Positive electrode active material, preparation method thereof and lithium secondary battery containing the same
By forming a coating containing B, LiOH, Li2CO3 and Li2SO4 on the surface of lithium metal oxide particles, the problems of structural collapse and low thermal stability of layered cathode active materials during charging and discharging are solved, achieving high capacity and excellent performance. The high temperature life characteristics reduce the initial resistance and resistance increase rate.
Patent Information
- Application Number
- CN202080088648.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Existing layered cathode active materials are prone to structural collapse during charging and discharging. The oxidation number problem leads to low thermal stability and difficulty in commercialization. The initial resistance and resistance increase rate are high, which affects the high capacity and high temperature life characteristics of the battery. .
A coating is formed on the surface of lithium metal oxide particles. The coating contains B, LiOH, Li2CO3 and Li2SO4. It is prepared through co-precipitation reaction and secondary heat treatment technology. The content of B, LiOH, Li2CO3 and Li2SO4 in the coating is within a specific range. Improve electrochemical stability and high temperature life characteristics.
It significantly reduces the initial resistance and resistance increase rate, improves the high capacity and high-temperature life characteristics of the cathode active material, and is suitable for use in high-energy-density lithium secondary batteries.
Smart Images

Figure CN114846649B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material, a preparation method thereof and a lithium secondary battery comprising the same. Background Art
[0002] In recent years, with the explosive growth in demand for IT mobile devices and small electric drive devices (electric bicycles, small EVs, etc.) and the increasing demand for electric vehicles with a range of more than 400 km, research and development of secondary batteries with high capacity and high energy density are actively carried out worldwide.
[0003] In order to prepare such a high-capacity battery, a high-capacity positive electrode active material is required. Among the existing layered positive electrode active materials, the material with the highest capacity is LiNiO 2 (275 mAh / g), but it is prone to structural collapse during charge and discharge, and has low thermal stability due to oxidation number problems, making it difficult to commercialize in practice.
[0004] To solve such problems, a NCM system cathode active material was developed to improve the electrochemical stability by replacing Ni sites with heterogeneous transition metals (Co, Mn, etc.). Summary of the invention
[0005] Technical issues
[0006] This embodiment aims to provide a coating layer on the surface of lithium metal oxide particles containing B, LiOH, Li 2 CO 3 and Li 2 SO 4 Thus, a positive electrode active material can be provided which can ensure high capacity, have excellent high temperature life characteristics, and reduce initial resistance and resistance increase rate.
[0007] Technical Solution
[0008] According to an embodiment of the present invention, the positive electrode active material of a lithium secondary battery comprises: lithium metal oxide particles; and a coating layer located on at least a portion of the surface of the lithium metal oxide particles, wherein the coating layer may comprise B, LiOH, Li 2 CO 3 and Li 2 SO 4 .
[0009] The content of B may be 10 ppm to 5000 ppm based on the total amount of the positive electrode active material.
[0010] The content of LiOH may be 100 ppm to 10000 ppm based on the total amount of the positive electrode active material.
[0011] Based on the total amount of the positive electrode active material, the Li 2 CO 3 The content may be from 1000ppm to 5000ppm.
[0012] Based on the total amount of the positive electrode active material, the Li 2 SO 4 The content can be from 10ppm to 3000ppm.
[0013] The Li 2 CO 3 It can be derived from internal reactions without adding additional lithium raw materials.
[0014] The content of nickel in the metal in the lithium metal oxide particles may be 85 mol % or more.
[0015] According to another embodiment, the preparation method of the positive electrode active material of a lithium secondary battery comprises: placing a metal salt aqueous solution into a coprecipitation reactor to obtain a metal precursor; mixing the metal precursor, a lithium raw material and a doping raw material to prepare a mixture; cooling the mixture after a heat treatment; and washing and drying the product of the cooling step, mixing it with a coating forming substance, and then performing a secondary heat treatment. The coating forming substance may include a boron compound, LiOH and Li 2 SO 4 .
[0016] The secondary heat treatment may be performed at a temperature ranging from 200 to 450°C.
[0017] After the secondary heat treatment step, a step of obtaining a positive electrode active material having a coating layer is included. The coating layer may include B, LiOH, Li 2 CO 3 and Li 2 SO 4 .
[0018] The Li 2 CO 3 Can originate from internal reactions.
[0019] The boron compound may be included in the coating-forming substance in an amount of 10 ppm to 5000 ppm based on the entire coating-forming substance.
[0020] The coating layer forming substance may contain LiOH in an amount of 100 ppm to 7000 ppm based on the entire coating layer forming substance.
[0021] Based on the total coating-forming substance, the Li contained in the coating-forming substance is2 SO 4 The content can be from 10ppm to 3000ppm.
