Methods for purifying α-olefins and compositions for this purpose.
Through the combination of shaped activated carbon and alumina-zeolite composite materials, the problem of amine-based impurity removal in α-olefins is solved, the impurity removal rate and purification capacity are significantly improved, and the production and long-term performance of high-purity α-olefins are ensured.
Patent Information
- Application Number
- CN202080087281.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-18
- Filing Date
- 2020-12-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-08
AI Technical Summary
Existing technologies struggle to effectively remove amine-based impurities in alpha-olefins, resulting in degraded purification capabilities and long-term performance degradation.
A combination of shaped activated carbon and alumina-zeolite composite materials is used, and its specific surface area, pore volume and pore size characteristics are measured by nitrogen adsorption method, which significantly improves the removal efficiency of impurities, especially the adsorption selectivity of nitrogen-containing impurities.
Significantly improves the removal rate of impurities in α-olefins, especially nitrogen-containing impurities, prolongs the purification capacity, ensures the production of high-purity α-olefins, and prevents performance degradation.
Abstract
Description
Technical Field
[0001] The following disclosure relates to a method for purifying α-olefins and a composition for purifying α-olefins therefor. More specifically, the following disclosure relates to a method for purifying α-olefins having an excellent effect of removing impurities in α-olefins and a composition for purifying α-olefins therefor. Background Art
[0002] Typically, α-olefins contain impurities generated during the oligomerization process or the polyolefin polymerization process. Typical impurities include residues from catalysts used in the polymerization, such as co-catalysts, scavengers, oligomers, by-products, various volatile low molecular weight compounds, etc. Even in the case where impurities are included in the polymer only at low concentrations, the impurities may have adverse effects.
[0003] As an example, polymers used in water pipes may deteriorate the taste or odor of the water being transported. Furthermore, for membranes used in electrical devices, it is difficult to escape electrical breakthrough when the membranes contain metallic impurities. Furthermore, polymers used in automotive applications may cause fogging problems when volatile compounds evaporate and condense on the windows, deteriorating the appearance of interior parts.
[0004] Particularly, among impurities present in α-olefins, amine-based substances are strongly adsorbed to the adsorbent and are not regenerated during the regeneration process to cause pore loss, thereby significantly reducing long-term purification capabilities.
[0005] There is currently a need for a method of significantly preventing the deterioration of the purification ability of an adsorbent and significantly improving the purification ability of removing amine-based substances in α-olefins. Summary of the invention
[0006] Technical issues
[0007] One embodiment of the present invention is directed to providing a method for purifying α-olefin and a composition for purifying α-olefin that can significantly improve the effect of removing impurities in α-olefin.
[0008] Particularly, provided are a method for purifying α-olefins having excellent purification selectivity for amine-based substances among impurities and a composition for purifying α-olefins.
[0009] Another embodiment of the present invention is directed to providing a method for purifying α-olefins and a composition for purifying α-olefins, which can exhibit a long-term purification effect by significantly preventing a long-term decrease in impurity purification ability.
[0010] Technical Solution
[0011] In one general aspect, in a method of purifying alpha-olefins, impurities are removed by a combination of: formed activated carbon having 1,200 m 2 / g or more specific surface area, an average particle size of 0.8 mm to 40 mm, and a particle size greater than 0.6 cm as measured by nitrogen adsorption. 3 / g of pore volume, pores having a diameter of 2 nm or more in the shaped activated carbon account for 60% or more of all pores; and
[0012] Alumina-zeolite composites.
[0013] The method of purifying α-olefin according to an exemplary embodiment of the present invention may be performed during a poly-α-olefin polymerization reaction or an ethylene oligomerization reaction.
[0014] Preferably, according to an exemplary embodiment of the present invention, the method of purifying α-olefin may be performed during the polymerization reaction of poly-α-olefin.
[0015] A method of purifying α-olefin according to an exemplary embodiment of the present invention may include treating with activated carbon and then treating with an alumina-zeolite composite material.
[0016] According to an exemplary embodiment of the present invention, the activated carbon and the alumina-zeolite composite material may be included in a weight ratio of 1:1 to 1:20.
