A short-range oriented amorphous colloidal material that can be peeled off from an electrode and an electrochemical preparation method thereof
Through the electrochemical method of adding hydrogen peroxide and acetic acid to the electrolyte, the problem of special-shaped structure shaping and operational convenience in the preparation of collagen materials on electrodes has been solved, and efficient, fast and uniform preparation of collagen materials has been achieved. The appearance of the material is transparent and It has a dense structure and has the ability to be recycled.
Patent Information
- Application Number
- CN202210102038.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-01-27
AI Technical Summary
Existing electrochemical deposition technology is difficult to obtain collagen materials directly on electrodes, and the special-shaped structure shaping and operation convenience of the materials are insufficient. Traditional methods have problems such as difficulty in controlling the uniformity of the material structure and long operation time.
Hydrogen peroxide and acetic acid are added to the electrolyte, and peelable collagen materials are prepared on the electrodes through electrochemical methods. Titanium sheets are used as cathodes and platinum sheets are used as anodes. The electrode spacing is controlled at 0.5-3.0cm, and constant voltage or constant current is used. During deposition, the pH and concentration of the collagen solution are adjusted to achieve rapid formation and uniformity of the collagen gel film.
It is possible to directly obtain collagen materials on electrodes. The distance between electrodes is expanded to centimeter level. The material has a transparent appearance and dense structure. The preparation time is shortened to 10-15 minutes. It has the ability of plastic deformation and can be produced cyclically.
Smart Images

Figure CN114808081B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomacromolecule assembly and relates to a collagen material that can be stripped from an electrode and an electrochemical preparation method thereof. Background Art
[0002] Collagen is one of the most abundant proteins in vertebrates. It has been widely used in various biomedical materials due to its low immunogenicity, high biocompatibility, and ability to promote cell proliferation and wound healing. Collagen is a triple helical structure that can be assembled hierarchically and orderly under the guidance of some endogenous signals in the body, starting from the triple helical structure, undergoing hierarchical assembly of collagen microfibrils, collagen fibrils, and collagen fibers, and finally forming a tissue structure.
[0003] In vitro, people often use solution casting to process simple collagen into collagen biomaterials. The operation steps are to adjust the collagen solution to neutrality and then put it into the mold, incubate it at 37°C for a period of time to complete the collagen hierarchical assembly process. The disadvantages are: 1. It is not easy to process various special-shaped collagen materials; 2. It takes several hours or even overnight to complete; 3. The collagen fibers inside the material are disordered, the collagen arrangement density is low, and the material appearance is opaque.
[0004] The use of electrochemical deposition technology (Electro-deposition EDP) to prepare collagen materials is a relatively advanced processing method. Its principle is to apply an electric field to the acidic solution of collagen to drive the collagen molecules to electrophoretically migrate to the cathode area; at the same time, the electrochemical reaction occurring on the cathode (usually the electrolysis of water) can increase the pH value of the solution near the electrode, and the collagen that migrates to the collagen isoelectric point area is precipitated, thus forming collagen materials. Compared with the solution assembly method, the advantages are that the process is usually faster and can be completed in about 30-60 minutes; second, the material can be shaped; third, the material microstructure has orientation characteristics, the collagen is densely arranged, and the material appearance is transparent. The disadvantages are also obvious: because the isoelectric point region is usually located at a certain position in the electrolyte, the collagen material cannot be directly deposited on the electrode, which is inconvenient to obtain the material, and it is also inconvenient to use the shape of the electrode to shape the collagen material (for example, to obtain tubular or irregular shaped collagen materials); and the distance between the two electrodes is very small, generally 1-2 mm, which is not convenient for operation (An electrochemical fabrication process for the assembly of anisotropically oriented collagen bundles, Biomaterials 29 (2008) 3278-3288; Tenogenic Induction of Human MSCs by Anisotropically Aligned Collagen Biotextiles, Adv. Funct. Mater. 2014, 24, 5762-5770).
[0005] In addition, some researchers have used pulsed EDP technology to obtain collagen materials on electrodes. The main strategy is to add 50% organic solvent ethanol to the electrolyte (probably to reduce the solubility of collagen) and use pulse voltage (to reduce the hydrogen bubbles generated on the cathode to facilitate collagen deposition). The disadvantages of this method are: organic solvents may cause structural changes in collagen, the structural uniformity of the material obtained by the electrode is not easy to control, the operation time is long, requiring 1.5 hours, and the obtained material is opaque (Fabrication of free standing collagen membranes by pulsed electrotrophoretic deposition, Biofabrication 11, 2019, 045017).
[0006] Therefore, it is necessary to develop new methods to overcome the above shortcomings so as to obtain collagen materials that meet the requirements more quickly and effectively. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide an electrochemical deposition preparation method which can directly obtain collagen material from an electrode, so as to efficiently obtain collagen material that meets the requirements.
[0008] To achieve the above object, the present invention provides a method for preparing a collagen material that can be peeled off from an electrode, wherein hydrogen peroxide and / or acetic acid are added to an electrolyte, and a peelable collagen material is prepared on an electrode by an electrochemical method. Optionally, the cathode can be stainless steel, carbon paper, carbon cloth, Pt electrode, gold electrode, graphite electrode, Ti electrode; the anode can be stainless steel, carbon paper, carbon cloth, Pt electrode, gold electrode, graphite electrode, but cannot be Ti.