[0022] A lithium secondary battery according to still another embodiment includes: a positive electrode including the positive electrode active material according to one embodiment; a negative electrode; and a nonaqueous electrolyte.
[0023] Effects of the Invention
[0024] According to the positive electrode active material of one embodiment, the coating layer contains B, LiOH, Li 2 CO 3 and Li 2 SO 4 , which can ensure the high capacity of the positive electrode active material, has excellent high-temperature life characteristics, and can significantly reduce the initial resistance and resistance increase rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the SEM analysis result of the surface of the positive electrode active material of Example 3.
[0026] Figure 2 This is the SEM analysis result of the surface of the positive electrode active material of Comparative Example 1.
[0027] Figure 3 As shown in Examples 1 to 5, the Li contained in the coating 2 SO 4 The room temperature initial discharge capacity of the content and the resistance increase rate at high temperature.
[0028] Figure 4 The life characteristics and the resistance increase rate at high temperature according to the content of LiOH contained in the coating layer as in Examples 6 to 11 are shown.
[0029] Figure 5 The 0.1C initial capacity and initial resistance according to the B content contained in the coating layer as in Examples 18 to 20 are shown.
[0030] Figure 6 The 0.1C charge-discharge capacity and initial resistance value at 25° C. and the life span and resistance increase rate at 45° C. when the secondary heat treatment temperature is controlled as in Examples 12 to 17 are shown.
[0031] Figure 7 The results of evaluating the life characteristics of the positive electrode active materials of Comparative Example 1 and Example 3 at high temperatures are shown. DETAILED DESCRIPTION
[0032] The words first, second, third, etc. herein are used to describe various parts, components, regions, layers, and / or segments, but these parts, components, regions, layers, and / or segments should not be limited by these words. These words are only used to distinguish a certain part, component, region, layer, and / or segment from another part, component, region, layer, and / or segment. Therefore, without departing from the scope of the present invention, the first part, component, region, layer, and / or segment described below can also be described as the second part, component, region, layer, and / or segment.
[0033] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. Unless the context otherwise clearly indicates the opposite, the singular form used herein is also intended to include the plural form. "Including" used in the specification may specifically refer to a certain characteristic, field, integer, step, action, element and / or component, but does not exclude the existence or addition of other characteristics, fields, integers, steps, actions, elements, components and / or groups.
[0034] If a part is described as being "on" another part, it may be directly on the other part or there may be other parts therebetween. When a part is described as being "directly on" another part, there may be no other parts therebetween.
[0035] Although not otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. Terms defined in dictionaries should be interpreted as having the same meaning as that disclosed in the relevant technical literature and this article, and should not be interpreted in an idealized or overly formal sense.
[0036] In addition, unless otherwise specified, % means weight %, and 1 ppm means 0.0001 weight %.
[0037] The embodiments of the present invention are described in detail below so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in various different ways and is not limited to the embodiments described herein.
[0038] According to an embodiment of the positive electrode active material of a lithium secondary battery, the positive electrode active material comprises: lithium metal oxide particles; and a coating layer located on at least a portion of the surface of the lithium metal oxide particles, wherein the coating layer comprises B, LiOH, Li 2 CO 3 and Li 2 SO 4 .
[0039] More specifically, the lithium metal oxide particles may be a layered structure, due to the inclusion of B, LiOH, Li2 CO 3 and Li 2 SO 4 The coating is located on the surface of these particles, which can reduce the resistance of the surface of the positive electrode active material. As a result, the capacity can be increased and the life characteristics at high temperatures can be improved. In addition, it also has the advantage of significantly reducing the initial resistance and the resistance increase rate at high temperatures.
[0040] That is, the positive electrode active material of the present embodiment includes at least four elements or compounds as described above in the coating layer, and thus can exert a synergistic effect.
[0041] In this embodiment, the content of B may be 50 ppm to 2000 ppm, more specifically 100 ppm to 1000 ppm, based on the total amount of the positive electrode active material. When the content of B satisfies the range, the average grain size of the positive electrode active material during calcination can be reduced, thereby significantly reducing the initial resistance of the positive electrode active material and the resistance increase rate at high temperature.
[0042] The content of LiOH may be 1200 ppm to 4000 ppm, more specifically 1500 ppm to 3500 ppm, based on the total amount of the positive electrode active material. When the content of LiOH contained in the coating layer satisfies the range, high capacity may be ensured while improving life characteristics.
[0043] Based on the total amount of the positive electrode active material, the Li 2 CO 3 The content of Li may be 1000 ppm to 5000 ppm, more specifically 1500 ppm to 4000 ppm or 2000 ppm to 3500 ppm. 2 CO 3 When the content of Li satisfies the above range, the room temperature and high temperature life characteristics can be improved, and the resistance increase rate and the average leakage current value can be reduced. 2 CO 3 It is a compound derived from the reaction of a metal raw material for forming lithium metal oxide with other coating forming raw materials, and no additional coating forming raw materials need to be added.
