A gel-state rechargeable and dischargeable light-assisted iron-air battery and its preparation method

By preparing TiO2-CuO thin film photoelectrode and calcium alginate hydrogel electrolyte, a gel-based iron-air battery was constructed, which solved the safety, storage and portability problems of traditional batteries and achieved efficient solar energy conversion and electrical energy. storage, reducing costs.

CN114824588BActive Publication Date: 2024-10-18LIAONING UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210473079.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-29
Publication Date
2024-10-18
Estimated Expiration
2042-04-29

AI Technical Summary

Technical Problem

Traditional lithium-ion batteries are highly dangerous, have small reserves, and are difficult to mine. Moreover, the aqueous electrolyte of traditional air batteries has leakage and is difficult to carry. The gel electrolyte has poor conductivity, which affects its use.

Method used

TiO2-CuO thin film photoelectrode material with excellent photocatalytic activity was prepared using hydrothermal method and electrochemical deposition method, and calcium alginate hydrogel was used as the electrolyte to replace the traditional aqueous electrolyte to construct a gel-based iron-air battery. , to realize the coordinated conversion of solar energy, chemical energy and electrical energy.

Benefits of technology

It reduces the charging voltage of iron-air batteries, increases the discharge voltage, solves the leakage problem of traditional batteries, broadens the application scope of green energy, reduces costs, and improves the safety and life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824588B_ABST
    Figure CN114824588B_ABST
Patent Text Reader

Abstract

The present invention relates to a gel-state rechargeable and dischargeable light-assisted iron-air battery and a preparation method thereof. The iron-air battery is composed of a TiO2-CuO thin film photoelectrode as an air electrode, an iron sheet as a metal electrode, and a calcium alginate hydrogel as an electrolyte. The TiO2-CuO light-assisted material prepared by the present invention has excellent photocatalytic activity and stability. The present invention reduces the charging voltage of the iron-air battery and increases the discharge voltage of the iron-air battery by introducing sunlight. On the other hand, the present invention realizes the conversion between solar energy, chemical energy and electrical energy, and opens up a new way for rechargeable iron-air batteries. In addition, the traditional aqueous solution is replaced by a hydrogel electrolyte as an electrolyte, which solves the leakage problem of traditional batteries and provides a new way for the development of electronic equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal-air batteries, and in particular relates to an iron-air battery based on semiconductor photoelectrode materials and gel electrolyte. Background Art

[0002] Energy has always been an important topic of human research and development, and batteries as an important carrier of energy have received widespread attention. The most common battery is the lithium-ion battery, which is widely used due to its long cycle life, good low-temperature discharge performance, and high specific energy. However, lithium-ion batteries have defects such as high risk, small reserves, and difficulty in mining. Therefore, a more efficient and cheap battery is needed to replace lithium-ion batteries. The emergence of metal-air batteries just makes up for this deficiency.

[0003] On the other hand, with the continuous depletion of fossil fuel derivatives, the development and utilization of abundant and clean renewable energy has become an urgent need for contemporary energy development. Among them, solar energy, as one of the most popular clean energy sources, has broad development prospects. At this time, light-assisted metal-air batteries based on photocatalytic technology have gradually come into people's view. Metal-air batteries are composed of metal electrodes, air electrodes and electrolyte solutions. Metal-air batteries are considered to be a new energy technology with great development potential due to their high theoretical energy density, environmental friendliness and low cost.

[0004] Iron (Fe) is the fourth most abundant element and is also a low-cost, environmentally friendly anode material. Therefore, in terms of material cost, iron-air batteries are more advantageous. Moreover, Fe is more corrosion-resistant and will relatively reduce the self-discharge rate. Therefore, among various metal-air batteries, iron-air batteries have received widespread attention due to their high energy density, environmental friendliness, abundant content and excellent safety. Many electrochemical devices use light energy, but light energy is rarely used in iron-air battery systems. Therefore, introducing light energy into iron-air batteries can make full use of solar energy and realize the conversion of solar energy to electrical energy. At the same time, using semiconductor photoelectrode materials to replace precious metal electrodes can significantly reduce the cost of iron-air batteries. In addition, traditional air batteries usually choose aqueous electrolytes, which have problems such as leakage and difficulty in carrying. However, gel electrolytes have poor conductivity, and solid electrolytes are prone to deterioration during long-term measurements, affecting their use, so further exploration is needed. Summary of the invention

[0005] In order to solve the above-mentioned technical problems, the present invention uses a hydrothermal method, an electrochemical deposition method and a calcination method to prepare a TiO2-CuO thin film photoelectrode material with excellent photocatalytic activity, and replaces the traditional aqueous electrolyte with a gel electrolyte as the electrolyte of the iron-air battery. The iron-air battery provided by the present invention can reduce the charging voltage of the iron-air battery and increase the discharge voltage of the iron-air battery under illumination conditions. The synergistic conversion between solar energy, chemical energy and electrical energy is achieved.