[0009] Optionally, the preparation method comprises the following steps:
[0010] S1, preparation of collagen solution: adding acetic acid to the collagen solution to completely dissolve the collagen, adjusting the pH value of the final solution to 1.5-4.0, and concentrating to obtain a collagen solution with a concentration in the range of 1-20 mg / ml;
[0011] S2, adding hydrogen peroxide standard liquid to the collagen solution obtained in step S1 so that the final volume percentage of the solution is 5%-17%, stirring, removing bubbles, and placing at 0-10° C. for standby use;
[0012] S3, using a titanium sheet as a cathode and platinum as an anode, the two electrodes are placed in parallel in an electrolytic cell with a distance between the electrodes controlled at 0.5-3.0 cm, and the collagen solution prepared in step S2 is slowly added to the electrolytic cell;
[0013] S4, electrochemical reaction is carried out by constant voltage or constant current deposition, the deposition time is 10-60 minutes, and a collagen gel film that can be peeled off from the cathode is obtained.
[0014] In the preparation method of the present invention, the collagen material can be directly obtained on the electrode. The electrode spacing can be increased from millimeters to centimeters, which is significantly wider than the currently commonly used electrode spacing of 2 mm, greatly facilitating the construction of the electrode and subsequent operation. For example, the distance between the electrodes can be controlled at 0.5-3.0 cm, and better controlled at 1.0-1.5 cm.
[0015] Optionally, the electrode installation method includes: placing two electrodes vertically and parallel in the electrolytic cell, or placing two electrodes horizontally and parallel in the electrolytic cell. Both horizontal electrodes and vertical electrodes can prepare collagen materials, but it is found that the materials prepared by vertical electrodes are prone to being thin on the top and thick on the bottom due to gravity, and the use of horizontal electrodes can avoid this situation.
[0016] Optionally, in step S1, the mass of the added collagen raw material is adjusted so that the concentration of the collagen solution finally obtained is 5-10 mg / ml. Through repeated tests, the present invention can achieve the preparation of self-supporting collagen (gel film) (that is, it can be peeled off from the electrode to become an independent material) by adjusting other parameters in the preparation method without using organic solvents in the electrolyte, while effectively preventing the cathode from generating bubbles. By changing the mass of the added collagen raw material, the concentration of the collagen solution finally obtained can be adjusted. When the concentration of the collagen solution finally obtained exceeds 20 mg / ml, the solution loses fluidity, and generally better results can be obtained within the range of 1-20 mg / ml.
[0017] In the present invention, collagen can be various commercially available collagens. For example, the collagen used in Example 1 of the present invention comes from Shanghai Haohai Biotechnology Co., Ltd. The self-supporting is Free-standing, which does not use other substrates as support.
[0018] Optionally, the final concentration of acetic acid added to the dialysate in step S1 needs to be determined based on the pH of the collagen electrolyte. Too little acetic acid in the dialysate will reduce the amount of acetic acid in the collagen electrolyte in the dialysis bag, and reduce the fluidity of the collagen molecules during the electrophoresis process in the subsequent electrochemical reaction. Too much acetic acid in the dialysate will increase the amount of acetic acid in the collagen electrolyte, which can easily lead to the inability of collagen molecules to deposit on the cathode surface in subsequent electrochemical reactions. The actual operation is: place the collagen raw material in ultrapure water and stir, and add acetic acid dropwise, and use a pH meter to monitor the pH value of the process until the pH range specified in the present invention is reached, at which time the collagen has been completely dissolved.
[0019] Optionally, the final concentration of hydrogen peroxide added in step S2 is 50-200 μl / ml. In theory, the addition of hydrogen peroxide contributes to the rapid formation of the collagen gel film, but experimental results show that when the concentration of hydrogen peroxide is higher than 200 μl / ml, hydrogen peroxide will directly decompose in the electrolyte, resulting in bubbles in the electrolyte, which is not conducive to the preparation of a uniform collagen gel film. For convenience of calculation, the concentration of hydrogen peroxide is 5-17%, volume ratio. For example, various commercially available hydrogen peroxide standards can be used, such as the hydrogen peroxide standard liquid used in the embodiment of the present invention from (Yonghua Chemical Co., Ltd., Article No. 210401204).
[0020] Optionally, the centrifugal speed in step S2 is 6000-8000 rpm / min. This centrifugal speed helps to remove bubbles generated in the solution due to operation and prevent the subsequent preparation of the collagen gel film from being uneven. The collagen solution prepared in step S2 should be added slowly to the electrolytic cell to prevent bubbles caused by excessive solution viscosity.
[0021] Optionally, in step S4, the voltage variation range is 0.22-1.67 V / cm2 The deposition time can be controlled within 10-45 minutes, and the deposition time can be set and optimized according to parameters such as temperature, voltage, and expected thickness of the collagen gel film. Step S4 can also be performed using a constant voltage.