[0017] The alumina-zeolite composite material according to an exemplary embodiment of the present invention may include 50 wt % to 95 wt % of alumina and 5 wt % to 50 wt % of zeolite.
[0018] According to an exemplary embodiment of the present invention, the α-olefin is any one or a mixture of two or more selected from the following: 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, and the like.
[0019] Preferably, according to an exemplary embodiment of the present invention, the α-olefin may be any one or a mixture of two or more selected from the following: 1-hexene, 1-octene, and the like.
[0020] The impurity according to an exemplary embodiment of the present invention may be an amine-based compound.
[0021] In another general aspect, a composition for purifying alpha-olefins comprises: a shaped activated carbon having 1,200 m 2 / g or more specific surface area, an average particle size of 0.8 mm to 40 mm, and a particle size greater than 0.6 cm as measured by nitrogen adsorption. 3 / g of pore volume, pores having a pore diameter of 2 nm or more in the shaped activated carbon account for 60% or more of all pores; and
[0022] Alumina-zeolite composites.
[0023] The composition for purifying α-olefin according to an exemplary embodiment of the present invention may be a two-reagent type composition including activated carbon as a first reagent and an alumina-zeolite composite material as a second reagent.
[0024] Other features and aspects will be apparent from the following detailed description, the accompanying drawings, and the claims.
[0025] Beneficial Effects
[0026] The method for purifying α-olefin according to the present invention has excellent purification selectivity particularly for nitrogen-containing impurities among impurities in α-olefin.
[0027] Furthermore, the composition for purifying α-olefin according to the present invention has excellent impurity purification capability even at a low concentration. DETAILED DESCRIPTION
[0028] Hereinafter, the present invention will be described in more detail with reference to specific examples and exemplary embodiments (including accompanying drawings). However, the following specific examples or exemplary embodiments are only references for describing the present invention in detail, and the present invention is not limited thereto and can be implemented in various forms.
[0029] In addition, unless otherwise defined, all technical and scientific terms have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used herein are only used to effectively describe a specific example and are not intended to limit the present invention.
[0030] Throughout the present specification describing the present invention, unless explicitly described to the contrary, “comprising” any elements will be understood to imply the further inclusion of other elements rather than excluding any other elements.
[0031] Furthermore, singular forms used in the specification and the claims appended hereto may be intended to include plural forms as well, unless the context indicates otherwise.
[0032] Since α-olefins contain impurities generated by nitrogen components derived from crude oil, it is difficult to produce or provide pure α-olefins without impurities through conventional purification techniques.
[0033] In order to solve this problem, the inventors of the present invention have found that it is possible to provide a purification method having a significantly improved nitrogen-containing impurity removal efficiency by a combination of specific constituent components and a specific method, thereby completing the present invention.
[0034] The method for purifying α-olefin according to the present invention is specifically as follows.
[0035] The method for purifying α-olefins according to the present invention removes impurities by a combination of: molded activated carbon having 1,200 m 2 / g or more specific surface area, an average particle size of 0.8 mm to 40 mm, and a particle size greater than 0.6 cm as measured by nitrogen adsorption. 3 / g of pore volume, pores having a pore diameter of 2 nm or more in the shaped activated carbon account for 60% or more of all pores; and
[0036] Alumina-zeolite composites.
[0037] By using a combination of specific activated carbon and alumina-zeolite composite materials, impurities, especially nitrogen-containing impurities, can be removed with remarkably superior efficiency.
[0038] In addition, as an exemplary embodiment, in the activated carbon, the pore volume measured by the nitrogen adsorption method may be greater than 0.6 cm 3 / g, and pores with a pore size greater than 2 nm may account for 60% or more of all pores. More specifically, the pore volume may be greater than 0.6 cm 3 / g, and pores having a pore diameter of 2 nm or more may account for 60% to 99% of all pores. Within this range, the adsorption efficiency of nitrogen-containing impurities may be further improved.