[0006] The technical solution adopted by the present invention is: a gel-state rechargeable and dischargeable light-assisted iron-air battery, which is an iron-air battery composed of a TiO2-CuO film photoelectrode as an air electrode, an iron sheet as a metal electrode, and a calcium alginate hydrogel as an electrolyte.

[0007] A preparation method of a gel-state rechargeable and dischargeable light-assisted iron-air battery comprises the following steps:

[0008] 1) Preparation of TiO2-CuO thin film photoelectrode: Cuprous oxide is deposited on the TiO2 thin film by electrochemical deposition to obtain a TiO2-Cu2O thin film, which is then calcined at high temperature in a muffle furnace and cooled to obtain a TiO2-CuO thin film photoelectrode.

[0009] Preferably, the method for preparing the TiO2 film comprises the following steps: mixing deionized water, concentrated hydrochloric acid and n-butyl titanate and stirring until clear and transparent, placing the obtained mixed solution and a conductive substrate into a high-pressure reactor, reacting at 170°C for 4 hours, taking out after cooling to room temperature, washing with deionized water, drying at room temperature, placing in a muffle furnace, and calcining at 500°C for 2 hours to obtain a TiO2 film loaded on the conductive substrate.

[0010] Preferably, by volume ratio, deionized water: concentrated hydrochloric acid: n-butyl titanate = 7.5:7.5:1.

[0011] Preferably, step 1) is specifically as follows: dissolving CuSO4·5H2O and lactic acid in deionized water, adjusting the pH to between 11 and 12 with NaOH solution, using the obtained solution as a deposition solution, using Pt wire as a counter electrode, Ag / AgCl as a reference electrode, and a conductive substrate loaded with a TiO2 film as a working electrode, using an electrochemical deposition method to deposit cuprous oxide on the TiO2 film to obtain a TiO2-Cu2O film, which is then placed in a muffle furnace, calcined at 550°C for 2h, and cooled to obtain a TiO2-CuO thin film photoelectrode.

[0012] Preferably, the mass ratio is CuSO4·5H2O:lactic acid=1:10-11.

[0013] Preferably, the electrodeposition is performed at a bias voltage of -0.5 V for 600 to 650 seconds.

[0014] 2) Preparation of calcium alginate hydrogel: Sodium alginate solution and potassium hydroxide solution are mixed evenly, the mixed solution is immersed in calcium chloride solution, and stirred evenly to form a gel to obtain calcium alginate hydrogel.

[0015] Preferably, step 2) is specifically as follows: a sodium alginate solution with a mass percentage concentration of 1% and a potassium hydroxide solution with a concentration of 1M are uniformly mixed in a volume ratio of 6:1, and the resulting mixture is immersed in a 0.05 g / mL calcium chloride solution for about 5 minutes to obtain a calcium alginate hydrogel.

[0016] 3) An iron-air battery is composed of a TiO2-CuO thin film photoelectrode as an air electrode, an iron sheet as a metal electrode, and a calcium alginate hydrogel as an electrolyte.

[0017] Compared with the prior art, the present invention has the following significant advantages:

[0018] 1. The present invention utilizes semiconductor material TiO2-CuO thin film to replace precious metal materials, thereby improving battery performance and saving costs.

[0019] 2. In the present invention, the metal electrode uses iron sheets, which are cheap and easy to obtain. The energy density and theoretical voltage of iron-air batteries are relatively large. At present, there is little research on iron-air batteries, so there is a lot of room for research. In addition, compared with other air batteries, iron-air batteries have the advantages of high safety and long life.

[0020] 3. The present invention uses TiO2-CuO film for air electrode to prepare a TiO2-CuO air semiconductor photoelectrode material, which reduces the charging voltage of the iron-air battery, increases the discharge voltage of the iron-air battery, and fully realizes the conversion between solar energy and electrical energy.

