Polypropylene preforms

By adjusting the melting parameters of polypropylene preforms to ensure stable molding during liquid blow molding, the problem of preform rupture is solved and the applicable range of molding conditions is expanded.

CN114932673BActive Publication Date: 2024-10-25DISCMA AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210748118.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2014-10-24
Filing Date
2015-10-05
Publication Date
2024-10-25
Estimated Expiration
2035-10-05

AI Technical Summary

Technical Problem

Polypropylene preforms are prone to cracking during liquid blow molding, and stable molding conditions have not been effectively addressed.

Method used

By adjusting the relationship between the melting start temperature (Ts), melting peak temperature (Tm) and melting enthalpy (ΔHm) in the polypropylene preform to satisfy (Tm-Ts)/ΔHm = 0.60 to 1.00 to ensure that the resin The melting process of the crystallized part is easy to control and avoids the breakage of the preform.

Benefits of technology

It achieves stable completion of molding without preform breakage during the liquid blow molding process, expands the range of molding conditions, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114932673B_ABST
    Figure CN114932673B_ABST
Patent Text Reader

Abstract

A polypropylene preform for biaxial stretch blow molding using a liquid as a pressurizing medium, wherein the relationship between a melting start temperature (Ts), a melting peak temperature (Tm) and a melting enthalpy (ΔHm) is (Tm-Ts) / ΔHm=0.60 to 1.00 when measured by a differential scanning calorimeter (DSC).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polypropylene preform, and more particularly, to a polypropylene preform for biaxial stretch blow molding using a liquid as a pressurizing medium. Background Art

[0002] In recent years, plastic blow-molded containers have been used for a variety of applications due to numerous excellent characteristics such as being lightweight and having a beautiful appearance. Generally, such containers are molded by biaxial stretch blow molding a preform formed into a closed-end tube in a test tube shape in a state heated to a temperature at which stretching properties can be achieved, which is stretched vertically in the axial direction by using a stretch rod and stretched horizontally in an expanded state by blowing air into the interior of the preform from nozzles densely inserted into the tubular portion of the preform.

[0003] Meanwhile, in Patent Document 1, an invention is recorded relating to a plastic container molding method in which a preform is blow-molded by supplying a liquid (not air) as a pressurizing medium. In addition, according to this biaxial stretch blow molding method using a liquid (hereinafter sometimes referred to as "liquid blow molding"), when a liquid is used as a pressurizing medium, the filling process can be omitted by using water, tea, or soft drinks, etc., which fill the container, as a product, thereby simplifying the production line.

[0004] Prior art literature

[0005] Patent Literature

[0006] Japanese Unexamined Patent Application Publication No. 2000-43129 Summary of the invention

[0007] Problems to be Solved by the Invention

[0008] However, a problem associated with this type of liquid blow molding, particularly liquid blow molding using a polypropylene preform, is that the preform may break during molding, and the types of conditions that allow stable molding are currently still under investigation and are not yet well known.

[0009] An object of the present invention is to provide a technology that can perform stable molding by finding the optimum specifications for liquid blow molding in a polypropylene preform for biaxial stretch blow molding using a liquid as a pressurizing medium.

[0010] Means of solving the problem

[0011] The present invention is a polypropylene preform for biaxial stretch blow molding using a liquid as a pressurizing medium, wherein the relationship between the melting start temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) is (Tm-Ts) / ΔHm=0.60 to 1.00 when measured using a differential scanning calorimeter (DSC).

[0012] The inventors of the present invention have found that, by using various polypropylene preforms for liquid blow molding, when measured using a differential scanning calorimeter (DSC) made of a polypropylene resin used in the preform, the melting start temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) contribute greatly to stable molding. Specifically, when the melting peak is relatively sharp (the difference between the melting start temperature and the melting peak temperature is small), the crystalline part of the resin reaches the melting peak temperature as soon as it starts to melt, and although the amount of melting is excessively increased, making it difficult to maintain the shape of the preform, it is known that if the melting peak is wide (the difference between the melting start temperature and the melting peak is large), the melting of the crystalline part included in the resin becomes easy to control. In addition, it is known that when the melting enthalpy is too small, the crystalline part is excessively melted and it is difficult to maintain the shape of the preform, on the contrary, when it is too large, the crystalline part that is not melted becomes too much and the preform is easily broken because it is not fully stretched. That is, for stable molding, the balance between the melting peak and the melting enthalpy is critical, and when this point was further investigated, it was found that when the melting start temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) satisfied the relationship (Tm-Ts) / ΔHm=0.60~1.00, problems such as preform breakage did not occur, and stable molding could be performed.