[0039] According to an exemplary embodiment of the present invention, the method for purifying α-olefins can be provided in various processes. Specifically, for example, the method can be used for any one or two or more processes selected from the following: a process for purifying α-olefins, a process for producing α-olefins, a process for polymerizing α-olefins, a process for recycling α-olefins, a process for recovering α-olefins, etc., but the process is not limited thereto, as long as it is a process containing α-olefins.
[0040] According to an exemplary embodiment of the present invention, the method of purifying α-olefin may be performed at any one or two or more locations selected from an introduction unit, a reaction unit, a circulation unit, a recovery unit, etc. in a process containing α-olefin.
[0041] Specifically, for example, the introduction unit means the path for the reactants to enter the reactor, and the reaction unit may mean the reactor in which the reactants are polymerized or synthesized. In addition, the circulation unit means the circulation path for the residual materials to be reintroduced into the reactants, and the recovery unit means the path for the final materials after the reaction to be discharged.
[0042] Preferably, according to an exemplary embodiment of the present invention, impurities are present in α-olefins, and when a purification method is set or added to a path containing α-olefins, the impurity purification capacity can be significantly improved. For example, when α-olefins are provided as monomers, a purification method can be set or added at any one or two or more positions selected from an introduction unit, a reaction unit, a circulation unit, etc. As another example, when α-olefins are produced, a purification method can be set or added at any one or two or more positions selected from a reaction unit, a circulation unit, a recovery unit, etc.
[0043] Specifically, according to an exemplary embodiment of the present invention, the method for purifying α-olefins can be carried out during a poly-α-olefin polymerization reaction in which α-olefins are added as monomers or an ethylene oligomerization reaction in which α-olefins are produced. By purifying impurities by the method for purifying α-olefins during a reaction in which α-olefins are provided or produced as described above, high-purity α-olefins can be provided, and performance degradation due to impurities can be prevented in various fields to be provided. In addition, due to the long-term purification capability, a significant impurity purification effect can be achieved.
[0044] According to an exemplary embodiment of the present invention, the method for purifying alpha-olefins can be carried out during poly-alpha-olefin polymerization or ethylene oligomerization, specifically, can be carried out in any one or two or more steps selected from before reaction, during reaction and after reaction. Specifically, for example, the purification method can be carried out before the polymerization of poly-alpha-olefin or after ethylene oligomerization. Preferably, in order to achieve the effect of excellent purification impurities (particularly nitrogen-containing impurities), the purification method can be carried out before poly-alpha-olefin polymerization.
[0045] According to an exemplary embodiment of the present invention, in a method for purifying alpha-olefins, the alpha-olefins may be treated with a mixture of activated carbon and an alumina-zeolite composite material or sequentially treated with each of them for impurity purification. Preferably, the alpha-olefins may be sequentially treated with the alumina-zeolite composite material after being treated with activated carbon. As described above, after first purifying impurities by activated carbon as a guard bed, additional impurity purification is performed by the alumina-zeolite composite material, thereby achieving a significantly improved impurity purification effect. In addition, the problem that impurities are adsorbed into the interior of the alumina-zeolite composite material and are not removed is prevented, thereby achieving long-term purification capabilities.
[0046] The activated carbon according to the present invention has a 2 / g specific surface area and an average particle size of 0.8mm to 40mm. Preferably, the activated carbon may be a shaped activated carbon having a specific surface area of 1,200m 2 / g to 3,000m 2 / g specific surface area and an average particle size of 0.8mm to 30mm. More preferably, the activated carbon may be a shaped activated carbon having a specific surface area of 1,200m 2 / g to 2,500m 2 / g specific surface area and an average particle size of 0.85mm to 20mm. Here, the shaped activated carbon means a porous particle form formed by agglomerating fine powders. In addition, the activated carbon may have a particle diameter greater than 0.6cm as measured by nitrogen adsorption method. 3 / g of pore volume, and pores having a pore diameter greater than 2 nm account for 60% or more of all pores, more preferably 60% to 99%.
