Acidic aqueous solution zinc ion secondary battery electrolyte containing betaine additive
By using betaine as an electrolyte additive in zinc-ion batteries, the electric field distribution on the zinc metal surface is controlled, solving the problem of uneven deposition on the zinc metal surface, significantly improving the stability of the zinc metal electrode and battery efficiency, and extending the cycle life.
Patent Information
- Application Number
- CN202210607739.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Zinc metal corrodes in aqueous solutions, resulting in low Coulombic efficiency and poor cycle stability. The problem of uneven deposition of zinc ions on the surface of zinc metal is difficult to solve, affecting the cycle life of the battery.
Betaine is used as an electrolyte additive to construct a weakly acidic aqueous zinc ion secondary battery electrolyte. The electric field distribution on the zinc metal surface is controlled through the molecular dipole effect, forming uniform deposition and extending the stable working cycles of the zinc metal electrode.
It significantly increases the number of stable working cycles of the zinc metal electrode to 1,000 cycles, improves the dissolution and deposition stability of the zinc electrode and the wettability of the electrode, suppresses the hydrogen evolution side reaction, and improves the Coulombic efficiency and charge utilization of the battery.
Smart Images

Figure HDA0003671014730000011 
Figure HDA0003671014730000012 
Figure HDA0003671014730000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zinc ion batteries, and in particular to an acidic aqueous solution zinc ion secondary battery electrolyte containing a betaine additive. Background Art
[0002] Zinc metal as a metal electrode has the advantages of extremely high energy density, low price, safety and stability, abundant resources, and easy processing. However, due to its corrosion in aqueous solution, the coulombic efficiency of zinc metal is low and the cycle stability is poor.
[0003] At present, in order to solve this problem, the use of cationic surfactant tetrabutylamine sulfate electrolyte additive has shown a certain improvement effect (paper author: Aruuhan Bayaguud, Xiao Luo, Yanpeng Fu, and Changbao Zhu, paper title: Cationic Surfactant-Type Electrolyte Additive Enables Three-Dimensional Dendrite-Free Zinc Anode for Stable Zinc-Ion Batteries. Paper journal: ACS Energy Letters, paper volume: 2020.5(9): p.3012-3020.). The report pointed out that when the content of tetrabutylamine sulfate additive is 0.029g·L -1 When the zinc metal is charged, it can work stably for about 500 cycles. However, in order to achieve the commercial use of metal zinc negative electrode, this number of stable working cycles is not very ideal.
[0004] The requirements of zinc metal in secondary batteries are different from those of common alkaline zinc-manganese batteries. During the charging process, the zinc metal electrode needs to have a uniform surface deposition to ensure the cycle life of the zinc electrode. In common electrolyte systems, since a single zinc ion carries two positive charges, the tip deposition caused by the uneven morphology when deposited on the zinc metal surface is more obvious. In order to solve the uneven deposition of zinc ions on the zinc metal surface, it is necessary to adjust the electric field distribution on the zinc metal surface and reduce the difference in the electric field intensity distribution on the zinc metal surface in different areas. Summary of the invention
[0005] The purpose of the present invention is to provide a weakly acidic electrolyte containing a betaine additive for a rechargeable zinc ion aqueous solution battery, solve the problem of uneven electric field distribution on the surface of zinc metal, and reduce the electric field intensity on the surface of zinc metal by utilizing the principle of orientation polarization of molecules in the electric field. In order to extend the number of cycles of stable operation of zinc metal, the present invention adopts a zwitterionic compound betaine as an electrolyte additive to form a novel aqueous zinc ion secondary battery electrolyte. Compared with cationic surfactants, betaine can construct a molecular dipole on the surface of a zinc metal electrode, can more effectively regulate the electric field distribution on the surface of zinc metal, and increase the number of stable operation cycles of the zinc metal electrode to 1000.
[0006] The invention provides the use of a betaine additive to construct a weakly acidic electrolyte.
[0007] An acidic aqueous solution zinc ion secondary battery electrolyte containing betaine additive, comprising betaine, zinc sulfate and purified water, wherein the chemical formula of the betaine is C 5 H 11 NO 2 ; Wherein: the concentration of betaine is 0.04~0.9mol·L -1 ; The concentration of zinc sulfate is 1.5 mol·L -1 .
[0008] Furthermore, the pH value of the electrolyte is about 4. In this weakly acidic environment, the reaction principle of zinc metal is Zn→Zn 2+ +2e - .
[0009] The weakly acidic zinc ion battery aqueous solution electrolyte containing a betaine additive provided by the present invention can significantly improve the stability of dissolution and deposition of zinc electrodes, and the electrolyte has good wettability to the electrodes.