[0022] Optionally, the collagen solution in step S1 is prepared as follows: accurately weigh collagen and ultrapure water according to the ratio of 400 mg type I collagen to 40 mL ultrapure water, dropwise add glacial acetic acid and stir thoroughly to completely dissolve the collagen, and adjust the pH value of the final solution to 1.5-3.0; put into a dialysis bag (which does not penetrate collagen, for example, M Wcut off =7.0 kDa) were placed in an aqueous solution containing glacial acetic acid and dialyzed at 0-5°C for 3 days to remove small molecular impurities; after dialysis, collagen viscous liquid was obtained.
[0023] Optionally, in step S2, 50-100 μl / ml of hydrogen peroxide is added to the collagen solution described in step S1, and the mixture is stirred evenly. The mixture is centrifuged at 5000-10000 rpm / min at 0-5°C to remove bubbles. The centrifuged collagen solution is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0024] Optionally, in step S3, a titanium sheet is selected as the cathode and a platinum wire or platinum sheet is selected as the anode, and the collagen solution prepared in step S2 is carefully added to the electrolytic cell slowly to prevent bubbles caused by excessive viscosity of the solution.
[0025] Optionally, in step S4, the electrode is then connected to an electrochemical workstation, a cathode voltage is applied, and constant current deposition is performed with a current density of 5-7 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time 500-2000 seconds. The preparation time of the present invention can be shortened to 8-15 minutes, and a collagen material with a wet thickness of about 300 μm can be obtained within this time window, so as to obtain the required collagen more quickly. The deposition time can also be adjusted according to the thickness of the required collagen film.
[0026] Optionally, the electrode half-reactions are as follows:
[0027] Anode: 2H2O-4e - →4H + +O2; or, cathode: 4H2O+4e - →4OH - +2H2.
[0028] Accordingly, the present invention provides a collagen gel film, which has a very uniform appearance, is highly transparent in both dry and wet states, and is formed by short-range oriented collagen microfibrils connected by non-covalent bonds; the collagen is densely arranged; the material has a transparent appearance and a uniform structure; the collagen material can be dissolved again by a solvent and can be prepared in a recycling manner. If the interior of the material is not uniform (especially due to the generation of bubbles, resulting in internal defects), when subjected to external forces, the material will produce stress concentration and break first at the structural defects. In addition, the structural defects that appear inside will also cause the incident light to scatter, reducing the transparency of the material. After the collagen gel film of the present invention is prepared, it can be peeled off from the electrode.
[0029] Optionally, the collagen gel membrane is obtained by the preparation method of the collagen material peeled off from the electrode according to the present invention.
[0030] On the other hand, the present invention provides an application of the collagen gel film or the preparation method thereof, wherein the preparation method is used to prepare a collagen gel film on an electrode, and then a collagen material is obtained. The collagen material prepared by the present invention can be dissolved again by a solvent and can be prepared again using EDP technology, that is, it can be prepared in a recycling manner, which can promote energy conservation and environmental protection.
[0031] In the present invention, the collagen gel film is produced and peeled off on the electrode, and a collagen heteromorphic material of the same shape can be prepared according to the shape of the cathode. For example, in a preferred embodiment of the present invention, when the cathode is a titanium tube, a hollow collagen tube can be obtained; when the cathode is in a shape similar to a heart valve, a collagen heteromorphic material similar to a heart valve can be obtained.
[0032] The present invention adopts improved EDP technology, uses acetic acid as an acid regulator to prepare collagen electrolyte, uses hydrogen peroxide decomposition as a cathode reaction, uses a Ti sheet as a cathode (i.e., a working electrode), and a Pt sheet as an anode (i.e., a counter electrode), and adopts a horizontal or vertical placement method to prepare collagen material.
[0033] In the present invention, ultrapure water is also called UP water, which is water with a resistivity of 18MΩ*cm (25°C). In addition to water molecules, this water has almost no impurities, no mineral trace elements, and no bacteria, viruses, chlorinated dioxins and other organic substances. When ultrapure water is treated, the conductive medium in the water is almost completely removed, and the undissociated colloid substances, gases and organic substances in the water are removed to a very low level. It usually requires four steps: pretreatment, reverse osmosis technology, ultrapurification treatment and post-treatment.
[0034] In the present invention, constant current deposition refers to an electrodeposition process in which the current remains constant. For example, in a preferred embodiment of the present invention, the current density in the electrodeposition reaction is 6.67 mA / cm 2 .
[0035] In the present invention, the collagen heteromorphic material refers to collagen whose outer shape can be prepared into various shapes as needed, such as rectangle, circle, triangle, trapezoid, hollow tube, etc.
[0036] Advantages of the present invention include:
[0037] A. Since acetic acid is a weak acid, it can provide a certain buffering capacity, so that the pH value near the cathode can be close to the isoelectric point of collagen, thereby obtaining collagen material directly on the electrode surface.
[0038] B. By changing the shape of the cathode electrode, the collagen material can be easily shaped into various special-shaped structures.
[0039] C. The cathode reaction is the decomposition of hydrogen peroxide, which does not produce bubbles. Therefore, it is conducive to obtaining a collagen material with a very uniform and dense appearance. Especially when using a horizontal electrode, it can also solve the problem of the collagen membrane being thin at the top and thick at the bottom caused by gravity.
[0040] D. The distance between electrodes can be at centimeter level, which is convenient for operation.
[0041] E. Preparation time is short, 10-15 minutes.