[0047] When an activated carbon satisfying the physical properties as described above is provided, the effect of purifying impurities in α-olefins is excellent, and in particular, the adsorption selectivity of nitrogen-containing impurities is good. More specifically, such an effect can be shown that the removal rate of nitrogen-containing impurities is 85% or more, more specifically 85% to 99.9%, and more preferably 87% to 98%. This can increase the removal efficiency of nitrogen-containing impurities by 3 times or more, specifically 3 times to 5 times, compared to the case where activated carbon is not used.
[0048] Furthermore, such an effect can be exhibited by using an alumina-zeolite composite material in combination.
[0049] When the activated carbon has a mass less than 1,200 m 2 / g of specific surface area, the adsorption capacity is significantly low, making it difficult to remove impurities in α-olefins. In addition, the selectivity for impurities such as moisture and other hydrocarbons is higher than the selectivity for nitrogen-containing impurities, and the purification performance and life may be reduced.
[0050] Furthermore, when the activated carbon has an average particle size of less than 0.8 mm or greater than 40 mm, it is difficult to adsorb impurities, and in particular, selectivity for nitrogen-containing impurities decreases, thereby deteriorating purification performance of the alumina-zeolite composite material provided later.
[0051] In addition, when activated carbon is provided as a powder form rather than shaped activated carbon, although the average particle size and pore distribution can be satisfied, additional process costs due to pressure loss, separation at the rear end of the purification tower, etc. are caused, and therefore, economic feasibility is significantly reduced.
[0052] According to an exemplary embodiment of the present invention, the alumina-zeolite composite material may be a composite material of alumina and zeolite, specifically a formulation of the same kind of modified activated alumina and zeolite molecular sieve adsorbent.
[0053] The alumina-zeolite composite material according to the present invention is not limited, but specifically, for example, is in the form of beads with a crushing strength of 10N to 60N and an average particle size of 1.0mm to 5.0mm. Preferably, the alumina-zeolite composite material can be in the form of beads with a crushing strength of 20N to 60N and an average particle size of 1.0mm to 4.5mm. More preferably, the alumina-zeolite composite material can be in the form of beads with a crushing strength of 30N to 60N and an average particle size of 1.3mm to 4.5mm. Here, beads mean the shape of particles in which the composite material itself is formed in the form of beads. The crushing strength is measured according to ASTM D3102-72.
[0054] When an alumina-zeolite composite material satisfying the above physical properties is provided, the effect of purifying impurities in α-olefins is excellent, the purification capacity does not deteriorate even when exposed to excessive impurities, and an excellent purification effect can be exhibited. Such an effect can be exhibited by constituting activated carbon together.
[0055] Furthermore, when the alumina-zeolite composite material has an average particle size of less than 1.0 mm or greater than 5.0 mm, it is difficult to adsorb impurities, and in particular, long-term durability and life of purification capability may be reduced due to strong adsorption of nitrogen-containing impurities.
[0056] Furthermore, when the alumina-zeolite composite material is not in the form of beads but in the form of powder, the crushing strength and the average particle size as described above may not be satisfied, and the impurity purification effect is significantly reduced.
[0057] According to an exemplary embodiment of the present invention, the alumina-zeolite composite material may include 50 wt % to 95 wt % of alumina and 5 wt % to 50 wt % of zeolite. Preferably, the alumina-zeolite composite material may include 85 wt % to 90 wt % of alumina and 10 wt % to 15 wt % of zeolite, but is not limited thereto.
[0058] According to an exemplary embodiment of the present invention, activated carbon and alumina-zeolite composite material may be included in a weight ratio of 1:1 to 1:20. Preferably, the weight ratio may be 1:5 to 1:20. When activated carbon and alumina-zeolite composite material are included in the above ratio, the removal efficiency of impurities in α-olefins, especially nitrogen-containing impurities, can be significantly improved. In addition, even when impurities are present at low concentrations, the adsorption efficiency is excellent.
[0059] According to an exemplary embodiment of the present invention, the total content of the activated carbon and the alumina-zeolite composite material may be 1 to 20 parts by weight, preferably 4 to 20 parts by weight, based on 100 parts by weight of the α-olefin. When the activated carbon and the alumina-zeolite composite material are included in the above content, the purification capability of impurities in the α-olefin can be maximized.
