A creep fatigue life assessment method for welded joints considering welding residual stress

Through finite element modeling and thermal coupling calculation, the Omega creep damage model is modified to consider welding residual stress, which solves the problem of failure to evaluate the life of welded joints in the existing technology and improves the accuracy of creep fatigue life and design accuracy.

CN114818193BActive Publication Date: 2024-10-11CHINA UNIV OF PETROLEUM (EAST CHINA) +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210490978.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-07
Publication Date
2024-10-11
Estimated Expiration
2042-05-07

AI Technical Summary

Technical Problem

Existing creep fatigue life assessment methods fail to consider welding residual stress, resulting in inaccurate life assessment of welded joints and the inability to accurately design and evaluate the creep fatigue life of welded joints.

Method used

Finite element modeling and thermal coupling calculation methods are used to modify the Omega creep damage constitutive model, taking into account the interactive evolution law of welding residual stress in creep fatigue, and calculate the creep fatigue life through the modified model, combined with elastic stability analysis and Correct coefficients to improve evaluation accuracy.

Benefits of technology

The calculation accuracy of creep fatigue life is significantly improved, the structural design of welded joints can be evaluated more accurately, and the accuracy of life prediction of high-temperature equipment is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114818193B_ABST
    Figure CN114818193B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for evaluating the creep fatigue life of a welded joint taking into account welding residual stress. By studying the relaxation law of welding residual stress in the creep fatigue process, the relationship between welding residual stress and cycle number is proposed, and the welding residual stress is introduced into the Omega creep damage constitutive model for correction. Then, the corrected Omega creep damage constitutive model is used to calculate the pure creep life without considering fatigue damage, the allowable fatigue cycle number when considering creep damage, and the creep fatigue life considering fatigue damage, so as to evaluate the structural design of the welded joint. Compared with the traditional evaluation method that does not consider the influence of residual stress, the creep fatigue life evaluation method of the present invention can be more in line with the actual stress condition of the welded joint, so as to more accurately evaluate the structural design of the welded joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of creep fatigue life prediction, and in particular to a method for evaluating the creep fatigue life of a welded joint taking welding residual stress into consideration. Background Art

[0002] In the energy and chemical, nuclear power, aerospace and other industries, a large number of mechanical equipment such as petrochemical hydrogenation reactors, aircraft engines, heat exchangers, steam pipes and nuclear power core equipment have a large number of welded joints and are in service under high temperature conditions for a long time. Due to frequent start-up and shutdown, temperature fluctuations in a large range, and extreme environments of high temperature and high pressure, creep fatigue interaction has become one of the most common ways for high-temperature equipment to fail, especially welded joints. Therefore, accurately evaluating the creep fatigue interaction life of materials has become a severe test.

[0003] In the 1990s, Prager et al. proposed the Omega method through material testing and theoretical research for the design of pressure vessels under creep conditions and the evaluation of creep fatigue life. However, the creep fatigue life evaluation method did not consider the influence of welding residual stress, and the initial welding residual stress is inevitable for welded joints, and the residual stress has a great influence on the mechanical behavior and deformation of the creep fatigue process. Therefore, it is urgent to propose a creep fatigue life evaluation method that considers welding residual stress to accurately design and evaluate the creep fatigue life of welded joints. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for evaluating the creep fatigue life of a welded joint taking into account welding residual stress, which can improve the accuracy of welded joint design and improve the accuracy of creep fatigue life evaluation.

[0005] The technical solution adopted by the present invention is:

[0006] The present invention provides a method for evaluating the creep fatigue life of a welded joint taking into account welding residual stress, comprising the following steps:

[0007] (1) Perform finite element modeling on the structure of the selected material, select the design temperature and design pressure, use the linear elastic model for analysis and design, select the area with the largest Mises stress value as the dangerous area, perform linear analysis and strength verification on the dangerous area, and determine the fatigue stress amplitude S of the dangerous area a , and set the design life L of the material w And design cycle number N T ;

[0008] (2) Establishing a finite element model of a standard welded joint specimen, using a thermal-mechanical coupling calculation method to calculate the creep-fatigue interactive evolution law of the welding residual stress at the design temperature in step (1), modifying the Omega creep damage constitutive model, and establishing a modified Omega creep damage constitutive model;