[0042] F. The characteristics of the collagen material are: it is composed of short-range oriented amorphous collagen microfibrils; the collagen is densely arranged; the collagen material is transparent in appearance and has a uniform structure, which is conducive to obtaining better mechanical and optical properties; it has plastic deformation ability; the collagen microfibrils are connected by non-covalent bonds, so they can be dissolved again by solvents and can be re-prepared using EDP technology, that is, they can be recycled. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic diagram of the EDP technology assembly process.
[0044] There are two ways to install the electrodes: one is to place the two electrodes vertically and parallel in the electrolytic cell (such as Figure 1 a), the other is to place two electrodes horizontally and parallel in the electrolytic cell (such as Figure 1 b).
[0045] Figure 2 It is a collagen gel membrane.
[0046] Among them, a layer of collagen gel film appeared on the cathode, such as Figure 2 As shown in (a), Figure 2 (b) shows that the E-Col collagen material has a very uniform appearance and is highly transparent in both dry and wet states.
[0047] Figure 3 It is the test result of the optical properties of collagen.
[0048] Among them, E-Col exhibits high optical transparency, with an optical transmittance of nearly 90% in the range of 450nm to 780nm (visible light range) (a). At the same time, the haze of the collagen gel film is also very low, only 10% in the visible light range (b).
[0049] Figure 4 It is a microscopic morphology characterization of collagen.
[0050] It can be seen that the E-Col membrane has a dense structure with a density of 0.88g / cm 3 The surface and cross section of the S-Col membrane have oriented nanofibers. In contrast, the interior of the solution-assembled S-Col membrane is a loose network with a density of 0.45 g / cm 3 , in which thicker fibers with a diameter of about a few microns are randomly aggregated (a). Figure 4 TEM image (b) shows that E-Col is composed of finer microfibrils tightly organized, and high-magnification TEM reveals that its diameter is about 10nm, without obvious collagen fiber characteristic D band. In contrast, S-Col has loosely arranged micron-sized fibers. High-magnification TEM images show that the micron-sized fibers in the S-Col membrane are assembled from fibrils with a diameter of 50nm. The fibrils show obvious D band characteristics of type I collagen, about 64.5nm.
[0051] Figure 5 This is the orientation characterization result diagram.
[0052] in, Figure 5 As shown in the polarized light microscope image of (a), the S-Col film has no obvious optical birefringence and exhibits an isotropic structure; while optical birefringence is observed in some areas of the E-Col gel film, indicating that some areas have an oriented structure. Figure 5 The SAXS data in (b) show that the 2D SAXS pattern of S-Col shows a ring with almost uniform intensity, indicating that it is an isotropic structure; while the 2D SAXS pattern of E-Col shows a distinct elongated ring, which indicates the emergence of an anisotropically arranged structure. Figure 5 (c) The 1D-SAXS spectrum on the left shows that when the q value ranges from 0.2 to 1.2 nm -1 When in the region, S-Col showed an obvious D-band characteristic scattering peak in the 1D-SAXS spectrum (the D-band calculated by the Bragg equation was about 62.7nm), while compared with before, E-Col did not show an obvious D-band characteristic peak, indicating its amorphous structure. Figure 5 (c) In the 1D-SAXS spectrum shown in the right figure, when the q value is at 0.05nm -1 To 0.4nm -1When the q-values are within the 400 nm region, the E-Col film shifts to higher q-values compared to the S-Col, indicating a tightening of the fiber phase arrangement.
[0053] Figure 6 This is a characterization result diagram of the dynamic and static mechanical properties of EDP collagen materials.
[0054] Among them, stretching the collagen membrane obtained in Example 1 will produce obvious plastic deformation, and the shape is irreversible after unloading (a). Static mechanical testing shows that the stress-strain curve of the collagen membrane is obtained when the stretching rate is set at 10 mm / min; the Young's modulus of the E-Col gel membrane is 0.32±0.11 MPa, the deformation is large, the elongation at break is 220.41±5.07%, and the tensile strength is 0.13±0.03 MPa. The E-Col gel membrane undergoes stress yielding in a very small area, indicating that there is only a weak cross-linking mechanism inside (b). Dynamic mechanical testing shows that the E-Col membrane exhibits large deformation, and there is obvious hysteresis between loading and unloading cycles, showing viscoelastic mechanical properties (c).
[0055] Figure 7 This is the result of the collagen membrane reversibility test.
[0056] The collagen membrane prepared in Example 1 was immersed in 0.1M acetic acid or 0.1M urea solution with a pH value of 3.5, respectively. In less than 10 minutes, E-Col dissolved rapidly. In contrast, S-Col remained stable. This indicates that the intermolecular bonding in the E-Col membrane mainly depends on some weak molecular interactions, and the solution after dissolution with acetic acid can be electrodeposited again to obtain E-Col material.
[0057] Figure 8 It is a controllable preparation of collagen membrane.
[0058] It can be seen that the thickness of the collagen film can be controlled by changing the constant current density and deposition time. When the control time is from 0 seconds to 3000 seconds, the current density is 2.5 mA / cm 2 The thickness of the collagen membrane can range from 0 μm to 400 μm; the current density is 5 mA / cm 2 The thickness of the collagen membrane can range from 0 μm to 450 μm; the current density is 10 mA / cm 2 , the thickness of the collagen membrane can range from 0 μm to 550 μm.