[0060] According to an exemplary embodiment of the present invention, the α-olefin may specifically be, for example, any one selected from the following or a mixture of two or more thereof: 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, etc. Preferably, the α-olefin may be any one selected from 1-hexene, 1-octene, etc. or a mixture of two or more thereof. More preferably, the α-olefin may be 1-octene.
[0061] When the purification method of α-olefin according to the present invention is performed, impurities present in α-olefin can be significantly purified. In particular, impurities present in 1-octene can be removed with significantly improved purification efficiency.
[0062] According to an exemplary embodiment of the present invention, impurities may include moisture, hydrocarbons with 6 or less carbon atoms, hydrocarbons with 10 carbon atoms, hydrocarbons with 12 or more carbon atoms, nitrogen-containing impurities, etc. Among them, the present invention can well remove the adsorption of nitrogen-containing impurities, and the nitrogen-containing impurities can specifically be amine-based compounds. For example, amine-based compounds can include dioctylamine, etc. When such substances are adsorbed in alumina-zeolite composite materials, it is impossible to remove them, and it is difficult to maintain long-term purification capabilities by permanently reducing the purification capabilities.
[0063] However, when the method for purifying α-olefin according to the present invention is carried out, a purification capacity significantly improved compared with conventional purification capacity can be achieved, and the purification life is improved, thereby allowing long-term use.
[0064] The method for purifying α-olefins according to the present invention significantly improves the problem of deterioration of the purification performance of the adsorbent and can achieve excellent impurity purification effects. Therefore, by producing or providing high-purity α-olefins, the α-olefins produced thereby can achieve high performance in various fields.
[0065] Another exemplary embodiment applies the above-mentioned method for purifying α-olefins, and is a composition for purifying α-olefins, comprising: a molded activated carbon having a carbon content of 1,200 m 2 / g or more specific surface area, an average particle size of 0.8 mm to 40 mm, and a particle size greater than 0.6 cm as measured by nitrogen adsorption. 3 / g of pore volume, pores having a pore diameter of 2 nm or more in the shaped activated carbon account for 60% or more of all pores; and
[0066] Alumina-zeolite composites.
[0067] Since the physical properties and contents of the activated carbon and the alumina-zeolite composite material are as described above, a description thereof will be omitted.
[0068] According to an exemplary embodiment of the present invention, the composition for purifying α-olefins can be applied to any one or two or more positions selected from an introduction unit, a reaction unit, a circulation unit, a recovery unit, etc. in a process capable of purification. The shape provided is not particularly limited as long as the purification effect is exhibited.
[0069] Specifically, according to an exemplary embodiment of the present invention, the composition for purifying alpha-olefins can be applied during a poly-alpha-olefin polymerization reaction in which an alpha-olefin is added as a monomer or an ethylene oligomerization reaction in which an alpha-olefin is produced. By applying the composition during a reaction in which an alpha-olefin is provided or produced as described above, impurities can be purified, high-purity alpha-olefins can be provided, and performance degradation due to impurities in various fields to be provided can be prevented. In addition, due to the long-term purification capability, a significant impurity purification effect can be achieved.
[0070] According to an exemplary embodiment of the present invention, the composition for purifying alpha-olefins can be specifically applied during poly-alpha-olefin polymerization or ethylene oligomerization, and specifically, can be applied to any one or two or more steps selected from before, during and after the reaction. Specifically, for example, the purification method can be applied before the polymerization of poly-alpha-olefins or after the ethylene oligomerization. Preferably, in order to achieve excellent impurity purification effect, particularly nitrogen-containing impurities, the composition can be applied before the poly-alpha-olefin polymerization.
[0071] According to an exemplary embodiment of the present invention, for impurity purification, a process may be performed by applying the composition for purifying α-olefin at one time by mixing activated carbon and an alumina-zeolite composite material, or sequentially applying each.
[0072] Preferably, in order to apply each sequentially, the composition may be applied as a two-agent type composition comprising activated carbon as a first agent and an alumina-zeolite composite material as a second agent.
