adjust the current to 120A and the evaporation rate to When the rate drops to 0, the evaporation ends and a 150 nm thick Ag electrode is obtained.
[0045] The structure of the final prepared sample is as follows Figure 1 shown.
[0046] Example 2, using halogen-like anion PF6 - Partially replace halogen ions.
[0047] In this example, a high-efficiency and stable wide bandgap perovskite solar cell device was prepared according to the following steps. The selected system was FA with a bandgap of 1.67 eV. 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 Wide bandgap perovskite.
[0048] (1) Cleaning the substrate: The ITO conductive glass was placed in a cleaning solution (commercially available), deionized water, acetone, isopropanol, and anhydrous ethanol, respectively, and ultrasonically cleaned for 20 min each. After that, it was blown dry with nitrogen gas and then placed in an ultraviolet ozone (UVO) instrument for 30 min of ultraviolet ozone treatment.
[0049] (2) The ITO conductive glass treated with UV ozone was transferred to a glove box filled with nitrogen. A PTAA solution with a concentration of 5 mg / mL was spin-coated at a speed of 5000 rpm (accelerated at an acceleration of 2500 rpm / s) for 25 s (the 25 s includes the acceleration time, the same below), and the spin-coated film was annealed on a heating table at 100°C for 10 min. After annealing, the film was allowed to stand at room temperature before starting the next step.
[0050] (3) The sample obtained in step (2) is rinsed with DMF: the DMF solution is heated on a heating table at 100°C for 5 min, 40 μL of the heated DMF solution is aspirated with a pipette, and spin-coated at a rotation speed of 4000 rpm (accelerated at an acceleration of 2000 rpm / s) for 25 s. The DMF solution is dripped at 8 s, thus achieving dynamic spin coating of the DMF solution. The dynamic spin coating process is called DMF rinsing.
[0051] (4) Before starting to spin-coat the perovskite, the glove box was cleaned and the prepared MAPF6 wide bandgap perovskite precursor solution was fully dissolved for 12 hours.
[0052] The preparation steps of MAPF6 wide bandgap perovskite precursor solution are as follows: 167.7 mg FAI, 553.2 mg PbI2, 33.6 mg MABr, 110.1 mg PbBr2, 58.5 mg CsI, 24 mg MACl, and 2 mg MAPF6 are dissolved in 1 mL of a mixed solution of DMF and DMSO with a ratio of 4:1.
[0053] Figure 2 For the halogen-like anion BF4 - PF6 - The structure and action process of BF4 - PF6 - Ion substitution I - process.
[0054] Place the prepared MAPF6 wide bandgap perovskite precursor solution with a concentration of 2 mg / mL in the glove box. Pipette 30 μL of the precursor solution and spread it on the sample obtained in step (3), spin-coat it at a low speed of 1100 rpm (accelerated at an acceleration of 1000 rpm / s) for 2 seconds; then spin-coat it at a high speed of 6000 rpm (accelerated at an acceleration of 2000 rpm / s) for 30 seconds. At a high speed of 20-25 seconds, add 110 μL of anti-solvent chlorobenzene solution, and immediately place the spin-coated perovskite film on a 100°C heating table for annealing for 45 minutes to obtain a crystallized perovskite film. After annealing, let it stand at room temperature before starting the next step.
[0055] (5) The filtered PCBM solution was spin-coated on the sample obtained in step (4). The concentration of the solution was 20 mg / mL. The solution was spin-coated at a rotation speed of 1500 rpm (accelerated at an acceleration of 1000 rpm / s) for 30 seconds. The solution was statically spin-coated and then allowed to stand for about 15 minutes.
[0056] (6) Then, the sample obtained in step (5) was spin-coated at 5000 rpm (accelerated at 2000 rpm / s) for 30 s, and 40 μL of BCP solution with anhydrous ethanol as solvent was dynamically spin-coated at 8 s, wherein the concentration of the BCP solution was 0.5 mg / mL.
[0057] (7) Place the sample obtained in step (6) in a vapor deposition mold and perform thermal evaporation of metal electrode Ag in the vapor deposition chamber. Place the Ag particles on a thermal evaporation boat, close the door, and pump the vacuum of the chamber to 6×10 -4 Pa. Adjust the current to 120A and the evaporation rate to When the rate drops to 0, the evaporation ends and a 150 nm thick Ag electrode is obtained.
[0058] Comparative Example 1, basic perovskite film.
[0059] In this example, a high-efficiency and stable wide bandgap perovskite solar cell device was prepared according to the following steps. The selected system was FA with a bandgap of 1.67 eV. 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 Wide bandgap perovskite.
