A method for synthesizing carbon beads

By preparing microfluidic droplet generator technology for viscous slurry and hydrocolloids in non-polar solvents, carbon beads are generated and processed, the problem of insufficient size and structural integrity of carbon microspheres in the prior art is solved, and high Carbon bead production with mechanical strength and controllable properties.

CN115103715BActive Publication Date: 2024-11-22MILLENNIAL MATERIALS & DEVICES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180014913.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-02
Filing Date
2021-03-02
Publication Date
2024-11-22
Estimated Expiration
2041-03-02

AI Technical Summary

Technical Problem

The existing carbon microsphere synthesis methods are difficult to control the bead size and structural integrity, and commercial microfluidic systems are not suitable for the production of hard all-carbon microspheres, and lack controllable viscous carbon slurries and customized manufacturing technology.

Method used

Prepare a viscous slurry as a dispersed phase in a non-polar solvent, and prepare a viscous gel as a continuous phase using hydrocolloids, and generate spherical droplets of predetermined sizes through a microfluidic droplet generator, and form carbon beads by heat treatment or UV radiation. Combining additives to adjust physical and chemical properties.

Benefits of technology

The controllable size, morphology and physical and chemical properties of carbon beads is achieved, and carbon beads with high mechanical strength and stability are produced, suitable for composite materials and biomedical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention provides a method for synthesizing carbon beads including submicron size, micron size or millimeter size. The method can adjust the viscous slurry to synthesize carbon beads with better physicochemical properties. The method improves the tolerance of carbon beads to extreme pH and high temperature. The present invention also provides a composition for synthesizing carbon beads. The present invention also provides a microfluidic droplet generator for synthesizing carbon beads. The carbon beads synthesized by the present invention are suitable for separation, filtration, purification, wires and cables, electrodes, sensors, composite materials and additive manufacturing, and drug delivery applications.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Earliest priority date:

[0002] This application claims priority to the U.S. provisional patent application filed on March 2, 2020 (patent application number 62983863, entitled "A method for synthesizing carbon beads and its products"). Technical Field

[0003] Embodiments of the present invention relate to submicron, micron and millimeter structures, and more particularly to methods for synthesizing submicron, micron or millimeter sized carbon beads. Background Art

[0004] Spherical carbon particles with a size range of 1-80 microns produced during the spinning pitch refining process are called carbon beads. Carbon beads are available in three purity grades, such as green, carbonized, and graphitized powders. They are used as composite materials with new functions by taking advantage of electrical conductivity, thermal conductivity, and other properties. Carbon beads are also called secondary carbon microbeads, spherical carbon fines, spherical carbon powder, carbon balls, spherical carbon particles, spherical balls, etc.

[0005] Traditionally, carbon beads having submicron, micron or millimeter-sized carbon bead structures are assembled using starting materials selected from raw carbon materials (e.g., carbon black, activated carbon, pyrolyzed or natural graphite, diamond, graphene, single-walled or multi-walled carbon nanotubes, fullerenes or metallofullerenes) or carbon materials functionalized with molecules or polymers.

[0006] Over the past four decades, various methods for synthesizing carbon microbeads have been explored. U.S. Pat. No. 4,263,268A discloses a method for synthesizing carbon microbeads, wherein the disclosure discusses the use of a carbon-rich polymer source deposited in a sacrificial inorganic template and then removing the template and pyrolyzing to synthesize a porous graphite carbon composite. Aromatic hydrocarbons such as coal tar, heavy oil residues, and asphalt have been shown to form mesophase carbon beads during liquid phase carbonization (see Lü, Y. et al., "Preparation of Mesophase Carbon Microbeads from Coal Tar", Journal of Materials Science, 34, 1999). Pyrolytic graphite shells are synthesized by flame pyrolysis processes. However, each of these methods involves harsh conditions (e.g., elevated temperatures) and provides suboptimal control or no control to customize bead size.

[0007] In the paper "Two-Dimensional and Three-Dimensional All-Carbon Nanomaterial Assemblies for Tissue Engineering and Regenerative Medicine" published in the journal Annals of Biomedical Engineering in 2016, Lalwani et al. disclosed an assembly of three-dimensional micron- and millimeter-scale structures using carbon nanotubes and graphene, in which the disclosure discussed the successful assembly of three-dimensional micron- and millimeter-scale structures using carbon nanotubes and graphene by "bottom-up" (e.g., chemical vapor deposition) or "top-down" (e.g., capillary-induced self-assembly) methods. However, these structures are brittle and the structural integrity is insufficient for use in applications requiring high mechanical strength or under dynamic mechanical loading and unloading forces. These conditions are experienced in vivo by biomedical implants or in vitro by stationary phase materials for filtration and / or separation. Dynamic stresses caused by constant loading and unloading cycles in tissues (e.g., bones) or under fluid flow (in chromatographic columns) can cause fatigue and loosen the three-dimensional structure, causing it to collapse or fragment. In addition, significant batch-to-batch variability in the porosity and pore size of carbon micron- and millimeter-scale structures was noted. However, the synthesis of all carbon micro- and millimeter structures in the form of microspheres of various sizes in a controlled manner using these carbon material-binder combinations has not yet been demonstrated.