[0044] Based on the total amount of the positive electrode active material, the Li 2 SO 4 The content of Li may be 5 ppm to 1000 ppm, more specifically 10 ppm to 700 ppm or 10 ppm to 500 ppm. 2 SO 4 When the content of MgO satisfies the above range, excellent capacity characteristics can be ensured, life characteristics can be improved, and the initial resistance value can be reduced.
[0045] As described above, since the positive electrode active material of this embodiment contains B, LiOH, Li 2 CO 3 and Li 2 SO 4 The lithium secondary battery using the positive electrode active material exhibits excellent discharge capacity, improved initial efficiency, excellent room temperature and high temperature life characteristics, and can significantly reduce initial resistance and resistance increase rate.
[0046] This effect is B, LiOH, Li 2 CO 3 and Li 2 SO 4 All are included in the coating, and if any one of them is not included, the required performance cannot be obtained.
[0047] On the other hand, in this embodiment, the nickel content in the metal of the lithium metal oxide may be 85 mol % or more, and more specifically, may be 88 mol % or 90 mol % or more.
[0048] As described in this embodiment, when the nickel content in the metal in the lithium metal oxide is 80% or more, a positive electrode active material with high output characteristics can be realized. The positive electrode active material of this embodiment having these components has a higher energy density per unit volume, so the capacity of the battery using the positive electrode active material can be increased, and it is suitable for use in electric vehicles.
[0049] According to another embodiment, the preparation method of the positive electrode active material comprises: placing a metal salt aqueous solution into a coprecipitation reactor to obtain a metal precursor; mixing the metal precursor, a lithium raw material and a doping raw material to prepare a mixture; cooling the mixture after a heat treatment; and washing and drying the product of the cooling step, mixing it with a coating forming substance, and then performing a secondary heat treatment. The coating forming substance may include a boron compound, LiOH and Li 2 SO 4 .
[0050] Firstly, the following steps are implemented: placing a metal salt aqueous solution into a co-precipitation reactor to obtain a metal precursor.
[0051] More specifically, metal raw materials for forming lithium metal oxides, such as nickel raw materials, cobalt raw materials, manganese raw materials, etc., are mixed with distilled water to prepare a metal salt aqueous solution, and then placed in a reactor for a coprecipitation process, thereby obtaining a metal precursor.
[0052] Next, the following steps are performed: the metal precursor, the lithium raw material material and the doping raw material are mixed to prepare a mixture.
[0053] The lithium metal oxide of this embodiment can be a lithium metal oxide doped with Al or the like as a doping element. At this time, with respect to the content of the doping element, for example, the doping raw material is added in a manner such that the content of Zr is 3000ppm to 4000ppm and the content of Al is 200ppm to 350ppm based on the total lithium metal oxide, thereby preparing the lithium metal oxide.
[0054] Since Zr ions occupy the Li site, Zr plays a role of a pillar, relieving the contraction of the lithium ion path during charging and discharging, thereby achieving the stability of the layered structure. In addition, Al can stabilize the layered structure of the positive electrode active material. Therefore, the life characteristics of the lithium secondary battery can be further improved. Therefore, by including these doping elements, the life characteristics of the lithium secondary battery using the positive electrode active material of the present embodiment can be further improved.
[0055] Then, the following steps are performed: the mixture is subjected to a heat treatment and then cooled.
[0056] For example, the primary heat treatment can be performed at a temperature range of 700 to 850 degrees. The primary heat treatment time can be 3 to 40 hours. When the primary heat treatment conditions meet the range, the residual lithium LiOH and Li 2 CO 3 The sum is less than 10000 ppm and the grain size is 80 nm to 210 nm, so a lithium secondary battery with excellent life and resistance characteristics and good thermal stability can be achieved.
[0057] After the heat treatment is performed, the calcined body is cooled. Specifically, the cooling step can be performed by a conventional method.
[0058] Next, the following steps are performed: the product produced in the cooling step is washed with water and dried, mixed with a coating forming substance, and then subjected to a secondary heat treatment.
[0059] The water washing and drying are used to remove residual lithium on the surface and remove moisture on the surface of the positive electrode active material after the water washing treatment. Such water washing and drying can be carried out by conventional methods.
[0060] The secondary heat treatment can be performed at a temperature range of 200 to 450°C, and the heat treatment time can be 1 hour to 12 hours. This is an appropriate temperature and time range that does not damage the high temperature life characteristics. When the secondary heat treatment process meets these conditions, B, LiOH, Li 2 CO 3 and Li 2 SO 4All included coating.
[0061] In the prepared positive electrode active materials, B, LiOH, Li 2 CO 3 and Li 2 SO 4 The respective content ranges are the same as those described in the aforementioned embodiment, and thus are not described in detail.