[0009] (3) Based on the finite element model established in step (1), the most dangerous working condition is selected, at least two loading and unloading cycles with holding time are calculated, and elastic stability analysis is performed on the weld joint to be evaluated. If the elastic stability analysis meets the requirements, proceed to step (4); if the elastic stability analysis does not meet the requirements, modify the structural parameters in step (1) and recalculate;

[0010] (4) According to the modified Omega creep damage constitutive model determined in step (2), calculate the pure creep life L without considering fatigue damage f , if L f <10 6 h, creep life L f That is the calculated value, such as L f ≥10 6 h, then the creep life L f Recorded as 10 6 h;

[0011] (5) Based on the pure creep life obtained in step (4) and the fatigue stress amplitude obtained in step (1), calculate the allowable number of fatigue cycles N when creep damage is considered. Sa and the design cycle number N T Compare, if N Sa ≥N T , then the assessment is passed, if N Sa <N T , then it is necessary to modify the structural parameters in step (1) and recalculate;

[0012] (6) The pure creep life L obtained in step (4) is corrected by the correction factor f Correction is made to calculate the creep fatigue life L considering fatigue damage f-m , compared with the modified creep fatigue life L f-m Design life L w , if L f-m ≥L w , then the assessment is passed, if L f-m <L w , then it is necessary to modify the structural parameters in step (1) and recalculate.

[0013] Furthermore, the modified Omega creep damage constitutive model in step (2) is as follows:

[0014]

[0015] Among them, D c is the creep damage ratio, is the corrected initial creep strain rate, Ω and n are the process calculation parameters of the Omega creep damage model, and β is the input parameter of the Omega creep damage model;

[0016] In the above formula, The calculation formula of Ω and n is as follows:

[0017]

[0018]

[0019]

[0020] in, N=t / (T+T0), σ0 is the initial residual stress of the welded joint, a is the proportionality coefficient, N is the number of cycles, T is the test period, T0 is the load holding time, t represents the loading time at the current moment, σ e is the equivalent stress, σ1, σ2, σ3 are the three-dimensional principal stresses, Tem is the temperature, A0~A4, B0~B4 are the creep damage coefficients of CrMoV steel material.

[0021] Furthermore, the initial residual stress σ0 of the weld joint takes the maximum value of the initial residual stress of the weld joint.

[0022] Furthermore, the calculation formula of the correction coefficient in step (6) is:

[0023]

[0024] In the above formula,

[0025] Among them, Δε peq is the equivalent plastic strain amplitude, σ rs is the welding residual stress, ε rs is the welding residual strain, and E is the cyclic Young's modulus at half life cycle.

[0026] Furthermore, in step (6), the corrected creep fatigue life L f-m The calculation formula is:

[0027]

[0028] Furthermore, in the elastic stability analysis process in step (3), the ideal elastic-plastic model is combined with the modified Omega creep damage constitutive model for analysis.

[0029] Furthermore, the load holding time of each loading and unloading cycle in step (3) is greater than 8800 hours.

[0030] The beneficial effects of the present invention are:

[0031] The present invention studies the relaxation law of welding residual stress in the creep fatigue process, proposes the relationship between welding residual stress and cycle number, and introduces welding residual stress into the Omega creep damage constitutive model to correct the creep damage constitutive model. The corrected Omega creep damage constitutive model of the present invention can be more in line with the actual stress conditions of the welded joint, and can significantly improve the calculation accuracy of the creep strain rate and the creep fatigue life, thereby more accurately evaluating the structural design of the welded joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 is the evolution law of residual stress with the number of cycles;

[0034] Figure 2 It is a schematic diagram of the relationship between stress and time and stress and strain in the stability analysis;

[0035] Figure 3 This is the relationship diagram between creep damage and creep life. DETAILED DESCRIPTION

[0036] The present invention provides a method for evaluating the creep fatigue life of a welded joint taking into account welding residual stress. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0037] The present invention provides a method for evaluating the creep fatigue life of a welded joint taking into account welding residual stress, comprising the following steps:

[0038] (1) Perform finite element modeling on the structure of the selected material, select the design temperature and design pressure, use the linear elastic model for analysis and design, select the area with the largest Mises stress value as the dangerous area, perform linear analysis and strength verification on the dangerous area, and determine the fatigue stress amplitude S of the dangerous area a , and set the design life L of the material w And design cycle number NT ;

[0039] (2) Establish a finite element model of a standard welded joint specimen, modify the Omega creep damage constitutive model, and establish a modified Omega creep damage constitutive model; the modification process is as follows:

[0040] (21) Based on the ABAQUS finite element analysis, the thermal-mechanical coupling calculation method is used to calculate the creep-fatigue interaction evolution law of welding residual stress at the design temperature in step (1), and the welding residual stress σ is established. rs The relationship between the number of cycles N is as follows:

[0041]

[0042] N=t / (T+T0) (2)

[0043] Among them, σ0 is the initial residual stress of the welded joint (σ0 takes the maximum value of the initial residual stress during the calculation process), a is the proportionality coefficient, N is the number of cycles, T is the test period, T0 is the load holding time, and t represents the loading time at the current moment;

[0044] (22) The welding residual stress σ rs Converted into welding residual strain ε rs , the formula is as follows:

[0045]

[0046] Where E represents the cyclic Young's modulus of half-life cycles;

[0047] The above welding residual strain ε rs Taking the derivative of the loading time and taking the absolute value, the residual strain rate is obtained The formula is as follows:

[0048]

[0049] (23) Considering welding residual strain ε rs , corrected initial creep strain rate The formula is as follows:

[0050]

[0051] in, σ e is the equivalent stress, σ1, σ2, σ3 are the three-dimensional principal stresses, Tem is the current temperature, and A0~A4 are the creep damage coefficients of CrMoV steel materials;

[0052] (24) Based on the above modified initial creep strain rate Creep damage ratio Dc Correction is made, and the calculation formula is:

[0053]

[0054] in, B0~B4 are creep damage coefficients of CrMoV steel materials;

[0055] (3) Based on the finite element model established in step (1), the most dangerous working condition is selected, at least two loading and unloading cycles with holding time are calculated, and an elastic stability analysis is performed on the weld joint to be evaluated. If the elastic stability analysis meets the requirements, step (4) is continued; if the elastic stability analysis does not meet the requirements, the structural parameters in step (1) are modified and recalculated; in the elastic stability analysis process in step (3), an ideal elastic-plastic model is combined with a modified Omega creep damage constitutive model for analysis, and the holding time of each loading and unloading cycle in step (3) is greater than 8800 hours;

[0056] (4) According to the modified Omega creep damage constitutive model determined in step (2), calculate the pure creep life L without considering fatigue damage f , if L f <10 6 h, creep life L f That is the calculated value, such as L f ≥10 6 h, then the creep life L f Recorded as 10 6 h; In this step, the pure creep life L f The time corresponding to when the creep damage ratio Dc reaches 0.95;

[0057] (5) Based on the pure creep life obtained in step (4) and the fatigue stress amplitude obtained in step (1), calculate the allowable number of fatigue cycles N when creep damage is considered. Sa and the design cycle number N T Compare, if N Sa ≥N T , then the assessment is passed, if N Sa <N T , then it is necessary to modify the structural parameters in step (1) and recalculate;

[0058] (6) The pure creep life L obtained in step (4) is corrected by the correction factor f Correction is made to calculate the creep fatigue life L considering fatigue damage f-m , compared with the modified creep fatigue life L f-m Design life L w , if L f-m ≥L w, then the assessment is passed, if L f-m <L w , then the structural parameters in step (1) need to be modified and recalculated; in this step, the calculation formula of the correction coefficient is:

[0059]

[0060] Among them, Δε peq is the equivalent plastic strain amplitude, and N is calculated using the allowable fatigue cycle number N Sa ;

[0061] Based on the above correction factor, the corrected creep fatigue life L f-m The calculation formula is:

[0062]

[0063] Example 1

[0064] In this embodiment 1, the creep fatigue life assessment method is described in detail by taking the top head and the cylinder welded joint of the hydrogenation reactor made of CrMoV steel as an example, and the steps are as follows:

[0065] (1) Finite element modeling was performed on the selected head and cylinder connection area. The design temperature was selected as 450 °C and the design pressure was selected as 18 MPa. The linear elastic model was used for analysis and design. The dangerous area with the largest Mises stress value was selected for linear analysis and strength verification. The evaluation results are shown in Table 1, and the fatigue stress amplitude S of the dangerous point was determined. a is 192.3MPa, and the design life of the material is set to L w 1.1*10 5 h. Design cycle number N T is 1000 times;

[0066] (2) Establish a finite element model of a standard welded joint specimen, modify the Omega creep damage constitutive model, and establish a modified Omega creep damage constitutive model; the modification process is as follows:

[0067] (21) Based on the finite element analysis of abaqus, a standard model of the welded joint in the connection area was established. The thermal-mechanical coupling calculation method was used to calculate the evolution law of the welding residual stress under creep-fatigue interaction at 450 °C, stress ratio R = 0, stress amplitude 36 MPa, cycle T = 5 s, and holding time T0 = 30 min. Eight points on the transverse path of the center of the sample were selected, and the residual stress evolution of each point as the cycle progressed was as follows: Figure 1 As shown in the figure, the correlation between the residual stress and the number of cycles is selected to fit the points in the middle area. Figure 2 As shown, the welding residual stress σ rsThe relationship between it and the cycle number N is:

[0068]

[0069] At the same time, the cyclic Young's modulus of half-life cycle E=1.83*10 5 MPa;

[0070] (22) The above welding residual stress σ rs Converted into welding residual strain ε rs , and according to the simulated cyclic mechanical response half-life cycle cyclic Young's modulus E = 1.83*10 5 MPa, the welding residual strain is obtained as:

[0071]

[0072] Then the above welding residual strain is derived with respect to the loading time and the absolute value is taken to obtain the residual strain rate:

[0073]

[0074] (23) Substitute the creep damage coefficients A0~A4 and B0~B4 of CrMoV steel material in Table 2 into the initial creep strain rate And creep failure ratio D c The calculation formula for updating and D c ;

[0075] (3) The elastic stability analysis of the connection area between the head and the shell was carried out. The design temperature was selected as 450°C and the design pressure was 18 MPa. Two loading and unloading cycles with holding time were calculated. The holding time of each cycle was 9000 h. The stability analysis adopted the ideal elastic-plastic model. At the same time, the creep damage model was secondary developed using Fortran. The elastic analysis of the structure was carried out by combining the ideal elastic-plastic model with the modified Omera creep damage model. Figure 2 As shown, it is found that each time the structure is reloaded, the stress can reach the value before unloading, and each loading and unloading section completely overlaps, and no reverse yielding occurs, and there is no accumulation of plastic strain. Therefore, in this case, the structure meets the requirements of elastic stability.

[0076] (4) Without considering the influence of fatigue damage, the modified Omega creep damage model is selected, and the working conditions of 450℃ and 36MPa are selected to calculate the relationship between the simulated creep damage and the creep life, thus obtaining the following: Figure 3 The relationship between creep damage and creep life is shown in the figure. When Dc = 0.95, L f =1.2*10 6 >106 h, then the pure creep life L f Recorded as 10 6 h;

[0077] (5) According to the relationship between the fatigue life stress amplitude and the number of cycles of CrMoV material in Table 3M of the AMSE standard (as shown in Table 3 below), combined with the pure creep life L obtained in step (4), f =10 6 h and the fatigue stress amplitude S obtained in step (1) a =192.3MPa, determine the allowable fatigue cycle number N when creep damage is considered Sa =2731, and the design cycle number N T Compare, meet the requirements;

[0078] (6) The pure creep life L obtained in step (4) is calculated by the correction factor ξ f Correction is made to calculate the creep fatigue life L considering fatigue damage f-m , the specific calculation is as follows:

[0079] (6-1) Calculate the correction coefficient ξ

[0080] Δε peq It is obtained by ASME standard, as shown in Table 4 below, when S a When <207, Δε peq =0, in this embodiment, S a =192.3MPa, therefore, Δε peq =0;

[0081] ε rs By formula Calculation, when N is 2731, ε rs =2.68*10 -4 ;

[0082] Thus: Δε peq +ε rs >0

[0083]

[0084] (6-2) Calculation of creep fatigue life L considering fatigue damage f-m

[0085] L f-m =ξL f =4.41*10 5 h, meet the design requirements.

[0086] In addition, if the influence of welding residual stress on creep fatigue life is not considered in the calculation process of step (6) of this embodiment, it can be seen from Table 4 that when Sa =192.3MPa, Δε peq = 0, the creep fatigue life L considering creep damage is obtained at this time f-m =L f =10 6 h, the predicted value of creep fatigue life is too large.