[0008] Choi, A. et al. disclosed a method for synthesizing microspheres in "Recent Advances in Engineered Microparticles and Their Emerging Applications in Biomedical Delivery and Diagnostic Applications" in 2017, which explained that the microspheres were synthesized mainly using unsaturated polymers by adopting traditional emulsion free radical polymerization with manual or mechanical (using an ultrasonicator and a homogenizer) stirring. Patent application number WO2014070987A1 discloses adjustments to the above method and the use of carbon materials such as carbon black, carbon nanotubes and graphene as stabilizers in water / oil spherical droplets known as Pickering emulsions. Shah, RK et al. disclosed in their paper "Designed Emulsions Using Microfluidics" published in the 11th issue of "Today's Materials" in 2008 that problems include polydispersity, poor reproducibility of these traditional methods, and the development of complex emulsification methods such as film extrusion, viscoelastic shear and microfilament generation. Spray devices (also called atomizers, applicators, sprayers or nozzles) discharge liquids at high speed into a gas phase (usually slow-moving air), or use electrical or ultrasonic pressure to generate droplets, which have been used in material synthesis (as described in D'Addio et al. 2013, Taksima, T. et al. 2015, and U.S. Pat. No. 7,131,597B2). Chinese patent CN104525070A discloses microbeads using atomization technology, which uses a mixture of carboxylic acid functionalized carbon nanotubes and other additives. However, these technologies are insufficient in controlling the size of the droplets.

[0009] Microfluidics-based reproducible micron-scale droplet generation for material synthesis has emerged as a promising technique (as described in papers by Choi, A. et al. 2017 and Shah, RK et al. 2008). Here, materials (usually monomers or polymers that undergo free radical polymerization) are dispersed in an organic or aqueous phase. Droplets of these dispersions are generated within millifluidic or microfluidic channels, and the material trapped within the droplets undergoes free radical polymerization in situ to form the shape of microspheres. These methods have higher precision and reproducibility than traditional atomization techniques.

[0010] Passive and active methods are used to generate droplets within microfluidic channels. Passive methods of droplet generation rely on the instability formed at the interface of two low-viscosity immiscible liquid phases to produce a specific droplet geometry at a set speed (as described in the paper by Joanicot, M. et al., 2005). The deformation of the phase interface boundary and the subsequent rupture are driven by the forces contained in the phases themselves and provided as they merge and pass through the confined channel. Passive methods also include manipulating the intrinsic properties of the materials (viscosity, interfacial tension, channel wettability, fluid density) to regulate droplet rupture (as described in the paper by Zhu, P. et al., 2017). Typically, one fluid is water (aqueous phase) and the other is an organic solvent (oil phase, such as tetradecane or hexadecane). The fluid phase that preferentially wets the channel walls will be the continuous phase (external phase), while the fluid that interacts less favorably with the channel walls forms droplets (inner phase) (as described in the paper by Joanicot, M. et al., 2005). The external carrier fluid is called the continuous phase and the internal droplet forming fluid is called the dispersed phase. Therefore, if water is the continuous phase, oil droplets will form. If oil is the continuous phase, water droplets will form. Active methods use additional energy, such as electrical, magnetic, centrifugal, optical, thermal, or mechanical, to create or enhance phase instabilities.

[0011] Microfluidics-based droplet generation techniques have been primarily explored for low-viscosity dispersions to generate spherical soft gels or hydrophobic polymer microparticles (as described in Choi, A. et al. 2017, Shah, RK et al. 2008, Chu, LY et al. 2007, and Kim, DY et al. 2018).