[0021] 4. The present invention successfully introduces gel electrolyte and solar energy into the iron-air battery system. Compared with the traditional iron-air battery, the present invention makes full use of the renewable resource of sunlight, greatly reduces the charging voltage of the battery while controlling the battery cost, broadens the road of green energy, and solves the problems of leakage and difficulty in carrying of traditional batteries. At the same time, the photocatalyst of the present invention is simple to prepare, low in price, and has good photoelectric performance. It is a photoelectrode material with considerable development prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a working principle diagram of the gel-state rechargeable and dischargeable light-assisted iron-air battery of the present invention.

[0023] Figure 2This is a test diagram of the charge and discharge performance of the TiO2-CuO film as the air electrode in the gel-state chargeable and dischargeable light-assisted iron-air battery of the present invention.

[0024] Figure 3 It is the AC impedance curve of the TiO2-CuO film as the air electrode in the gel-state chargeable and dischargeable light-assisted iron-air battery of the present invention.

[0025] Figure 4 It is a schematic structural diagram of the gel-state rechargeable and dischargeable light-assisted iron-air battery of the present invention.

[0026] Figure 5 It is a device assembly diagram of the gel-state rechargeable and dischargeable light-assisted iron-air battery of the present invention.

[0027] Figure 6 This is a diagram of two series-connected gel-state rechargeable and dischargeable light-assisted iron-air batteries of the present invention lighting up an LED bulb under simulated sunlight. DETAILED DESCRIPTION

[0028] In order to better explain the content of the present invention, the present invention is further described below through specific implementation:

[0029] Example 1: Gel-state rechargeable and light-assisted iron-air battery

[0030] (I) The preparation method comprises the following steps:

[0031] 1. Preparation of TiO2 thin film

[0032] 7.5 mL of deionized water, 7.5 mL of concentrated hydrochloric acid and 1 mL of n-butyl titanate were mixed and stirred until the mixed solution was clear and transparent. The obtained mixed solution and conductive glass were placed in a high-pressure reactor, reacted at 170°C for 4 hours, cooled to room temperature and taken out, the conductive glass was rinsed with deionized water, and dried at room temperature, and then placed in a muffle furnace and calcined at 500°C for 2 hours to obtain a TiO2 film loaded on the conductive glass.

[0033] 2. Preparation of TiO2-CuO thin film photoelectrode:

[0034] 1.25 g CuSO4·5H2O and 13.5 g lactic acid were dissolved in 50 mL deionized water, and the pH was adjusted to 11-12 with 6 M NaOH solution. The resulting solution was used as a deposition solution.

[0035] Electrochemical deposition was used for electrodeposition, with conductive glass loaded with TiO2 film as the working electrode, Ag / AgCl as the reference electrode, Pt wire as the counter electrode, -0.51V bias applied, and electrodeposition was performed at 80°C for 600s to deposit cuprous oxide on the TiO2 film to obtain a TiO2-Cu2O film. The obtained product was placed in a muffle furnace, calcined at 550°C for 2 hours, and cooled to room temperature to obtain a TiO2-CuO film photoelectrode.

[0036] 3. Preparation of calcium alginate hydrogel:

[0037] 6 mL of sodium alginate solution (1% wt) was mixed evenly with 1 mL of potassium hydroxide solution (1 M), and the resulting solution was immersed in a calcium chloride solution (0.05 g / mL) for about 5 min to obtain a calcium alginate hydrogel.

[0038] 4. Assembly of iron-air battery

[0039] like Figure 4 As shown, the TiO2-CuO thin film photoelectrode (1) is used as the air electrode, the iron sheet (2) is used as the metal electrode, and the calcium alginate hydrogel (3) is used as the electrolyte. The air electrode and the iron sheet are fixed with foam glue (4) to assemble into an iron-air battery. The physical assembly diagram of the iron-air battery device is shown in Figure 5 .

[0040] (II) Performance test

[0041] 1. AC impedance and charge and discharge performance test

[0042] Method: The AC impedance and charge-discharge performance of the iron-air battery were measured under light and dark conditions using an electrochemical workstation. Figure 2 and Figure 3 shown.