[0073] Specifically, in an exemplary embodiment, a composition can be provided so that pretreatment is performed with the first reagent, and then posttreatment is performed with the second reagent. For example, pretreatment can be performed in a region comprising the first reagent, and then posttreatment can be performed in a region comprising the second reagent. In other aspects, the first reagent is added for pretreatment, and then the first reagent is removed, and the second reagent is added for posttreatment, but it is not limited, as long as each of the first reagent and the second reagent can be processed sequentially.
[0074] According to an exemplary embodiment of the present invention, the time for purifying impurities by the first reagent and the second reagent is not particularly limited, but the processes may be performed independently of each other for 1 hour to 48 hours, preferably 5 hours to 30 hours.
[0075] When the composition is provided as a dual-reagent type composition as described above, impurities are first purified by activated carbon acting as a guard bed, and then additional impurities are purified by the alumina-zeolite composite material, thereby having significantly improved impurity purification efficiency. In addition, the problem that impurities are adsorbed to the inside of the alumina-zeolite composite material and are not removed is prevented, thereby achieving long-term purification capability.
[0076] According to an exemplary embodiment of the present invention, the composition for purifying α-olefin has excellent selectivity for nitrogen-containing impurities among impurities in α-olefin, and thus, a purification effect with further improved selectivity for nitrogen-containing impurities can be achieved.
[0077] Hereinafter, preferred examples and comparative examples of the present invention will be described. However, the following examples are merely preferred exemplary embodiments of the present invention, and the present invention is not limited thereto.
[0078] [Measurement methods of physical properties]
[0079] 1. Crushing strength
[0080] Crush strength is measured according to ASTM D3102-72, ASTM D4179-88a.
[0081] 2. Measurement of specific surface area (BET)
[0082] The specific surface area (BET) was calculated by the Brunauer-Emmett-Teller (BET) method and the Barret-Joyner-Halenda (BJH) method via nitrogen adsorption-desorption at liquid nitrogen temperature (-196°C).
[0083] 3. Measurement of purification capacity
[0084] For 100 parts by weight of a sample containing 1,000ppm of dioctylamine, activated carbon was added to a batch reactor and then purified at room temperature at normal pressure for 24 hours. Afterwards, an alumina-zeolite composite was added to the batch reactor and purified at room temperature at normal pressure for 24 hours. (tert-butylamide) dimethyl (tetramethylcyclopentadienyl) silane titanium dichloride (IV) (4 μmol) and triphenylmethyl tetrakis (pentafluorophenyl) borate and triisobutylaluminum (as a co-catalyst) were added to 10g of the purified collected sample, and synthesized at room temperature at normal pressure. After 10 minutes, the rise in reaction temperature was measured and converted to impurity removal rate as follows. When calculating the impurity removal rate, correction was made by applying the exothermic temperature of the unpurified collected sample.
[0085] Impurity removal rate = {(exothermic temperature after purification with the corresponding adsorbent - exothermic temperature before purification) / (exothermic temperature of the fully purified collected sample - exothermic temperature before purification)} × 100
[0086] 4. Pore volume and diameter
[0087] The measurement principle of BET is as follows: when in a closed container, when a gas is adsorbed or desorbed onto a sample according to the partial pressure of the gas in the container without changing other conditions, the partial pressure change of the gas in the container is measured to calculate the adsorption amount and the specific surface area of the sample can be measured. In order to measure the mesopore size, the Barrett-Joyner-Halenda (BJH) method based on the Kelvin equation is used for calculation. In addition, in order to measure the mesopore volume, the amount of nitrogen adsorbed at a relative pressure of 0.95 or less is used for analysis.
[0088] [Example 1]
[0089] For 100 parts by weight of a sample containing 1,000 ppm of dioctylamine, 1 part by weight of activated carbon was added to a batch reactor, and then a purification treatment was performed at room temperature under normal pressure for 24 hours. Thereafter, 5 parts by weight of an alumina-zeolite composite material was added to the batch reactor, and a purification treatment was performed at room temperature under normal pressure for 24 hours.