[0059] Fig. 9 It is a diagram of the molding of collagen materials with different macro-geometric shapes.
[0060] It can be seen that by changing the shape of the cathode electrode, a titanium tube or a stainless steel shaped column with a valve shape at one end can be used as the cathode to prepare various special-shaped structural materials. When the cathode is a titanium tube, a hollow collagen tube (a) can be obtained; when the cathode is in a shape similar to a heart valve, a collagen shaped material similar to a heart valve can be obtained (b). DETAILED DESCRIPTION
[0061] The present invention provides a technology for electrochemical deposition of biomacromolecules - collagen, which is a method for directly obtaining collagen materials on the electrode surface rather than in the electrolyte. The characteristics of the collagen material are: it is composed of short-range oriented collagen microfibrils; the collagen is densely arranged; the material is transparent in appearance and uniform in structure; it can form various structures such as membranes and tubes. Compared with the electrochemical deposition preparation technology reported by peers, its characteristics are: large electrode spacing (centimeter level), easy operation; short preparation time; and it can be directly obtained on the electrode without using organic solvents.
[0062] The present invention will be further described below with reference to the embodiments.
[0063] Example 1: Preparation of collagen material I
[0064] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen viscous liquid was obtained.
[0065] (2) Add 80 μl / ml of hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. The collagen solution after centrifugation is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0066] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration of 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0067] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2, the voltage range is 1-1.5V / cm 2 , deposition time 800 seconds, the electrode half-reaction that occurred is shown below.
[0068] Anode: 2H2O-4e - →4H + +O2
[0069] Cathode: 4H2O+4e - →4OH - +2H2.
[0070] After the experiment, a layer of collagen gel film appeared on the cathode, such as Figure 2 (a) As shown. The cathode with collagen hydrogel film was washed with ultrapure water several times, and then the collagen material E-Col was peeled off from the electrode. Both horizontal and vertical electrodes can prepare collagen materials, but it was found that the materials prepared by vertical electrodes would be thinner at the top and thicker at the bottom due to gravity. The use of horizontal electrodes can avoid this situation. The appearance of E-Col collagen material is very uniform and highly transparent in both dry and wet states, such as Figure 2 (b) as shown.
[0071] Example 2: Preparation of collagen material II
[0072] (1) Preparation of collagen solution: Accurately weigh 800 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 20 mg / ml of collagen viscous liquid was obtained.
[0073] (2) Add 160 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0074] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration: 20 mg / ml) prepared in step (2) is carefully added to the electrolytic cell, and the addition should be slow to prevent bubbles from being introduced due to excessive viscosity of the solution.
[0075] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0076] Example 3: Preparation of collagen material III
[0077] (1) Preparation of collagen solution: Accurately weigh 40 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 1 mg / ml of collagen liquid was obtained.
[0078] (2) Add 50 μl / ml of hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. The collagen solution after centrifugation is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0079] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration: 1 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0080] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0081] Example 4: Preparation of collagen material IV
[0082] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 2.0. Place it in a dialysis bag (M Wcut off=7.0 kDa) and placed in a beaker containing 1000 ml of water and 200 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0083] (2) Add 80 μl / ml of hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. The collagen solution after centrifugation is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0084] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration of 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0085] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0086] Example 5: Preparation of collagen material V
[0087] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 4.0. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 20 μl of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0088] (2) Add 80 μl / ml of hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. The collagen solution after centrifugation is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0089] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration of 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0090] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0091] Example 6: Preparation of collagen material VI
[0092] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0093] (2) Add 50 μl / ml of hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. The collagen solution after centrifugation is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0094] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration of 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0095] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0096] Example 7: Preparation of collagen material VII
[0097] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0098] (2) Add 200 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0099] (3) Select a titanium sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration of 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0100] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0101] Example 8: Preparation Example VIII of Collagen Material
[0102] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0103] (2) Add 200 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0104] (3) Select a platinum sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 1.5 cm. The collagen solution (concentration of 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0105] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0106] Example 9: Preparation of collagen material Example IX
[0107] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0108] (2) Add 200 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0109] (3) Select a Pt sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 0.5 cm. The collagen solution (concentration: 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell, and the addition should be slow to prevent bubbles from being introduced due to excessive viscosity of the solution.
[0110] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2, deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0111] Example 10: Preparation of collagen material Example X
[0112] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0113] (2) Add 200 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0114] (3) Select a Pt sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 3.0 cm. The collagen solution (concentration: 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0115] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 800 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0116] Example 11: Preparation of collagen material XI
[0117] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0118] (2) Add 200 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0119] (3) Select a Pt sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 3.0 cm. The collagen solution (concentration: 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0120] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time 500 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0121] Example 12: Preparation Example XII of Collagen Material
[0122] (1) Preparation of collagen solution: Accurately weigh 400 mg of type I collagen in 40 mL of ultrapure water, add glacial acetic acid and stir thoroughly to dissolve the collagen completely. Adjust the pH value of the final solution to 3.5. Place it in a dialysis bag (M Wcut off =7.0 kDa) and placed in a beaker containing 1000 ml of water and 15 ml of glacial acetic acid, and dialyzed at 4°C for 72 hours to remove small molecular impurities. After dialysis, 10 mg / ml of collagen liquid was obtained.