[0013] Effects of the Invention

[0014] According to the present invention, in liquid blow molding using a polypropylene preform, problems such as preform breakage during molding do not occur, and stable molding can be performed. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a half-sectional view showing one embodiment of a polypropylene preform for liquid blow molding according to the present invention.

[0016] Figure 2 is shown using liquid blow molding by Figure 1 Side view of a preform-shaped container.

[0017] Figure 3 is a graph showing an example of measurement results from a differential scanning calorimeter (DSC). DETAILED DESCRIPTION

[0018] Hereinafter, one embodiment of a polypropylene preform for liquid blow molding (hereinafter sometimes referred to as a "preform") according to the present invention will be described in further detail.

[0019] exist Figure 1 In the figure, reference number 1 shows an embodiment of a preform according to the present invention. The preform 1 is made of polypropylene (PP) and has an overall test tube shape. More specifically, the preform includes: a bottom part 2 in a hemispherical shell shape and a cylindrical main body part 3 connected to the bottom part 2, and an opening part 4 for opening at the top of the main body part 3. In the opening part 4, a disc-shaped neck ring 5 is provided, and an external threaded part 6 is provided above the neck ring 5. The preform 1 of this embodiment has a weight of 9 g, an outer diameter of the cylindrical part of 19.4 mm, an average main body thickness of 2.3 mm, and a downward height of the neck extending from the lower surface of the neck ring to the lower surface of the bottom part 2 of 70 mm. It should be noted that in addition to injection molding, the preform 1 in this manner can also be produced by compression molding or extrusion blow molding.

[0020] Furthermore, when liquid blow molding is performed using the preform 1, the preform 1 heated to a temperature capable of achieving a stretching effect is attached to a molding die (not shown), so that the preform 1 is stretched vertically by a stretch rod of a blow molding device (not shown) and stretched in an expanded state by a pressurized liquid inserted into the preform 1 by a nozzle supplied to the opening portion 4, so that the preform 1 is molded into a desired container according to the shape of the cavity of the molding die. In the container 7 of the present embodiment, as shown in FIG. Figure 2 As shown, the bottom portion 2 and the main body portion 3 of the preform 1 are stretched, but the opening portion 4 is not stretched, and the container is a cylindrical container with a bottom (having a cylindrical bottom portion 8 and a cylindrical main body portion 9). In addition, the main body portion has an outer diameter of 66 mm, an average thickness of 0.18 mm, a height extending from the lower surface of the neck ring to the lower surface of the bottom portion is 195 mm, and a filling capacity of 420 ml.

[0021] It should be noted that there are three types of polypropylene: homopolymer, random copolymer and block copolymer (impact copolymer), but any of these can be used if they are 0.60 to 1.00 = (Tm-Ts) / ΔHm according to the preform of the present invention. Random copolymers and block copolymers are used in this example. It should be noted that in addition to being able to use random copolymers and block copolymers alone, a mixture of these can also be used.

[0022] Furthermore, in the preform according to the present invention, the melting start temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) measured by the differential scanning calorimeter (DSC) satisfy the relationship of 0.60 to 1.00 = (Tm-Ts) / ΔHm. Here, in the differential scanning calorimeter (DSC) measurement, a sample extracted from a predetermined position on the preform 1 is set in the differential scanning calorimeter, the temperature is at a set speed (10°C / min), and the melting enthalpy (ΔHm) is calculated from the surface of the endothermic peak and the melting is achieved in the temperature range of 40 to 200°C. Furthermore, the predetermined position on the preform 1 is a position where stretching has not been performed, and when a container after liquid blow molding is used, the measurement is performed by a sample extracted from the opening portion of the unstretched portion.

[0023] Examples

[0024] Liquid blow molding was performed using a variety of preforms in which the type of polypropylene was changed, and whether stable molding could be performed was confirmed. The type of polypropylene in each preform is as shown in Table 1. In Table 1, "homo" is a homopolymer, "random" is a random copolymer, and "block" is a block copolymer (impact copolymer). In addition, Comparative Examples 1 and 2 and Examples 1 to 10 are respectively single-grade resins, but Example 11 is a mixture of the random copolymer used in Example 5 and the block copolymer used in Example 8 (the proportion of the block copolymer is 20% of the whole), and Example 12 is a mixture of the random copolymer used in Example 5 and the block copolymer used in Example 9 (the proportion of the block copolymer is 20% of the whole).