[0060] (1) Cleaning the substrate: The ITO conductive glass was placed in a cleaning solution (commercially available), deionized water, acetone, isopropanol, and anhydrous ethanol, respectively, and ultrasonically cleaned for 20 min each. After that, it was blown dry with nitrogen gas and then placed in an ultraviolet ozone (UVO) instrument for 30 min of ultraviolet ozone treatment.
[0061] (2) The ITO conductive glass treated with UV ozone was transferred to a glove box filled with nitrogen. A PTAA solution with a concentration of 5 mg / mL was spin-coated at a speed of 5000 rpm (accelerated at an acceleration of 2500 rpm / s) for 25 s (the 25 s includes the acceleration time, the same below), and the spin-coated film was annealed on a heating table at 100°C for 10 min. After annealing, the film was allowed to stand at room temperature before starting the next step.
[0062] (3) The sample obtained in step (2) is rinsed with DMF: the DMF solution is heated on a heating table at 100°C for 5 min, 40 μL of the heated DMF solution is aspirated with a pipette, and spin-coated at a rotation speed of 4000 rpm (accelerated at an acceleration of 2000 rpm / s) for 25 s. The DMF solution is dripped at 8 s, thus achieving dynamic spin coating of the DMF solution. The dynamic spin coating process is called DMF rinsing.
[0063] (4) Clean the glove box before starting to spin-coat the perovskite. 0.65 MA0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 The wide bandgap perovskite precursor solution is fully dissolved for 12 hours.
[0064] FA 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 The preparation process of the wide bandgap perovskite precursor solution is as follows: 167.7 mg FAI, 553.2 mg PbI2, 33.6 mg MABr, 110.1 mg PbBr2, 58.5 mg CsI, and 24 mg MACl are dissolved in 1 mL of a mixed solution of DMF and DMSO with a volume ratio of 4:1.
[0065] The prepared FA with a concentration of 2 mg / mL 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 The wide bandgap perovskite precursor solution is placed in a glove box. 30 μL of the precursor solution is spread on the sample obtained in step (3), and spin-coated at a low speed of 1100 rpm (accelerated at 1000 rpm / s) for 2 seconds; then spin-coated at a high speed of 6000 rpm (accelerated at 2000 rpm / s) for 30 seconds. At a high speed of 20-25 seconds, 110 μL of anti-solvent chlorobenzene solution is added dropwise, and the spin-coated perovskite film is immediately placed on a 100°C heating table for annealing for 45 minutes to obtain a crystallized perovskite film (i.e., a basic perovskite film). After annealing, let it stand at room temperature before starting the next step.
[0066] The basic perovskite film prepared here and the improved film after adding the halogen-like additive in Examples 1 and 2 were respectively subjected to SEM testing, and the obtained SEM images and cross-sectional images are shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the grain size of the perovskite film with the addition of additives becomes larger and the film surface becomes smoother. - or PF6 - )The grain boundaries of the perovskite film after addition are significantly reduced compared with those of the base perovskite film.
[0067] The prepared basic perovskite film and the improved film after adding the halogen-like additive in Examples 1 and 2 were tested by AFM respectively. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that after adding halogen-like additives, the roughness of the perovskite film is significantly reduced.
[0068] The light stability of the prepared basic perovskite film and the improved film with halogen-like additives was tested. After continuous irradiation with sunlight for 1 hour, photoluminescence (PL) measurements were performed every 30 minutes. The obtained PL spectra are shown in Figure 2. Figure 5 As shown. Figure 5 It can be seen that the PL peak position of the halogen-like additive is 741nm, and the peak position does not move after illumination, indicating that the halogen in the perovskite is not separated; while the peak position of the base perovskite film moves from 741nm to 744nm after continuous irradiation with sunlight, indicating that halogen separation occurs under illumination conditions. This shows that the halogen separation in the perovskite is effectively reduced after treatment with the halogen-like additive.
[0069] Figure 7 The water contact angle diagram of the base perovskite film and the perovskite film with halogen-like additives. It can be clearly seen that the film with the additive is more hydrophobic, and the contact angle increases from 46.3° to 57.8° and 70.4°.
[0070] (5) The filtered PCBM solution was spin-coated on the sample obtained in step (4). The concentration of the solution was 20 mg / mL. The solution was spin-coated at a rotation speed of 1500 rpm (accelerated at an acceleration of 1000 rpm / s) for 30 seconds. The solution was statically spin-coated and then allowed to stand for about 15 minutes.
[0071] (6) Then, the sample obtained in step (5) was spin-coated at 5000 rpm (accelerated at 2000 rpm / s) for 30 s, and 40 μL of BCP solution with anhydrous ethanol as solvent was dynamically spin-coated at 8 s, wherein the concentration of the BCP solution was 0.5 mg / mL.