[0043] Depend on Figure 2 It can be seen that the charging voltage is 1.45V and the discharging voltage is 1.28V under light conditions; the charging voltage is 2.5V and the discharging voltage is 1.2V under dark conditions.

[0044] Depend on Figure 3 The electrochemical impedance spectroscopy shows that the radius of the EIS curve of the TiO2-CuO electrode under light conditions is smaller than that under dark conditions, indicating that the transfer speed of charge carriers is faster under light conditions and the resistance of the entire battery is reduced.

[0045] 2. Battery performance experiment

[0046] Two gel-state rechargeable and light-assisted iron-air batteries of the present invention are connected in series and then connected to an LED bulb. Under the irradiation of simulated sunlight, Figure 6 As shown, the LED bulb is lit.

Claims

1. A gel-state rechargeable and light-assisted iron-air battery, characterized in that: It is an iron-air battery composed of TiO2-CuO thin film photoelectrode as air electrode, iron sheet as metal electrode, and calcium alginate hydrogel as electrolyte. The preparation method of the gel-state chargeable and dischargeable light-assisted iron-air battery comprises the following steps: 1) Preparation of TiO2-CuO thin film photoelectrode: Cuprous oxide is deposited on the TiO2 thin film by electrochemical deposition to obtain a TiO2-Cu2O thin film, which is then calcined at high temperature in a muffle furnace and cooled to obtain a TiO2-CuO thin film photoelectrode; 2) Preparation of calcium alginate hydrogel: Mix sodium alginate solution and potassium hydroxide solution evenly, and immerse the resulting solution in calcium chloride solution to obtain calcium alginate hydrogel; 3) An iron-air battery is composed of a TiO2-CuO thin film photoelectrode as the air electrode, an iron sheet as the metal electrode, and a calcium alginate hydrogel as the electrolyte.

2. The gel-state rechargeable and light-assisted iron-air battery according to claim 1, characterized in that: Step 1), the preparation method of the TiO2 film comprises the following steps: mixing deionized water, concentrated hydrochloric acid and n-butyl titanate and stirring until clear and transparent, placing the obtained mixed solution and the conductive substrate into a high-pressure reactor, reacting at 170°C for 4 hours, cooling to room temperature and then taking out, washing with deionized water, drying at room temperature, placing in a muffle furnace, and calcining at 500°C for 2 hours to obtain a TiO2 film loaded on the conductive substrate.

3. The gel-state rechargeable and dischargeable light-assisted iron-air battery according to claim 2, characterized in that: By volume ratio, deionized water: concentrated hydrochloric acid: n-butyl titanate = 7.5:7.5:

1.

4. The gel-state rechargeable and dischargeable light-assisted iron-air battery according to claim 2, characterized in that: Step 1) is specifically as follows: dissolving CuSO4·5H2O and lactic acid in deionized water, adjusting the pH to between 11 and 12 with NaOH solution, using the obtained solution as a deposition solution, using Pt wire as a counter electrode, Ag / AgCl as a reference electrode, and a conductive substrate loaded with a TiO2 film as a working electrode, using an electrochemical deposition method to deposit cuprous oxide on the TiO2 film to obtain a TiO2-Cu2O film, which is then placed in a muffle furnace, calcined at 550°C for 2h, and cooled to obtain a TiO2-CuO film photoelectrode.

5. The gel-state rechargeable and dischargeable light-assisted iron-air battery according to claim 4, characterized in that: In terms of mass ratio, CuSO4·5H2O:lactic acid = 1:10~11.

6. The gel-state rechargeable and dischargeable light-assisted iron-air battery according to claim 4, characterized in that: The electrodeposition is performed at a bias voltage of -0.5 V for 600 to 650 seconds.

7. The gel-state rechargeable and dischargeable light-assisted iron-air battery according to claim 1, characterized in that: Step 2) is specifically as follows: a sodium alginate solution with a mass percentage concentration of 1% and a potassium hydroxide solution with a concentration of 1M are mixed evenly at a volume ratio of 6:1, and the resulting solution is immersed in a calcium chloride solution with a concentration of 0.05 g / mL to obtain a calcium alginate hydrogel.

Citation Information

Patent Citations

  • Hetero-structured copper oxide-composited titanium oxide nanowire array synthesized by hydrothermal method

    CN103433038A

  • Preparation method of rechargeable iron or zinc air battery based on hydrogel electrolyte

    CN114204167A