[0090] Here, activated carbon is a carbon having a 2 / g specific surface area and 95% or more of the particles are in the form of particles with a particle size of 0.85 mm to 1.7 mm, with a particle size greater than 0.6 cm as measured by nitrogen adsorption method 3 / g of pore volume, and pores having a particle size of 2 nm or more accounted for 60.1% of all pores.
[0091] As the alumina-zeolite composite material, a bead form containing 70 wt % of alumina and 30 wt % of zeolite, having a crushing strength of 33 N and a particle diameter of 1.4 mm to 2.8 mm was used.
[0092] [Example 2]
[0093] This process was performed in the same manner as in Example 1, except that 1 part by weight of activated carbon and 3 parts by weight of the alumina-zeolite composite material were added.
[0094] [Example 3]
[0095] This process was performed in the same manner as in Example 1, except that 1 part by weight of activated carbon and 20 parts by weight of the alumina-zeolite composite material were added.
[0096] [Example 4]
[0097] The process was carried out in the same manner as in Example 1, except that the alumina-zeolite composite was added first, and then the activated carbon was added.
[0098] [Example 5]
[0099] The process was carried out in the same manner as in Example 1, except that activated carbon produced by a production method different from that of conventional activated carbon was used, the activated carbon having a carbon content of 1,460 m 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 61.1% of all pores.
[0100] [Comparative Example 1]
[0101] The process was carried out in the same manner as in Example 1, except that activated carbon was not used.
[0102] [Comparative Example 2]
[0103] This process was performed in the same manner as in Example 1, except that the alumina-zeolite composite material was not used.
[0104] [Comparative Example 3]
[0105] The process was carried out in the same manner as in Example 1, except that an activated carbon having a molecular weight of 1,445 m 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 17.1% of all pores.
[0106] [Comparative Example 4]
[0107] The process was carried out in the same manner as in Example 1, except that an activated carbon having a m 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 20.5% of all pores.
[0108] [Comparative Example 5]
[0109] The process was carried out in the same manner as in Example 1, except that an activated carbon having a m 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 40.5% of all pores.
[0110] [Comparative Example 6]
[0111] The process was carried out in the same manner as in Example 1, except that an activated carbon having a molecular weight of 1,249 m 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 28.0% of all pores.
[0112] [Comparative Example 7]
[0113] The process was carried out in the same manner as in Example 1, except that activated carbon in the form of powder was used: it had a 1,505 m 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 63.0% of all pores.
[0114] [Comparative Example 8]
[0115] The process was carried out in the same manner as in Example 1, except that activated carbon in the form of powder was used: it had a 2 The specific surface area is greater than 0.6 cm / g as measured by nitrogen adsorption. 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounted for 61.7% of all pores.
[0116] Purification capability measurement was performed using the samples purified in Examples and Comparative Examples, and the impurity removal rates are shown in Table 1 below.
[0117] [Table 1]
[0118] Impurity removal rate Example 1 97.1% Example 2 73.2% Example 3 99.0% Example 4 72.7% Example 5 88.3% Comparative Example 1 27.8% Comparative Example 2 22.0% Comparative Example 3 3.41% Comparative Example 4 22.0% Comparative Example 5 46.8% Comparative Example 6 39.0% Comparative Example 7 29.3% Comparative Example 8 29.8%
[0119] As shown in Table 1, it was confirmed that when the method for purifying α-olefin according to the present invention was performed, the impurity purification effect was remarkably good. In particular, it was confirmed that the impurity removal rate was 85% or more, which was 3 times or more of the purification efficiency of the comparative example. It was confirmed that even in the case of containing impurities from a low concentration to a high concentration of 10 ppm to 500 ppm, the α-olefin purified by the method for purifying α-olefin according to the present invention had the impurities purified to less than the detection limit.
[0120] Furthermore, upon comparison of Example 1 and Example 5, it was confirmed that when the α-olefin was treated with activated carbon and then with the alumina-zeolite composite material, a further enhanced purification effect could be achieved.
[0121] Furthermore, after comparing Examples 1 to 3, it was confirmed that when activated carbon and the alumina-zeolite composite material were included in a weight ratio of 1:5 to 1:20, purification ability was better than when the activated carbon and the alumina-zeolite composite material were included in a weight ratio of 1:3.