[0072] (7) Place the sample obtained in step (6) in a vapor deposition mold and perform thermal evaporation of metal electrode Ag in the vapor deposition chamber. Place the Ag particles on a thermal evaporation boat, close the door, and pump the vacuum of the chamber to 6×10 -4 Pa. Adjust the current to 120A and the evaporation rate to When the rate drops to 0, the evaporation ends and a 150 nm thick Ag electrode is obtained.
[0073] The solar cell device prepared in this comparative example is a basic device.
[0074] Figure 6 (a) shows the JV curves of the basic device and the device with halogen-like additives (F in the figure represents forward scanning, and R represents reverse scanning). Compared with the basic device, the open circuit voltage of the device with halogen-like additives increases from 1.130 V to 1.195 V, and the current density increases from 20.3 mA / cm 2 Increased to 21.1mA / cm2 , the fill factor increased from 77% to 81.88%, and the conversion efficiency of the device with halogen-like additives was 20.643%, which is close to the world efficiency. Figure 6 (b) shows the external quantum efficiency (EQE) curves of the basic device and the device with halogen-like additives. It can be seen that the error between the current density measured by the JV curve and the current density measured by the EQE is within 5%.
[0075] The wettability of the F-type halogen perovskite precursor solution is poor, and the wettability of the PTAA film surface is poor. The present invention heats the DMF solvent to rinse the PTAA layer, so that the optimized PTAA layer is used as an intermediate to connect the perovskite film layer and the PTAA layer. At the same time, the non-wetting property of the PTAA film and the hydrophobicity of the F-type halogen perovskite precursor solution are improved, and finally a highly efficient and stable wide-bandgap perovskite solar cell is prepared.
[0076] The present invention utilizes halogen-like anions to partially replace halogen ions, thereby improving the halogen separation commonly seen in wide-bandgap perovskites while obtaining higher conversion efficiency, thereby increasing the stability of the perovskite; at the same time, it improves the tensile strain caused by the unstable thermal expansion coefficient between the perovskite and the underlying layer, thereby increasing the carrier transfer rate of the perovskite.
Claims
1. A high-stability wide-bandgap perovskite solar cell, comprising, from bottom to top, ITO conductive glass, a hole transport layer, a perovskite film, an electron transport layer, a barrier layer, and a metal electrode; characterized in that: The perovskite film uses FA with a band gap of 1.67 eV 0.65 MA 0.20 Cs 0.15 Pb(I 0.8 Br 0.2 )3 wide band gap perovskite; the perovskite film is composed of halogen-like anions BF4 - Partially replace halogen ions; The hole transport layer is a PTAA layer, and the PTAA layer is washed with a heated DMF solution.
2. A method for preparing a wide bandgap perovskite solar cell with high stability according to claim 1, characterized in that: The steps include: a. Cleaning the substrate: ultrasonically clean the ITO conductive glass in cleaning solution, deionized water, acetone, isopropanol and anhydrous ethanol in sequence, then blow dry with nitrogen, and then place it in a UV ozone instrument for UV ozone treatment; b. Preparation of hole transport layer: In a glove box filled with nitrogen, PTAA solution was spin-coated on ITO conductive glass by static spin coating, followed by annealing; c. Rinsing the hole transport layer: heat the DMF solution, then use a pipette to absorb the heated DMF solution, and spin-coat the heated DMF solution on the hole transport layer by dynamic spin coating to rinse the hole transport layer; d. Preparation of perovskite film: Spin coating a wide bandgap perovskite precursor solution on the rinsed hole transport layer by static spin coating; e. Preparation of electron transport layer: Spin coating the PCBM solution on the perovskite film by static spin coating; f. Preparation of the blocking layer: Spin coating the BCP solution on the electron transport layer by dynamic spin coating; g. Preparation of metal electrodes: The metal electrodes are prepared by thermal evaporation method; In step d, the wide band gap perovskite precursor solution is a MABF4 wide band gap perovskite precursor solution; the preparation process of the MABF4 wide band gap perovskite precursor solution is: dissolve 167.7 mg FAI, 553.2 mg PbI2, 33.6 mg MABr, 110.1 mg PbBr2, 58.5 mg CsI, 24 mg MACl, and 2 mg MABF4 in 1 mL of a mixed solution of DMF and DMSO with a volume ratio of 4:
1.
3. The method for preparing a wide bandgap perovskite solar cell with high stability according to claim 2, characterized in that: In step d, the wide bandgap perovskite precursor solution is spin-coated for 32 seconds; and the anti-solvent chlorobenzene solution is added dropwise when the spin coating lasts for 22 seconds to 27 seconds; and finally, the obtained perovskite film is annealed.
4. The method for preparing a wide bandgap perovskite solar cell with high stability according to claim 2, characterized in that: In step c, heating the DMF solution is specifically: placing the DMF solution on a heating table at 100° C. and heating for 5 minutes.