[0025] Furthermore, in the examples extracted from Comparative Examples 1 and 2 and Examples 1 to 12, the melting start temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) obtained from the measurement of the differential scanning calorimeter (DSC) are as shown in Table 1. It should be noted that Figure 3 A portion of the measurement results obtained from a differential scanning calorimeter (DSC) is shown, and Figure 3 In the graph, “Homo” shows Comparative Example 2, “Random” shows Example 5, and “Impact” shows Example 9.

[0026] In the liquid blow molding of the preform, a preform heated to 130° C. for a predetermined time was used before being attached to the molding die. In addition, the pressurizing medium used was water, and the water temperature was set to 20° C. In addition, the pressure of the molding die was set to 20° C. In addition, the total vertical and horizontal stretching ratio was about ten times.

[0027] [Table 1]

[0028]

[0029] ○: There is no problem with liquid blow molding, and the range of molding conditions is wide.

[0030] Δ: The preform does not break, but the range of molding conditions is narrow.

[0031] x: The preform may break due to liquid blow molding.

[0032] As shown in Table 1, in the preforms where the melting start temperature (Ts), the melting peak temperature (Tm), and the melting enthalpy (ΔHm) in the measurement from the differential scanning calorimeter (DSC) satisfy (Tm-Ts) / ΔHm=0.60 to 1.00 (Examples 1 to 12), problems such as preform breakage did not occur in liquid blow molding, and it is understood that stable molding can be performed. Specifically, in the preforms satisfying (Tm-Ts) / ΔHm=0.88 to 0.95, since the range of molding conditions is wide, it is understood that stable molding can be performed even when dispersoids are added in mass production.

[0033] The composition of the present invention and its operating effects are described above, but the preform according to the present invention is not limited to the above-mentioned embodiments, and various changes in scope are possible according to the scope of the claims. For example, in the above-mentioned embodiments, a container having a cylindrical shape with a bottom and an internal capacity of 420 ml is described, but another shape such as a rectangular shape with a bottom, as well as a container of a more complex or larger size can be applied.

[0034] Description of the number

[0035] 1: Prefab

[0036] 2: Bottom part

[0037] 3: Main part

[0038] 4: Opening

[0039] 5: Neck ring

[0040] 6: External thread part

[0041] 7: Container

[0042] 8: Bottom part

[0043] 9: Main part

Claims

1. A method for biaxial stretch blow molding of a polypropylene preform using a liquid as a pressurized medium, comprising the following steps: heating the polypropylene preform to a temperature capable of achieving a stretching effect; attaching the heated polypropylene preform to a forming mold having a cavity in the shape of a desired container; The polypropylene preform is molded into the shape of the cavity by being stretched vertically by a stretching rod and stretched in an expanded state by injecting a pressurized liquid into the polypropylene preform, wherein the polypropylene preform has a relationship between a melting start temperature (Ts), a melting peak temperature (Tm) and a melting enthalpy (ΔHm) when measured by a differential scanning calorimeter (DSC), the relationship being defined by (Tm-Ts) / ΔHm, and (Tm-Ts) / ΔHm being in the range of 0.88 to 0.95, and the polypropylene preform has one of the following: (i) the melting start temperature (Ts) is 85.8°C, the melting peak temperature (Tm) is 141.3°C, the melting enthalpy (ΔHm) is 59.4 mj / mg, the temperature difference (Tm-Ts) between the melting peak temperature (Tm) and the melting start temperature (Ts) is 55.5°C, and the relationship among the melting start temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) is (Tm-Ts) / ΔHm=0.93; (ii) the melting onset temperature (Ts) is 72.6°C, the melting peak temperature (Tm) is 141.1°C, the melting enthalpy (ΔHm) is 74.7 mj / mg, the temperature difference (Tm-Ts) between the melting peak temperature (Tm) and the melting onset temperature (Ts) is 68.5°C, and the relationship among the melting onset temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) is (Tm-Ts) / ΔHm=0.92; (iii) a melting onset temperature (Ts) of 58.9°C, a melting peak temperature (Tm) of 123.3°C, a melting enthalpy (ΔHm) of 73.2 mj / mg, a temperature difference (Tm-Ts) between the melting peak temperature (Tm) and the melting onset temperature (Ts) of 64.4°C, and a relationship among the melting onset temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) of (Tm-Ts) / ΔHm=0.88; and (iv) the melting onset temperature (Ts) is 82.1°C, the melting peak temperature (Tm) is 150°C, the melting enthalpy (ΔHm) is 71.4 mj / mg, the temperature difference (Tm-Ts) between the melting peak temperature (Tm) and the melting onset temperature (Ts) is 67.9°C, and the relationship among the melting onset temperature (Ts), the melting peak temperature (Tm) and the melting enthalpy (ΔHm) is (Tm-Ts) / ΔHm=0.95.