[0123] (2) Add 200 μl / ml hydrogen peroxide to the collagen solution described in step (1), stir evenly, and centrifuge at 8000 rpm / min at 4°C to remove bubbles. Store the collagen solution after centrifugation in an ice-water mixed bath to prevent decomposition of hydrogen peroxide.
[0124] (3) Select a Pt sheet (cathode) as the cathode (electrode size 2cm x 3cm) and a platinum wire or platinum sheet (anode) as the anode. Place the two electrodes horizontally and parallel in the electrolytic cell (e.g. Figure 1 b) The distance between the electrodes is controlled at 3.0 cm. The collagen solution (concentration: 10 mg / ml) prepared in step (2) is carefully added to the electrolytic cell slowly to prevent bubbles from being introduced due to high viscosity of the solution.
[0125] (4) Then the electrode was connected to the electrochemical workstation CHI660E, the cathode voltage was applied, and constant current deposition was performed with a current density of 6.67 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time was 3000 seconds, and a layer of collagen gel film was successfully prepared on the cathode after the experiment.
[0126] Example 13: Characterization of the physical and chemical properties of EDP collagen material E-Col
[0127] E-Col was prepared by the same method as in Example 1, and a gel-state thickness of about 400 μm was obtained by controlling the current intensity and the application time. For comparison, the dialyzed collagen solution was simultaneously prepared into a collagen membrane S-Col using a solution method, and the acidic collagen solution (5 mg / mL; pH = 3.5) was adjusted to a neutral pH = 7.2 with 0.5 M NaOH, and then cast in a round film culture dish (the collagen content per unit area was the same as the collagen mass per unit area assembled by EDP), incubated at 37°C for 12 hours for complete gelation, and then the gel was dehydrated at room temperature for 48 hours to form a milky white translucent gel membrane with a thickness of about 400 μm.
[0128] (1) Optical performance test
[0129] The S-Col and E-Col gel films obtained above were soaked in ultrapure water for 1 hour to reach saturated water content, cut into square pieces of fixed size and placed in a cuvette, and the transmittance (%) and haze (%) in the visible light wavelength range (380nm to 800nm) were detected using a UV-visible spectrophotometer (Lambda 950) (the measured values need to deduct the background of the cuvette). E-Col exhibits high optical transparency, with an optical transmittance of nearly 90% in the range of 450nm to 780nm (visible light range). At the same time, the haze of the collagen gel film is also very low, only 10% in the visible light range. Figure 3 shown.
[0130] (2) Micromorphology characterization
[0131] Microscopic morphology analysis was performed on a scanning electron microscope (SEM, S-4800, Hitachi). The internal ultrastructure was observed using a transmission electron microscope (TEM, JEM-2100, JEOL). First, the S-Col and E-Col gel film materials obtained above were dehydrated using a series of graded ethanol and then embedded in Eponate12 resin (Ted Pella, Redding, CA). 60-90nm thin slices were placed on a bare copper grid and then stained with uranyl acetate and lead. Images were taken at an accelerating voltage of 200kV. Figure 4 SEM surface and cross-sectional images of collagen membranes obtained by different methods. Figure 4 (a) shows that the E-Col membrane has a dense structure (density 0.88 g / cm 3 ), with oriented nanofibers on the surface and cross section. In contrast, the interior of the solution-assembled S-Col membrane is a loose network (density 0.45 g / cm 3 ), in which thicker fibers (about a few microns in diameter) are randomly aggregated.
[0132] Figure 4 The TEM image of (b) shows that E-Col is composed of finer microfibrils tightly organized, and high-magnification TEM reveals that its diameter is about 10nm, without obvious collagen fiber characteristic D band. In contrast, S-Col has loosely arranged micron-sized fibers. High-magnification TEM images show that the micron-sized fibers in the S-Col membrane are composed of fibrils with a diameter of 50nm, and the fibrils show obvious D band characteristics of type I collagen (about 64.5nm).
[0133] (3) Orientation Characterization
[0134] The orientation structure of E-Col was investigated by polarized light microscopy and small angle x-ray scattering (SAXS), respectively.
[0135] Small angle X-ray scattering (SAXS) experiments were performed at the BL19U2 SAXS beamline at the Shanghai Synchrotron Radiation Facility. Scattering data were acquired with X-ray beam illumination at a sample to detector distance of 1900 mm. The sample was measured for 60 seconds to obtain the scattering signal. The 2D SAXS data were averaged into a one-dimensional scattering intensity curve vs. q, with the background set to a polynomial function passing through the scattering minima of each SAXS curve. The degree of alignment of the collagen network was quantified by calculating the Herman orientation factor (f) using equations (I) and (II):
[0136]
[0137]
[0138] where φ is the azimuthal angle and I(φ) is the 1D intensity distribution over azimuthal angle after subtracting the background intensity. The average cos2φ is calculated by integrating the intensity of a specific 2θ diffraction peak along φ, using the above equation. Isotropic material f c = 0, and for an ideal unidirectional material, f c =1.