[0012] End-to-end microfluidics-based manufacturing solutions that use viscous raw materials as input and produce final dry products as output (customized in terms of composition, density, size, shape or porosity) are not available in the market. Current commercial technologies are not suitable or directly applicable to viscous slurries of carbon materials that can produce hard all-carbon microspheres due to the following reasons:

[0013] a) A custom setup is required that can handle viscous carbon slurries: Most commercial microfluidic systems use pure water as the dispersed phase and the continuous phase is oil (silicone, or a hydrocarbon oil like decane). The materials used to make the microfluidic channels in these chips are hydrophobic (e.g., made using polydimethylsiloxane (PDMS)). The external oil continuous phase (which is hydrophobic) preferentially wets the chip surface, ensuring proper droplet formation. However, these chips are not suitable for carbon materials. Carbon materials disperse well in a selected organic fluid (e.g., ethyl acetate). Therefore, the dispersed phase to produce droplets is this organic fluid (considered to be "oil") with the carbon slurry. The continuous phase is water (a polar solution). The surface of the glass or quartz channels is hydrophilic and ensures that the polar water-based continuous phase preferentially wets the chip surface to form droplets. Therefore, a microfluidic setup with glass channels is required.

[0014] Commercially available microfluidic devices work well with low viscosity solutions. To provide some perspective on the viscosity values ​​used in these setups, the viscosity of water is 0.89 mPa·s, and oils or organic solvents used in typical microfluidic devices are between 1 (e.g., decane) and 50 (e.g., safflower oil) mPa·s. However, droplets formed using carbon dispersions in these viscosity ranges do not have an adequate amount of carbon material per droplet. High viscosity carbon slurries (>100 mPa·s) are required. The flow pressures achievable by commercially available microfluidic syringe pumps are insufficient to push high viscosity slurry formulations through the nozzle. High pressure syringe pumps, depending on syringe size, allow a maximum pressure of between 65-600 psi, which does not produce a uniform flow rate for viscous carbon slurries. High viscosity droplet generation, using phase inversion techniques (as described in papers by Man, J. et al. 2017, Chen, H. et al. 2017, and Li, J. et al. 2018), still has not demonstrated the ability to make droplets customized to a specific size.

[0015] b) A customized setup is required to post-process the generated droplets into solid spheres. Low-density carbon slurry droplets are buoyant once they are formed. They rise immediately in the continuous phase and break apart when they reach the surface. Therefore, the carbon material within the droplets needs to stay together to form spheres during the time required to rise to the surface. Alternatively, the time frame for the carbon spheres to rise to the surface needs to be extended to provide enough time to bond together to maintain their spherical conformation.

[0016] As mentioned above, UV-activated polymerization techniques have been used to cure the droplets. However, not all UV-activatable crosslinkers can be used with carbon slurries. As mentioned above, the correct ratio of carbon material and binder is required to ensure hard-cured droplets within time limits (complete bonding through the entire volume of the droplet sphere). UV-based instant crosslinking methods or binders that lead to rapid curing of other hybrid spheres do not work the same way or efficiently for carbon materials (as described in the 2018 paper by Kim, DY et al.). The reasons for this difference are as follows. Photoinitiators used for UV curing have absorbance in the 250-400nm spectral range. Glass filters out most of the shorter wavelengths emitted by the UV light source. Optimal curing conditions require direct contact without obstruction by glass tubes or closed containers. The black color of the carbon material slurry further adds to the challenge. The opaque nature of the slurry reduces the efficiency of UV light penetrating each drop to promote complete curing. Therefore, it is necessary to determine the correct combination or composition of carbon, binder, and any other additional additives to obtain mechanically stable microspheres that do not agglomerate within the limitations imposed by the generation method.

[0017] c) Additional changes will need to be made in the slurry preparation and processing steps to produce any further structural (e.g., porosity) or functional (e.g., mechanical properties) changes in the spheres. For example, porosity changes can be accomplished by adding porogens (e.g., sodium chloride, silica, or polystyrene particles) followed by leaching or etching of the porogen (as described in Ma, PX 2001 and Haugan, E. et al. 2011) or temperature annealing (Striemer, CC et al. 2007 and Striemer, CC et al. 2006). Other changes in chemical properties (e.g., hydrophobicity) and / or physical properties (e.g., electrical, thermal, or magnetic properties) will require functionalization of the carbon material or the introduction of atoms or molecules into the carbon slurry (e.g., copper to adjust conductivity or iron to adjust magnetism). Customized spheroid preparation protocols will be required to address the specific manufacturing constraints imposed by these changes.