[0062] On the other hand, in this embodiment, the coating forming material includes a boron compound, LiOH and Li 2 SO 4 That is, the Li contained in the coating of the positive electrode active material finally obtained 2 CO 3 It is formed by the internal reaction of other raw materials added during the preparation process, without adding additional raw materials.
[0063] In the coating forming material, the content of the boron compound may be 500 ppm to 2000 ppm based on the total coating forming material. When the content of the boron compound added as the coating forming material satisfies the range, the grain size of the positive electrode active material is 80 nm to 210 nm, thus showing excellent thermal stability.
[0064] In this case, as the boron compound, for example, H 3 BO 3 , boron oxide, boron compounds containing Li, BN, B 4 C. B 2 H 6 , B 2 F 4 , B 2 Cl 4 , B 2 Br 4 , B 2 I 4 wait.
[0065] In addition, the content of the LiOH contained in the coating forming material may be 500 ppm to 3500 ppm based on the total coating forming material. When the content of the LiOH added as the coating forming material satisfies the above range, the gelation phenomenon of the slurry caused by the residual lithium is suppressed, so that the slurry can be coated on the electrode when preparing the positive electrode.
[0066] Based on the total coating forming material, the coating forming material contains Li 2 SO 4 The content of Li can be 10ppm to 1000ppm. 2 SO 4When the content of satisfies the above range, Li-BC-SO 4 The lithium ion conductor is used as the main ion conductor, thereby improving the mobility of lithium ions on the surface of the positive electrode active material, so that a lithium secondary battery with excellent life characteristics can be realized.
[0067] That is, in this embodiment, LiOH and Li 2 SO 4 The amount of added is less than the LiOH and Li present in the coating of the final positive electrode active material. 2 SO 4 This is presumably caused by the reaction of lithium present in the lithium metal oxide and the metal raw material during the secondary heat treatment after the addition of the coating forming substance.
[0068] The specific characteristics of the positive electrode active material prepared by the method as described above are the same as those described in one embodiment, and thus will not be described in detail.
[0069] In addition, in the following examples, the process conditions for preparing the positive electrode active material of this example will be described in further detail.
[0070] In another embodiment of the present invention, a lithium secondary battery is provided, which includes: a positive electrode including the positive electrode active material according to one embodiment of the present invention; a negative electrode including the negative electrode active material; and an electrolyte located between the positive electrode and the negative electrode.
[0071] The description of the positive electrode active material is the same as that of the aforementioned embodiment of the present invention, and thus will not be repeated herein.
[0072] The positive electrode active material layer may include a binder and a conductive material.
[0073] The binder plays a role in allowing the positive electrode active material particles to be well bonded to each other and allowing the positive electrode active material to be well bonded to the current collector.
[0074] The conductive material is used to impart conductivity to the electrode, and any conductive material may be used as long as it does not cause chemical changes in the constituted battery.
[0075] The negative electrode includes a current collector and a negative electrode active material layer formed on the current collector, wherein the negative electrode active material layer includes a negative electrode active material.
[0076] As the negative electrode active material, a substance capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a substance capable of doping and dedoping lithium, or a transition metal oxide may be used.
[0077] As the substance capable of reversibly inserting and extracting lithium ions, any carbon-based negative electrode active material generally used as a carbon substance in lithium ion secondary batteries can be used, and as a typical example thereof, crystalline carbon, amorphous carbon, or a combination thereof can be used.
[0078] As the alloy of the lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.
[0079] Examples of the substance capable of lithium doping and dedoping include Si, SiO x (0<x<2), Si-Y alloy (the Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, other than Si), Sn, SnO 2 , Sn-Y (wherein Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, other than Sn), etc.
[0080] Examples of the transition metal oxide include vanadium oxide, lithium vanadium oxide, etc. The negative electrode active material layer also includes a binder and may further include a conductive material.
[0081] The binder plays a role in allowing negative electrode active material particles to be well bonded to each other and allowing the negative electrode active material to be well bonded to the current collector.
[0082] The conductive material is used to impart conductivity to the electrode, and any conductive material may be used as long as it does not cause chemical changes in the constituted battery.
[0083] As the current collector, a material selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer material coated with a conductive metal, and a combination thereof may be used.
[0084] For the negative electrode and the positive electrode, an active material, a conductive material and a binder are mixed in a solvent to prepare an active material composition, and the composition is coated on a current collector to prepare the negative electrode and the positive electrode. Such an electrode preparation method is well known in the art, so a detailed description is omitted in this specification. As the solvent, N-methylpyrrolidone and the like can be used, but it is not limited thereto.
[0085] The electrolyte includes a nonaqueous organic solvent and a lithium salt.
[0086] The nonaqueous organic solvent functions as a medium through which ions participating in the electrochemical reaction of the battery can migrate.