[0139] First, if Figure 5 (a) shows the polarized light microscope (POM) image: the S-Col film has no obvious optical birefringence and exhibits an isotropic structure; while optical birefringence is observed in some areas of the E-Col gel film, indicating that some areas have an oriented structure. Figure 5 The SAXS data in (b) show that the 2D SAXS pattern of S-Col shows a ring with almost uniform intensity, indicating that it is an isotropic structure; while the 2D SAXS pattern of E-Col shows a distinct elongated ring, which indicates the emergence of an anisotropically arranged structure. Figure 5 (c) The 1D-SAXS spectrum on the left shows that when the q value ranges from 0.2 to 1.2 nm -1 In the 1D-SAXS spectrum, S-Col shows an obvious D-band characteristic scattering peak (the D-band calculated by the Bragg equation is about 62.7nm), while E-Col does not show an obvious D-band characteristic peak compared with the previous one, indicating an amorphous structure. In the 1D-SAXS spectrum shown in the right figure of Figure 5(c), when the q value is at 0.05nm -1 To 0.4nm -1 When the q-values are within the 400 nm region, the E-Col film shifts to higher q-values compared to the S-Col, indicating a tightening of the fiber phase arrangement.
[0140] Example 14: Characterization of dynamic and static mechanical properties of EDP collagen materials
[0141] The collagen membrane described in Example 1 was cut into rectangular strips with a length of 30 mm and a width of 10 mm. When stretched, it produced obvious plastic deformation, and the shape was irreversible after unloading, such as Figure 6 (a) The static and dynamic tensile properties of the hydrogel at room temperature were studied using an Electro-Force 3200 biodynamic tester.
[0142] For static mechanical testing, the stretching rate was set at 10 mm / min, and the stress-strain curve of the collagen membrane was obtained. The Young's modulus of the E-Col gel membrane was 0.32 ± 0.11 MPa, the deformation was large, the elongation at break was 220.41 ± 5.07%, and the tensile strength was 0.13 ± 0.03 MPa. The E-Col gel membrane experienced stress yielding in a very small area, indicating that there was only a weak cross-linking mechanism (i.e., non-covalent bond interaction) inside, such as Figure 6 (b) as shown.
[0143] For dynamic mechanical testing, the loading and unloading process of the E-Col film was set between 0.001N and 0.04N. The tensile rate was set to 0.2N min -1 The dynamic cyclic tensile curve of the collagen membrane was obtained by 10 cycles. The E-Col membrane showed a large deformation, and there was an obvious hysteresis between the loading and unloading cycles, showing viscoelastic mechanical properties, such as Figure 6 (c) as shown.
[0144] Example 15: Reversibility of EDP collagen material
[0145] The collagen membrane prepared in Example 1 was immersed in a 0.1 M acetic acid solution or a 0.1 M urea solution (a strong hydrogen bond shielding agent) with a pH value of 3.5. In less than 10 minutes, E-Col was rapidly dissolved. Figure 7 As shown. In contrast, S-Col remained stable. This indicates that the intermolecular bonding in the E-Col film mainly depends on some weak molecular interactions, such as hydrogen bonds and hydrophobic interactions. The solution of E-Col dissolved in acetic acid can be electrodeposited again to obtain E-Col material.
[0146] Example 16: Controllable preparation of E-Col membrane
[0147] Based on the preparation method of Example 1, the size of the cathode titanium sheet was reduced to 1 cm x 1 cm, and the constant current density was changed to 2.5 mA / cm 2 , 5mA / cm 2 and 10mA / cm 2 ) and deposition time (500, 1000, 2000, 3000s), while other conditions remained unchanged, to obtain collagen films of different thicknesses.
[0148] By measuring the thickness of the sample under wet conditions, the relationship between the thickness and the constant current density and deposition time can be obtained. Figure 8 As shown, the thickness of the collagen film can be controlled by changing the constant current density and the deposition time.
[0149] Under the condition of controlling time from 0 to 3000 seconds, the current density is 2.5mA / cm2 , the thickness of the collagen membrane can range from 0 μm to 400 μm;
[0150] The current density is 5 mA / cm 2 , the thickness of the collagen membrane can range from 0 μm to 450 μm;
[0151] The current density is 10 mA / cm 2 , the thickness of the collagen membrane can range from 0 μm to 550 μm.
[0152] Example 17: Forming of collagen materials with different macroscopic geometries
[0153] In order to demonstrate the versatility of the improved EDP technology, which can produce macroscopic collagen structures of various shapes, we changed the shape of the cathode electrode (cathode), used a titanium tube (outer diameter 6.0 mm, inner diameter 5.0 mm) or a stainless steel shaped column with a valve shape at one end as the cathode, and used the EDP technology of Example 1 to prepare various shaped structural materials. When the cathode is a titanium tube, a hollow collagen tube can be obtained, such as Fig. 9 When the cathode is shaped like a heart valve, a collagen-shaped material similar to a heart valve can be obtained, such as Fig. 9 (b) as shown.