[0010] Application of the above acidic aqueous solution zinc ion secondary battery electrolyte containing betaine additive in acidic aqueous solution zinc ion secondary battery. The acidic aqueous solution zinc ion secondary battery consists of a positive electrode, a negative electrode, a diaphragm between the positive and negative electrodes, and an electrolyte, wherein the electrolyte is the above acidic aqueous solution zinc ion secondary battery electrolyte containing betaine additive, the negative electrode material is metallic zinc, the diaphragm is a glass fiber filter paper membrane, and the positive electrode is prepared by coating the slurry on a round sheet (for example, with a diameter of 6 mm) of a stainless steel mesh. The slurry is prepared by mixing an active substance, a conductive agent, and a binder in a mass ratio of 7:2:1. The active substance is MnO 2 Or quinone organic compound, the conductive agent is graphite, and the binder is polytetrafluoroethylene. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1The figure is the influence of the electrolyte containing betaine additive on the Tafel curve of zinc ion secondary battery, wherein: Curve 1 is the electrolyte prepared in Comparative Example 1; Curve 2 is the electrolyte prepared in Example 1.
[0012] Figure 2 This is a graph showing the effect of an electrolyte containing a betaine additive on the cycle stability of a zinc electrode in a zinc ion secondary battery, wherein: curves 3 and 4 are electrolytes prepared in comparative example 1; curves 1 and 2 are electrolytes prepared in example 1.
[0013] Figure 3 This is a graph showing the effect of an electrolyte containing a betaine additive on the coulombic efficiency of a zinc metal electrode of a zinc ion secondary battery, wherein: Curve 2 is the electrolyte prepared in Comparative Example 1; Curve 1 is the electrolyte prepared in Example 1.
[0014] Figure 4 This is a diagram showing the effect of an electrolyte containing a betaine additive on the surface wettability of a zinc metal electrode, wherein: 1 - the electrolyte prepared in Comparative Example 1; 2 - the electrolyte prepared in Example 1. DETAILED DESCRIPTION
[0015] The specific implementation modes of the present invention are further described below in conjunction with the accompanying drawings.
[0016] The raw materials and equipment in the specific embodiments of the present invention are all known products and are obtained by purchasing commercially available products.
[0017] The technical solution of the present invention is to provide a betaine additive that is added to a weakly acidic aqueous electrolyte containing a zinc sulfate solute, which can be very effectively adsorbed on the surface of zinc metal to form a covering layer, thereby weakening the electric field distribution on the surface of the zinc metal, obtaining a uniformly deposited zinc metal surface, and achieving the purpose of inhibiting the precipitation of zinc dendrites.
[0018] The M after the number in the present invention refers to the unit, mol·L -1 .
[0019] Example 1: Preparation of an acidic aqueous zinc ion secondary battery electrolyte containing betaine additive
[0020] Betaine and zinc sulfate were dissolved in purified water at room temperature, wherein: in terms of concentration, the content of betaine was controlled at 0.04 M, and the content of zinc sulfate was controlled at 1.5 M.
[0021] Example 2: Preparation of an acidic aqueous zinc ion secondary battery electrolyte containing betaine additive
[0022] Betaine and zinc sulfate were dissolved in purified water at room temperature, wherein: in terms of concentration, the content of betaine was controlled at 0.2 M, and the content of zinc sulfate was controlled at 1.5 M.
[0023] Example 3: Preparation of an acidic aqueous zinc ion secondary battery electrolyte containing betaine additive
[0024] Betaine and zinc sulfate are dissolved in purified water at room temperature, wherein: in terms of concentration, the content of betaine is controlled at 0.4 M, and the content of zinc sulfate is controlled at 1.5 M.
[0025] Example 4: Preparation of an acidic aqueous zinc ion secondary battery electrolyte containing betaine additive
[0026] Betaine and zinc sulfate were dissolved in purified water at room temperature, wherein: in terms of concentration, the content of betaine was controlled at 0.9 M, and the content of zinc sulfate was controlled at 1.5 M.
[0027] Comparative Example 1: Preparation of an acidic aqueous zinc ion secondary battery electrolyte
[0028] Zinc sulfate is dissolved in purified water at room temperature, wherein the content of zinc sulfate is controlled at 1.5 M in terms of concentration.