[0018] Therefore, there is a need for improved methods for synthesizing carbon microbeads and suitable compositions of carbon microbeads. Summary of the invention

[0019] According to one embodiment of the present invention, a method for synthesizing carbon beads is provided. The method includes preparing a viscous slurry in a non-polar solvent, which is configured to be used as a dispersed phase. The viscous slurry is prepared using an adhesive or a crosslinker molecule or a free radical polymerization initiator and at least one carbon material. Each of the adhesive and the crosslinker molecule includes a plurality of terminal carbon double bond groups and a spacer group. The method also includes preparing a viscous gel using one or more hydrocolloids, wherein the viscous gel is configured to be used as a continuous phase. In the next step, the method includes allowing the dispersed phase and the continuous phase to enter a microfluidic droplet generator to obtain spherical droplets of a predetermined size. The method also includes subjecting the spherical droplets to heat treatment or UV radiation to obtain carbon bead spherical particles. The method also includes drying the carbon bead spherical particles to obtain carbon beads of a predetermined size. According to another embodiment of the present invention, the method for synthesizing carbon beads also includes adding a first additive to the viscous slurry. The first additive is selected from a group including free radical promoters, porogens, one or more atoms and one or more molecules that adjust optical, electrical, acoustic, thermal or magnetic properties.

[0020] According to yet another embodiment of the present invention, the method for synthesizing carbon beads further comprises adding a second additive to the viscous gel to control the size of the spherical droplets. The second additive is selected from the group consisting of ammonium sulfate and sodium chloride.

[0021] According to one embodiment of the present invention, the method for synthesizing carbon beads further comprises functionalizing at least one of the internal structure and the external surface of the carbon beads with atoms, molecules or macromolecules through covalent bonds or non-covalent bonds. The internal structure comprises at least one of micropores, mesopores and macropores.

[0022] According to another embodiment of the present invention, a composition for synthesizing carbon beads is provided. The composition for synthesizing carbon beads includes a viscous slurry as a dispersed phase and a viscous gel as a continuous phase. The viscous slurry includes 0.1-20wt% of a carbon material, 50-99wt% of an adhesive or crosslinker molecule, and 1-3wt% of a suitable free radical polymerization initiator. The adhesive and crosslinker molecules contain one or more terminal carbon double bond groups and spacer groups. The free radical polymerization initiator includes benzoyl peroxide (BP) or 2,2-azobisisobutyronitrile (AIBN) or 2-hydroxy-2-methyl-phenylpropiodonate or diphenyliodonium nitrate or any combination thereof. The viscous gel accounts for about 0.05-5wt% of the composition. The viscous gel includes a hydrocolloid.

[0023] According to yet another embodiment of the present invention, the viscous slurry of the composition for synthesizing carbon beads further comprises a first additive, wherein the first additive is selected from the group consisting of free radical promoters, porogens, atoms and molecules.

[0024] According to yet another embodiment of the present invention, the viscous gel of the composition for synthesizing carbon beads further comprises a second additive for controlling the size of spherical droplets, wherein the second additive is selected from the group consisting of ammonium sulfate and sodium chloride.

[0025] According to one embodiment of the present invention, a microfluidic droplet generator for synthesizing carbon bead spherical particles having at least one of submicron size, micron size and millimeter size is provided. The microfluidic droplet generator includes a continuous phase pressure tank configured to maintain a viscous gel as a continuous phase. The microfluidic droplet generator also includes a continuous phase pressure regulator with or without a pulse solenoid coupled to the continuous phase pressure tank fluid, wherein the continuous phase pressure pulse solenoid is configured to control the flow rate and pattern of the continuous phase. The microfluidic droplet generator also includes a metering pressure pump connected to the slurry reservoir fluid, wherein the metering pressure pump (e.g., a syringe pump) is configured to control the flow of a viscous slurry loaded into the slurry reservoir as a dispersed phase. The microfluidic droplet generator includes a hydrophilic co-flow nozzle connected to the continuous phase pressure regulator with or without a pulse solenoid and the slurry reservoir fluid. The hydrophilic co-flow nozzle is configured to allow the continuous phase and the dispersed phase to mix. The microfluidic droplet generator further includes a hydrophilic reaction chamber fluidically coupled to the hydrophilic co-flow nozzle, wherein the hydrophilic reaction chamber is configured to perform a hydrophilic reaction to synthesize spherical carbon bead particles.

[0026] In order to further illustrate the advantages and features of the present invention, the present invention will be described in more detail below in conjunction with the specific embodiments shown in the accompanying drawings. It should be understood that these drawings only describe typical embodiments of the present invention and are therefore not to be considered as limiting the scope. The present invention will be described and explained with additional specificity and detail through the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present disclosure will be described and explained with additional specificity and detail in conjunction with the accompanying drawings, in which:

[0028] Figure 1 is a flow chart showing the steps involved in a carbon bead synthesis method according to an embodiment of the present invention;

[0029] Figure 2a is a schematic diagram of a microfluidic droplet generator according to an embodiment of the present invention;