[0087] The lithium salt is a material that functions as a lithium ion source in a battery when dissolved in an organic solvent, thereby ensuring the basic operation of a lithium secondary battery and promoting the migration of lithium ions between a positive electrode and a negative electrode.
[0088] Depending on the type of lithium secondary battery, a separator may also be present between the positive electrode and the negative electrode. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride or a multilayer film of at least two layers thereof may be used, and of course mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, polypropylene / polyethylene / polypropylene three-layer separators, etc. may be used.
[0089] For lithium secondary batteries, according to the types of separators and electrolytes used, they can be divided into lithium ion batteries, lithium ion polymer batteries and lithium polymer batteries. According to the shape, they can be divided into cylindrical, prismatic, coin and bag types. According to the size, they can be divided into block and film types. The structure and preparation method of these batteries are well known in the field, so they will not be described in detail.
[0090] Hereinafter, embodiments of the present invention will be described in detail. However, the following embodiments are examples only, and the present invention is not limited to the following embodiments, and the scope of the present invention is subject to the claims.
[0091] Preparation Example 1-Preparation of positive electrode active material precursor
[0092] The (Ni 0.92 Co 0.04 Mn 0.04 )(OH) 2 Precursor of components.
[0093] Specifically, NiSO is used as the nickel raw material. 4 6H 2 O, CoSO is used as the cobalt raw material 4 7H 2 O, MnSO as manganese raw material 4 ·H 2 O. These raw materials are dissolved in distilled water to prepare a metal salt aqueous solution.
[0094] Next, after preparing the coprecipitation reactor, N 2 Purging was performed and the reactor temperature was maintained at 50°C.
[0095] The coprecipitation reactor was added with NH 4 (OH) was used as a chelating agent, and NaOH was used to adjust the pH.
[0096] The precipitate obtained according to the co-precipitation process was filtered, washed with distilled water, and then dried in an oven at 100° C. for 24 hours to prepare a positive electrode active material precursor with an average particle size of 14.8 μm.
[0097] Comparative Example 1 - Preparation of positive electrode active material with 90% Ni
[0098] Based on 1 mol of the positive electrode active material precursor prepared in Preparation Example 1, 1.05 mol of LiOH·H 2 O (Sanquan Chemical, battery grade) and the doping raw material material are uniformly mixed to prepare a mixture. In this case, ZrO is used as the doping raw material. 2 (Aldrich, 3N), Al(OH) 3 (Aldrich, 4N), and mixed so that Zr is 3400ppm and Al is 280ppm.
[0099] The mixture was placed in a tube furnace and calcined by introducing oxygen at a rate of 200 mL / min. The calcination process was performed at 480°C for 5 hours, then heated to 760°C at a rate of 5°C / min, maintained at the temperature for 16 hours, and then the calcined product was naturally cooled to 25°C to prepare a positive electrode active material.
[0100] Comparative Example 2 - 90% Ni positive electrode active material containing 500 ppm boron
[0101] Based on 1 mol of the positive electrode active material precursor prepared in Preparation Example 1, 1.05 mol of LiOH·H 2 O (Sanquan Chemical, battery grade) and the doping raw material material are uniformly mixed to prepare a mixture. In this case, ZrO is used as the doping raw material. 2 (Aldrich, 3N), Al(OH) 3 (Aldrich, 4N), and mixed so that Zr is 3400ppm and Al is 280ppm.
[0102] The mixture was placed in a tube furnace and oxygen was introduced at a rate of 200 mL / min for calcination. The calcination process was performed at 480°C for 5 hours, then heated to 760°C at a rate of 5°C / min, maintained at this temperature for 16 hours, and then the calcined product was naturally cooled to 25°C.
[0103] Next, the cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3(Aldrich). The mixture was secondarily heat-treated at 280° C. for 5 hours to prepare a positive electrode active material having boron (B) coated on the surface.
[0104] Comparative Example 3 - containing 1700 ppm LiOH, 3000 ppm Li 2 CO 3 Ni is 90% of the positive electrode active material
[0105] The cooled product was dry-mixed with 250 ppm of LiOH in terms of Li and then subjected to secondary heat treatment. A 3D-printed carbon fiber having 1700 ppm of LiOH and 3000 ppm of Li formed on the surface was prepared by the same method as in Comparative Example 2. 2 CO 3 The coating of the positive electrode active material.
[0106] Comparative Example 4 - containing 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 30ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0107] The cooled product was dry mixed with 250 ppm LiOH, 30 ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 1700 ppm of LiOH and 3000 ppm of Li 2 CO 3 and 30ppm Li 2 SO 4 The coating of the positive electrode active material.
[0108] Example 1 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 10ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0109] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 10ppm Li 2 SO 4A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 10ppm Li 2 SO 4 The coating of the positive electrode active material.