[0122] As in Example 5, it was confirmed that similar purification capabilities were obtained even when activated carbon having the following characteristics produced by a different production method was used: 2 / g or more, a specific surface area greater than 0.6 cm as measured by nitrogen adsorption 3 / g of pore volume and pores having a pore diameter of 2 nm or more accounting for 60% or more of all pores.
[0123] It was confirmed that the purification ability was at a minute level when neither activated carbon nor alumina-zeolite composite material was included as in Comparative Examples 1 and 2. In particular, since in Comparative Example 1, impurities were strongly adsorbed to the inside of the alumina-zeolite composite material during the purification process and the life was shortened to reduce durability, it was difficult to achieve a long-term effect.
[0124] As in Comparative Examples 3 to 6, when a configuration in which the physical properties and shapes of the activated carbon and the alumina-zeolite composite material according to the present invention were different was used, it was confirmed that the effect was slight, and thus the purification effect of the present invention was not achieved.
[0125] When activated carbon having the following characteristics but in powder form was used as in Comparative Examples 7 and 8, the effect was confirmed to be small, thereby failing to achieve the purification effect of the present invention: greater than 0.6 cm as measured by nitrogen adsorption method; 3 / g of pore volume and pores having a pore size of 2 nm or more accounting for 60% or more of all pores.
[0126] In the above, although the present invention has been described by specific matters and specific exemplary embodiments, they are provided only to help a comprehensive understanding of the present invention. Therefore, the present invention is not limited to the exemplary embodiments, and those skilled in the art to which the present invention belongs can make various modifications and changes according to the description.
[0127] Therefore, the spirit of the present invention should not be limited to the above-described exemplary embodiments, and the appended claims and all modifications equivalent to or equivalent to the claims are intended to fall within the scope and spirit of the present invention.
Claims
1. A method for purifying alpha-olefins, wherein impurities are removed by a combination of: Shaped activated carbon, the shaped activated carbon having 1,200m 2 / g or more specific surface area, an average particle size of 0.8 mm to 40 mm, and a particle size greater than 0.6 cm as measured by nitrogen adsorption method. 3 / g of pore volume, pores having a pore diameter of 2 nm or more in the shaped activated carbon account for 60% or more of all pores; and Alumina-zeolite composite materials, The impurities are amine-based compounds.
2. The method for purifying α-olefin according to claim 1, wherein the method for purifying α-olefin is performed during a poly-α-olefin polymerization reaction or an ethylene oligomerization reaction. 3 . The method for purifying α-olefin according to claim 2 , wherein the method for purifying α-olefin is performed during the polymerization reaction of the poly-α-olefin.
4. The method for purifying α-olefin according to claim 1, wherein the method for purifying α-olefin sequentially comprises treating with the activated carbon and then treating with the alumina-zeolite composite material. 5 . The method for purifying α-olefin according to claim 1 , wherein the activated carbon and the alumina-zeolite composite material are contained in a weight ratio of 1:1 to 1:
20. 6 . The method for purifying α-olefin according to claim 1 , wherein the alumina-zeolite composite material comprises 50 to 95 wt % of alumina and 5 to 50 wt % of zeolite.
7. The method for purifying α-olefin according to claim 1, wherein the α-olefin is any one selected from the group consisting of 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene and 1-dodecene, or a mixture of two or more thereof. The method for purifying α-olefin according to claim 7, wherein the α-olefin is any one selected from 1-hexene and 1-octene or a mixture thereof.
9. A composition for purifying alpha-olefins containing amine-containing impurities, wherein the composition comprises: Shaped activated carbon, the shaped activated carbon having 1,200m 2 / g or more specific surface area, an average particle size of 0.8 mm to 40 mm, and a particle size greater than 0.6 cm as measured by nitrogen adsorption method. 3 / g of pore volume, pores having a pore diameter of 2 nm or more in the shaped activated carbon account for 60% or more of all pores; and Alumina-zeolite composite materials, The composition for purifying α-olefin containing amine-containing impurities comprises the activated carbon as a first agent and the alumina-zeolite composite material as a second agent.