[0154] The above-mentioned related explanations and descriptions of the embodiments are for the convenience of those skilled in the art to understand and apply the present invention. It is obvious that those familiar with the art can easily make various modifications to these contents and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above-mentioned related explanations and descriptions of the embodiments. Improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a collagen material peeled off from an electrode, characterized in that: Hydrogen peroxide and acetic acid are added to the collagen solution to prepare a collagen material that can be peeled off from the electrode at the electrode by an electrochemical method; The preparation method comprises the following steps: S1, preparation of collagen solution: adding acetic acid to the collagen solution to completely dissolve the collagen, adjusting the pH value of the final solution to 1.5-4.0, removing impurities and concentrating to obtain a collagen solution with a concentration in the range of 1-20 mg / ml; S2, adding hydrogen peroxide standard liquid to the collagen solution obtained in step S1 so that the final volume percentage of the solution is 5%-17%, stirring, removing bubbles, and placing at 0-10° C. for standby use; S3, placing the anode and cathode in parallel in an electrolytic cell with the distance between the electrodes controlled to be 0.5-3.0 cm, and adding the collagen solution prepared in step S2 into the electrolytic cell; S4, performing electrochemical deposition for 8-60 minutes to obtain a collagen gel film that can be directly peeled off from the cathode.
2. The preparation method according to claim 1, characterized in that: The two electrodes, the anode and the cathode, are placed horizontally and parallely in the electrolytic cell, and then the collagen solution prepared in step S2 is slowly added to prevent the generation of bubbles.
3. The preparation method according to claim 1, characterized in that: The cathode is selected from stainless steel, carbon paper, carbon cloth, Pt electrode, gold electrode, graphite electrode or Ti electrode; The anode is selected from stainless steel, carbon paper, carbon cloth, Pt electrode, gold electrode or graphite electrode, and Ti is not used for the anode; or, The electrode installation method includes placing two electrodes vertically and in parallel in the electrolytic cell; Alternatively, the distance between the electrodes is controlled at 1.0-2.5 cm.
4. The preparation method according to claim 2, characterized in that: In step S1, the mass of the added collagen raw material is adjusted so that the concentration of the final collagen solution is 5-10 mg / ml; or, In step S2, the concentration of hydrogen peroxide added is 20-150 μl / ml; the centrifugal speed is 6000-8000 rpm / min; or, Step S3: the electrode distance is 1.0-2.0 cm; or, In step S4, electrochemical deposition is performed in a constant current mode or a constant voltage mode.
5. The preparation method according to claim 2, characterized in that: The preparation of the collagen solution in step S1 is as follows: accurately weigh collagen and ultrapure water according to the ratio of 400 mg type I collagen to 40 mL ultrapure water, dropwise add glacial acetic acid and stir thoroughly to completely dissolve the collagen, and adjust the pH value of the final solution to 3.0-4.0; Wcutoff =7.0kDa dialysis bags were placed in an aqueous solution containing glacial acetic acid and dialyzed at 0-5°C for 3 days to remove small molecule impurities; after dialysis, a viscous collagen liquid was obtained; or, In step S2, 50-100 μl / ml of hydrogen peroxide is added to the collagen solution in step S1, and the mixture is stirred evenly, and the mixture is centrifuged at 5000-10000 rpm / min at 0-5°C to remove bubbles, and the collagen solution after centrifugation is stored in an ice-water mixed bath to prevent decomposition of hydrogen peroxide; or, In step S3, a titanium sheet is selected as a cathode, a platinum wire or a platinum sheet is selected as an anode, and the collagen solution prepared in step S2 is carefully added to the electrolytic cell. The addition should be slow to prevent bubbles from being introduced due to excessive viscosity of the solution; Alternatively, in step S4, the electrode is then connected to an electrochemical workstation, a cathode voltage is applied, and constant current deposition is performed with a current density of 5-10 mA / cm 2 , the voltage range is 1-1.5V / cm 2 , deposition time 500-2000 seconds.
6. The preparation method according to claim 1, characterized in that: The electrode half-reaction is as follows: Anode: 2H2O-4e-→4H + +O2; or Cathode: 4H2O+4e-→4OH-+2H2.
7. The collagen gel membrane prepared by the method for preparing a collagen material peeled off from an electrode according to any one of claims 1 to 6, characterized in that: Its appearance is very uniform and highly transparent in both dry and wet states; it is composed of short-range oriented collagen microfibrils connected by non-covalent bonds; the collagen is densely arranged; the collagen material can be dissolved again by the solvent and prepared in a cycle; or, the thickness of the wet film of the collagen material ranges from 180-550μm.
8. The collagen gel membrane according to claim 7, characterized in that The collagen gel membrane has one or more of the following characteristics: The optical transmittance in the visible light range of 450nm to 780nm is 90%; The haze is only 10% in the visible light range; It has a dense organizational structure with a density of 0.88g / cm 3 , there are oriented nanofibers on the surface and in the cross section; The collagen gel membrane has no obvious characteristic D band of collagen fibers and is an amorphous structure; Its 2D SAXS pattern shows obvious elongated rings with anisotropically arranged structures; Young's modulus is 0.32±0.11MPa, elongation at break is 220.41±5.07%, and tensile strength is 0.13±0.03MPa; After being immersed in 0.1 M acetic acid or 0.1 M urea solution at pH 3.5, respectively, it dissolved in less than 10 minutes.
9. The use of the preparation method according to claim 1, characterized in that: The preparation method is used to prepare a collagen gel film on an electrode to obtain a collagen material.
10. The use according to claim 9, characterized in that A collagen heteromorphic material of the same shape is prepared according to the shape of the cathode.