[0110] Example 2 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 100ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0111] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 20ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 100ppm Li 2 SO 4 The coating of the positive electrode active material.
[0112] Example 3 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0113] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 30ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 150ppm Li 2 SO 4The coating of the positive electrode active material.
[0114] Example 4 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0115] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0116] Example 5 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 300ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0117] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 120ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 300ppm Li 2 SO 4 The coating of the positive electrode active material.
[0118] Example 6 - Preparation of a 500 ppm B, 1500 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO4 Ni is 90% of the positive electrode active material
[0119] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 50ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was then performed. In addition, a substrate having 500 ppm of B, 1500 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 500ppm Li 2 SO 4 The coating of the positive electrode active material.
[0120] Example 7 - Preparation of a 500 ppm B, 1600 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode material
[0121] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 100ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1600 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0122] Example 8 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode material
[0123] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 60ppm Li2 SO 4 A second heat treatment was performed, except that a surface-containing film containing 500 ppm of B, 1700 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0124] Example 9 - Preparation of a 500 ppm B, 2000 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0125] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 500ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was then performed. In addition, a substrate having 500 ppm of B, 2000 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0126] Example 10 - Preparation of a 500 ppm B, 2500 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0127] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 1000ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 2500 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 200ppm Li2 SO 4 The coating of the positive electrode active material.
[0128] Example 11 - Preparation of a 500 ppm B, 3500 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0129] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 2000ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was then performed. In addition, a substrate having 500 ppm of B, 3500 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0130] Example 12 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode material
[0131] A substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0132] Example 13 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode material
[0133] A substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of LiOH and 1000 ppm of LiOH on the surface was prepared by the same method as in Example 3 except that a secondary heat treatment was performed at 220°C. 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0134] Example 14 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode material
[0135] A substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of LiOH and 1000 ppm of LiOH on the surface was prepared by the same method as in Example 3 except that a secondary heat treatment was performed at 240°C. 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0136] Example 15 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode material
[0137] A substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of LiOH and 1000 ppm of LiOH on the surface was prepared by the same method as in Example 3 except that a secondary heat treatment was performed at 260°C. 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0138] Example 16 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0139] A substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of LiOH and 1000 ppm of LiOH on the surface was prepared by the same method as in Example 3 except that a secondary heat treatment was performed at 300°C. 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0140] Example 17 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0141] A substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of LiOH and 1000 ppm of LiOH on the surface was prepared by the same method as in Example 3 except that a secondary heat treatment was performed at 450°C. 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0142] Example 18 - Preparation of a 1000 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0143] Dry mix 1000ppm H 3 BO 3 In addition, a molten-liquid-solid-state carbon foam containing 1000 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0144] Example 19 - Preparation of a 300 ppm B, 2000 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0145] Dry mix 300ppm H 3 BO 3 In addition, a mixture containing 300 ppm of B, 2000 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0146] Example 20 - Preparation of a 100 ppm B, 2000 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0147] Dry mix 100ppm H 3 BO 3 In addition, a sample containing 100 ppm of B, 2000 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0148] Example 21 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 、1ppmLi 2 SO 4 Ni is 90% of the positive electrode active material
[0149] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 10ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 1ppm Li 2 SO 4 The coating of the positive electrode active material.
[0150] Example 22 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 5ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0151] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 10ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 5ppm Li 2 SO 4 The coating of the positive electrode active material.
[0152] Example 23 - Preparation of a 500 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 1000ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0153] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 250ppm LiOH and 10ppm Li 2 SO 4 A second heat treatment was performed, and a substrate having 500 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 1000ppm Li 2 SO 4 The coating of the positive electrode active material.
[0154] Example 24 - Preparation of a 500 ppm B, 100 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0155] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 、60ppm Li 2 SO 4 A second heat treatment was then performed. In addition, a substrate having a surface containing 500 ppm of B, 100 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0156] Example 25 - Preparation of a 500 ppm B, 7000 ppm LiOH, 3000 ppm Li 2 CO 3 , 200ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0157] The cooled product was washed with distilled water, filtered and dried, and then dry-mixed with 500 ppm of H 3 BO 3 , 4000ppm LiOH and 60ppm Li 2 SO 4 A second heat treatment was performed, except that a surface-containing film containing 500 ppm of B, 7000 ppm of LiOH, and 3000 ppm of Li 2 CO 3 , 200ppm Li 2 SO 4 The coating of the positive electrode active material.
[0158] Example 26 - Preparation of a 10 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0159] Dry mix 10ppm H 3 BO 3 In addition, a molten-liquid-solid-state carbon foam containing 10 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li2 SO 4 The coating of the positive electrode active material.