[0029] Figure 1 This is a graph showing the influence of the electrolyte prepared in Comparative Example 1 (1) and Example 1 (2) on the Tafel characteristic curve of the zinc ion secondary battery. The test platform is a CHI-604E electrochemical workstation. A 20ml three-electrode electrolytic cell was used for the test. The electrolytes were tested separately using Comparative Example 1 and Example 1. The working electrode used was zinc metal with an area of 1cm×1cm and a thickness of 0.2mm. The auxiliary electrode was a platinum sheet with an area of 1cm×1cm and a thickness of 0.1mm. The test was carried out at room temperature. The reference electrode used was a silver / silver chloride electrode, and the filling solution was saturated potassium chloride. The scan rate was 10mV s -1 The results showed that the betaine additive increased the equilibrium potential from -0.93 V to -0.88 V in the weakly acidic electrolyte, and the reaction current increased from 10 -5.1 Down to 10 -5.8 Acm -2 This indicates that the electrolyte additives inhibit the probability of hydrogen evolution side reaction and reduce the rate of side reaction.
[0030] Figure 2 This is a graph showing the effect of the electrolyte prepared in Example 1 and Example 1 on the cyclic stable working characteristics of the zinc electrode of the zinc ion secondary battery. The button cell test method is used, and the button cell model is 2016. The diameter of the zinc metal electrode is 6 mm. The diaphragm used is a Whatman glass fiber filter paper membrane, model 1825-047, which is punched into a disc with a diameter of 20 mm. The two electrolytes of Example 1 and Example 1 are filled respectively. It can be seen that the Zn symmetric battery has a constant current (0.2 mA cm -2) charge and discharge working settings, after 1000 working cycles, the cut-off voltage of the battery in comparative example 1 (3, 4) showed an overall increasing trend, while the weakly acidic electrolyte in example 1 (1, 2) showed a stable trend. This indicates that the betaine additive in the electrode solution can stabilize the surface deposition process of zinc metal and improve the surface structural flatness of the zinc metal battery.
[0031] Figure 3 The effect of the electrolyte prepared in Example 1 (2) and Example 1 (1) on the working coulombic efficiency of the zinc electrode of the zinc ion secondary battery is shown in the figure. The test uses a zinc metal disc with a diameter of 6 mm as the negative electrode and a stainless steel mesh with a diameter of 6 mm as the positive electrode. -2 The battery was discharged at a current of 5 minutes, and then charged to 1V cutoff at the same current density. The charging time was taken as the effective deposition amount, and the deposition coulomb efficiency was taken as the deposition time divided by the deposition amount in 5 minutes. It can be seen that the coulomb efficiency of zinc metal dissolution deposition in the electrolyte modified with betaine additive was increased to 99%. This indicates that the hydrogen evolution side reaction of the zinc metal electrode modified with betaine additive was suppressed, and the charge utilization rate of the battery operation was improved.
[0032] Figure 4 This is a graph showing the effect of the electrolyte prepared in Example 1 (1) and Example 1 (2) on the surface wettability of the zinc metal electrode. Using a visual contact angle tester, the droplet volume was controlled at 20 μL. It can be seen that the contact angle of the electrolyte modified with the betaine additive was reduced from 48.4° to 37.7°, and the wettability was significantly improved.
[0033] The electrolyte prepared in Example 1 to Example 4 and Comparative Example 1 was tested for the zinc electrode working coulomb efficiency of the zinc ion secondary battery, and the results are shown in Table 1 below:
[0034] Table 1
[0035] Coulomb efficiency (%) Example 1 99 Example 2 99 Example 3 98 Example 4 96 Comparative Example 1 90
[0036] As shown in Table 1, when purified water is used as the solvent, when the betaine content is 0.04-0.9M and the zinc sulfate content is 1.5M, the coulombic efficiency of the zinc electrode in the weakly acidic electrolyte is higher than that without the betaine additive. This is mainly because betaine can inhibit the hydrogen evolution reaction of zinc metal on the surface of the weakly acidic electrolyte and improve the utilization efficiency of electrons.
Claims
1. An acidic aqueous solution zinc ion secondary battery electrolyte containing a betaine additive, characterized in that: It is composed of betaine, zinc sulfate and purified water, wherein the chemical formula of betaine is C5H 11 NO2; where: the concentration of betaine is 0.04~0.9mol·L -1 ; The concentration of zinc sulfate is 1.5 mol·L -1 .
2. An acidic aqueous solution zinc ion secondary battery, characterized in that: The battery consists of a positive electrode, a negative electrode, a separator between the positive and negative electrodes, and an electrolyte, wherein the electrolyte is the electrolyte according to claim 1, the negative electrode material is metallic zinc, and the separator is a glass fiber filter paper membrane.
Citation Information
Patent Citations
Preparation method and application of zinc negative electrode material for inhibiting zinc dendrites
CN113745520A
Metal zinc secondary battery
CN113937341A
Alkaline battery
JP1993062684A
Zinc negative electrode mixture, zinc negative electrode and battery
JP2014154260A
Electrolyte for zinc secondary batteries and zinc secondary battery
JP2015191781A