[0087] Example 2

[0088] In this embodiment 2, the Omega creep damage constitutive model before and after modification is used to calculate the creep fatigue life L of the connection area between the CrMoV steel head and the cylinder in embodiment 1 under different fatigue stress amplitudes. f-m , and a high temperature creep fatigue testing machine is used to detect its creep fatigue life to obtain the actual creep fatigue life of the welded joint. The specific predicted values ​​and actual creep fatigue life values ​​are shown in Table 5 below. It can be seen from Table 5 that the creep fatigue life prediction value after considering the welding residual stress in the present invention has high accuracy and the error is less than 5%, while the creep fatigue life prediction value without considering the welding residual stress is too large.

[0089] Table 1

[0090]

[0091] Table 2

[0092]

[0093] Table 3

[0094]

[0095] Table 4

[0096]

[0097] Table 5

[0098]

[0099] It should be noted that some parts not described in the present invention can be implemented by adopting or drawing on existing technologies.

[0100] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for evaluating the creep fatigue life of welded joints taking into account welding residual stress, characterized in that: The steps include: (1) Perform finite element modeling on the structure of the selected material, select the design temperature and design pressure, use the linear elastic model for analysis and design, select the area with the largest Mises stress value as the dangerous area, perform linear analysis and strength verification on the dangerous area, and determine the fatigue stress amplitude S of the dangerous area a , and set the design life L of the material w and design cycle number N T ; (2) Establishing a finite element model of a standard welded joint specimen, using a thermomechanical coupling calculation method to calculate the creep-fatigue interactive evolution law of the welding residual stress at the design temperature in step (1), modifying the Omega creep damage constitutive model, and establishing a modified Omega creep damage constitutive model; (3) Based on the finite element model established in step (1), the most dangerous working condition is selected, and at least two loading and unloading cycles with holding time are calculated. The elastic stability analysis of the welded joint to be evaluated is performed. If the elastic stability analysis meets the requirements, the process proceeds to step (4). If the elastic stability analysis does not meet the requirements, the structural parameters in step (1) are modified and recalculated. (4) According to the modified Omega creep damage constitutive model determined in step (2), calculate the pure creep life L without considering fatigue damage f , if L f <10 6 h, creep life L f That is the calculated value, such as L f ≥10 6 h, then the creep life L f Recorded as 10 6 h; (5) Based on the pure creep life obtained in step (4) and the fatigue stress amplitude obtained in step (1), calculate the allowable fatigue cycle number N when considering creep damage Sa and the design cycle number N T Compare, if N Sa ≥N T , then the assessment is passed, if N Sa <N T , then it is necessary to modify the structural parameters in step (1) and recalculate; (6) The pure creep life L obtained in step (4) is corrected by the correction factor f Make corrections and calculate the creep fatigue life L considering fatigue damage f-m , compared with the modified creep fatigue life L f-m and design life L w , if L f-m ≥L w , then the assessment is passed, if L f-m <L w , then it is necessary to modify the structural parameters in step (1) and recalculate; The modified Omega creep damage constitutive model in step (2) is as follows: Among them, D c is the creep failure ratio, is the corrected initial creep strain rate, Ω and n are the calculation parameters of the Omega creep damage model process, and β is the input parameter of the Omega creep damage model; In the above formula, The calculation formulas for Ω and n are as follows: in, N=t / (T+T0), σ0 is the initial residual stress of the weld joint, a is the proportional coefficient, N is the number of cycles, T is the test period, T0 is the holding time, t represents the loading time at the current moment, σ e is the equivalent stress, σ1, σ2, σ3 are the three-dimensional principal stresses, Tem is the temperature, A0~A4, B0~B4 are the creep damage coefficients.

2. A method for evaluating the creep fatigue life of welded joints considering welding residual stress according to claim 1, characterized in that: The initial residual stress σ0 of the weld joint is the maximum value of the initial residual stress of the weld joint.

3. The method for evaluating creep fatigue life of welded joints considering welding residual stress according to claim 1, characterized in that: The calculation formula of the correction coefficient in step (6) is: In the above formula, Among them, Δε peq is the equivalent plastic strain amplitude, σ rs is the welding residual stress, ε rs is the welding residual strain, and E is the cyclic Young's modulus of half-life cycles.

4. The method for evaluating creep fatigue life of welded joints considering welding residual stress according to claim 3, characterized in that: The creep fatigue life L in step (6) is corrected f-m The calculation formula is:

5. The method for evaluating creep fatigue life of welded joints considering welding residual stress according to claim 1, characterized in that: In the elastic stability analysis process in step (3), the ideal elastic-plastic model is combined with the modified Omega creep damage constitutive model for analysis.