[0160] Example 27 - Preparation of a 5000 ppm B, 1700 ppm LiOH, 3000 ppm Li 2 CO 3 , 150ppm Li 2 SO 4 Ni is 90% of the positive electrode active material
[0161] Dry mix 5000ppm H 3 BO 3 In addition, a sample containing 5000 ppm of B, 1700 ppm of LiOH, 3000 ppm of Li 2 CO 3 , 150ppm Li 2 SO 4 The coating of the positive electrode active material.
[0162] (Experimental Example 1) Evaluation of electrochemical characteristics
[0163] (1) Preparation of coin-type half-cell
[0164] Coin-type half cells were prepared using the positive active materials prepared according to Examples 1 to 27 and Comparative Examples 1 to 4.
[0165] Specifically, the positive electrode active material, the Denka black conductive material and the polyvinylidene fluoride binder (trade name: KF1100) were mixed in a weight ratio of 92.5:3.5:4, and the mixture was added to an N-methyl-2-pyrrolidone solvent so that the solid content in the solvent reached about 30 weight % to prepare a positive electrode active material slurry.
[0166] The slurry was coated on an aluminum foil (Al foil, thickness: 15 μm) as a positive electrode collector using a doctor blade, dried, and then pressed to prepare a positive electrode. The positive electrode loading was about 14.6 mg / cm 2 , the compression density is about 3.2g / cm 3 .
[0167] A 2032 coin-type half-cell was prepared by conventional methods using the positive electrode, a lithium metal negative electrode (thickness 200 μm, Honzo metal), an electrolyte and a polypropylene separator. The electrolyte was 1M LiPF 6The obtained product was dissolved in a mixed solvent of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate (EMC) (mixing ratio: EC:DMC:EMC=3:4:3% by volume), and the mixed solution was used as an electrolyte solution.
[0168] (2) Evaluation of 0.1C discharge capacity at 25°C and initial resistance at room temperature
[0169] The coin-type half-cell prepared in (1) was aged at room temperature (25° C.) for 10 hours and then subjected to a charge and discharge test.
[0170] For capacity evaluation, 215 mAh / g was used as the reference capacity, and the charge and discharge conditions were CC / CV 2.5 to 4.25 V, 1 / 20 C cut-off. For initial capacity, the test was performed under 0.1 C charge / 0.1 C discharge conditions.
[0171] The resistance was calculated by measuring the voltage change within 60 seconds after applying a 0.2 C discharge current when the battery was charged to 100% at 0.2 C and 4.25 V. The results are shown in Table 1 below.
[0172] (3) Evaluation of life span and resistance increase rate at 45°C
[0173] For high temperature cycle life characteristics, the ratio of the 30th capacity to the 1st capacity was measured after 30 tests at high temperature (45°C) under 0.3C charge / 0.3C discharge conditions. For resistance, the voltage change after applying the discharge current for 60 seconds when the battery was charged to 100% at 4.25V was measured, and the resistance was calculated.
[0174] For the resistance increase rate, the initial resistance (high temperature initial resistance) was detected at high temperature (45°C), and the resistance after 30 cycles was detected by the same method as the initial resistance detection method, and its increase rate was converted into a percentage (%), thereby calculating the resistance increase rate. The detection results are shown in Table 2 below.
[0175]
Table 1
[0176]
[0177]
[0178]
Table 2
[0179]
[0180]
[0181] Table 1 shows the results of measuring initial efficiency and initial resistance of the positive electrode active materials prepared according to Examples 1 to 27 and Comparative Examples 1 to 4 at room temperature.
[0182] Table 2 shows the results of measuring the high temperature life and the resistance increase rate of the positive electrode active materials prepared according to Examples 1 to 27 and Comparative Examples 1 to 4.
[0183] Referring to Table 1 and Table 2, the results are as follows: 2 CO 3 and Li 2 SO 4 Compared with the positive electrode active materials of Comparative Examples 1 to 4, the coatings containing B, LiOH, Li 2 CO 3 and Li 2 SO 4 The initial capacity and high-temperature life characteristics of the positive electrode active materials of Examples 1 to 23 are improved as a whole, and the initial resistance, high-temperature resistance and resistance increase rate are reduced.
[0184] (Experimental Example 2) SEM Analysis of the Surface of the Positive Electrode Active Material
[0185] The surfaces of the positive electrode active materials prepared in Example 3 and Comparative Example 1 were analyzed by SEM (scanning electron microscope, JEOL JSM-6610) and are shown in Figure 1 and Figure 2 middle.
[0186] from Figure 1 and Figure 2 It was confirmed that, compared with the positive electrode active material of Comparative Example 1, the positive electrode active material of Example 3 formed a uniform coating on the surface to such an extent that no primary particles were observed.
[0187] Figure 3 As shown in Examples 1 to 5, the Li contained in the coating 2 SO 4 The room temperature initial discharge capacity of the content and the resistance increase rate at high temperature.
[0188] from Figure 3 It was confirmed that the 0.1C discharge capacity was the highest when S was 300ppm, and the resistance increase rate was the lowest when S was 500ppm.
[0189] Figure 4 The life characteristics and the resistance increase rate at high temperature according to the content of LiOH contained in the coating layer as in Examples 6 to 11 are shown.
[0190] from Figure 4 It was confirmed that when the LiOH content was 1700 ppm, the 0.1C discharge capacity was the highest and the resistance increase rate was the lowest.
[0191] Figure 5 The 0.1C initial capacity and initial resistance according to the B content contained in the coating layer as in Examples 18 to 20 are shown.
[0192] from Figure 5 It can be seen that when B is 500ppm, the 0.1C discharge capacity is the highest, and when B is 300ppm, the initial resistance is the lowest.
[0193] Figure 6 The 0.1C charge-discharge capacity and initial resistance value at 25° C. and the life span and resistance increase rate at 45° C. when the secondary heat treatment temperature is controlled as in Examples 12 to 17 are shown.
[0194] from Figure 6 It was confirmed that when the secondary heat treatment temperature was 280° C., the 0.1C discharge capacity was the highest, excellent life characteristics were obtained, and the resistance increase rate was the lowest.
[0195] Figure 7 The results of evaluating the life characteristics of the positive electrode active materials of Comparative Example 1 and Example 3 at high temperatures are shown. Figure 7 It was confirmed that in the case of Comparative Example 1, the high temperature life was approximately 71%, but in the case of Example 3, the high temperature life was approximately 91%, and the high temperature life was significantly improved.
[0196] The present invention can be implemented in various ways and is not limited to the embodiments described. A person skilled in the art of the present invention can understand that the present invention can be implemented in other specific ways without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above embodiments are exemplary in all aspects and are not intended to limit the present invention.
Claims
1. A lithium secondary battery positive electrode active material, comprising: Nickel-containing layered lithium metal oxide particles, wherein the nickel content of the metal in the nickel-containing layered lithium metal oxide particles is 85 mol % or more; and a coating layer located on at least a portion of the surface of the nickel-containing layered lithium metal oxide particles, The coating comprises B, LiOH, Li2CO3 and Li2SO4, in, Based on the total amount of the positive electrode active material, the content of B is 10 ppm to 5000 ppm. Wherein, based on the total amount of the positive electrode active material, the content of LiOH is 100 ppm to 7000 ppm, Wherein, based on the total amount of the positive electrode active material, the content of Li2CO3 is 1000ppm to 5000ppm, Wherein, based on the total positive electrode active material, the content of Li2SO4 is 10 ppm to 500 ppm.
2. The positive electrode active material for lithium secondary battery according to claim 1, wherein The Li2CO3 is derived from an internal reaction without adding additional lithium raw materials.
3. A method for preparing a positive electrode active material for a lithium secondary battery, comprising: The step of placing a metal salt aqueous solution into a co-precipitation reactor to obtain a metal precursor; a step of mixing the metal precursor, the lithium raw material and the doping raw material to prepare a mixture; A step of subjecting the mixture to a heat treatment and then cooling it; as well as The product obtained in the cooling step is washed with water and dried, mixed with a coating forming material, and then subjected to a secondary heat treatment step. The coating forming substance comprises a boron compound, LiOH and Li2SO4, The positive electrode active material of the lithium secondary battery comprises: a layered lithium metal oxide particle containing nickel; and a coating layer located on at least a portion of the surface of the layered lithium metal oxide particle containing nickel, wherein the coating layer comprises B, LiOH, Li2CO3 and Li2SO4, Wherein, based on the total amount of the positive electrode active material, the content of B is 10 ppm to 5000 ppm, Wherein, based on the total amount of the positive electrode active material, the content of LiOH is 100 ppm to 7000 ppm, Wherein, based on the total amount of the positive electrode active material, the content of Li2CO3 is 1000ppm to 5000ppm, Wherein, based on the total amount of the positive electrode active material, the content of Li2SO4 is 10 ppm to 500 ppm, The nickel content of the metal in the nickel-containing layered lithium metal oxide particles is 85 mol % or more.
4. The method for preparing a positive electrode active material for a lithium secondary battery according to claim 3, wherein: The secondary heat treatment is performed at a temperature ranging from 200 to 450°C.
5. The method for preparing a positive electrode active material for a lithium secondary battery according to claim 3, wherein: After the secondary heat treatment step, a step of obtaining a positive electrode active material having a coating formed thereon is included. The coating comprises B, LiOH, Li2CO3 and Li2SO4.
6. The method for preparing a positive electrode active material for a lithium secondary battery according to claim 5, wherein: The Li2CO3 originates from an internal reaction.
7. A lithium secondary battery comprising: A positive electrode comprising the positive electrode active material according to any one of claims 1 to 2; a negative electrode; and Non-aqueous electrolytes.