[0030] Figure 2b is a schematic diagram of an enlarged view of a portion of a microfluidic droplet generator according to an embodiment of the present invention;

[0031] Figure 3 Bright field optical microscope images showing carbon microbeads prepared using various raw carbon materials and decanediol diacrylate or butanediol dimethacrylate as a binder according to an embodiment of the present invention;

[0032] Figure 4 represents a bright field optical microscope image of carbon microbeads prepared using graphene oxide and polyethylene glycol (PEG) diacrylate as a binder according to an embodiment of the present invention;

[0033] Figure 5 Represents bright-field optical microscopy images of smaller carbon microbeads (<10 μm in diameter) prepared using various pristine micrographites and decanediol dimethacrylate or butanediol dimethacrylate as a binder according to embodiments of the present invention;

[0034] Figure 6 represents a high resolution scanning electron microscope (SEM) image of carbon microbeads prepared using micrographite and decanediol dimethacrylate according to an embodiment of the present invention;

[0035] Figure 7 A scanning electron microscope (SEM) image showing cleaved carbon microbeads according to an embodiment of the present invention;

[0036] Figure 8 Represents high (top) and low (bottom) resolution scanning electron microscope (SEM) images of carbon microbeads prepared using carbon black according to embodiments of the present invention;

[0037] Fig. 9 Represents high (top) and low (bottom) resolution scanning electron microscope (SEM) images of carbon microbeads prepared using fullerenes according to embodiments of the present invention;

[0038] Fig.10 Represents low (top) and high (bottom) resolution scanning electron microscope (SEM) images of highly porous carbon microbeads prepared using micrographite according to embodiments of the present invention;

[0039] 11( a ), ( b ) and ( c ) respectively show scanning electron microscope (SEM) images of carbon microbeads prepared using carbon nanotubes, activated carbon and graphene oxide according to an embodiment of the present invention;

[0040] Furthermore, those skilled in the art will appreciate that the elements in the figures are illustrated for simplicity and may not necessarily be drawn to scale. Furthermore, one or more components of the device may have been represented in the drawings with conventional symbols with respect to the construction of the device, and the drawings may show only those specific details relevant to understanding the embodiments of the invention so as not to obscure the drawings with details that would be readily apparent to those skilled in the art having the benefit of the description herein. DETAILED DESCRIPTION

[0041] In order to promote an understanding of the principles of the present invention, reference will now be made to the embodiments shown in the accompanying drawings and specific language will be used to describe them. However, it should be understood that it is not intended to limit the scope of the present disclosure. Such changes and further modifications in the illustrated system, as well as such further applications of the principles of the present disclosure that would normally occur to a person skilled in the art, are to be construed as being within the scope of the present disclosure.

[0042] The terms "comprises," "comprising," or any other variation thereof are intended to encompass a non-exclusive inclusion, such that a process or method that includes a list of steps includes not only those steps, but may include other steps that are not explicitly listed or inherent to such a process or method. Similarly, without further limitations, one or more components, compounds, and ingredients beginning with "comprising ... -" do not exclude the presence of other components or compounds or ingredients or additional ingredients. The appearance of the phrases "in one embodiment," "in another embodiment," and similar language throughout this specification may, but do not necessarily, all refer to the same embodiment.

[0043] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs.The systems, methods, and examples provided herein are illustrative only and not limiting.

[0044] In the following specification and claims, reference will be made to a number of terms which shall be defined to have the following meanings: The singular forms "a", "an", and "the" include plural references unless the context clearly dictates otherwise.

[0045] Embodiments of the present invention relate to methods for synthesizing carbon beads and compositions of carbon beads. The present invention also provides carbon beads with spherical structures having controllable size, morphology, porosity and physicochemical properties. The controllable size of the spherical carbon beads includes submicron size, micron size or millimeter size.

[0046] Figure 1 is a flow chart showing the steps involved in a method 100 for synthesizing carbon beads according to an embodiment of the present invention. The method 100 mainly uses a viscous polar solution as a continuous phase and a viscous non-polar solution as a dispersed phase into a microfluidic system, which is different from a conventional microfluidic system.

[0047] The method 100 for synthesizing carbon beads begins with preparing a viscous slurry in a non-polar solvent, which is configured to act as a dispersed phase in step 102. The viscous slurry is prepared to be>100mPa·s. The dispersed phase flows as an inner phase. The viscous slurry is prepared using one of a binder, a crosslinker molecule, a free radical polymerization initiator, and at least one carbon material. Each of the binder and the crosslinker molecule contains a plurality of terminal carbon double bond groups and a spacer group. In one embodiment, one or more terminal carbon double bond groups include but are not limited to multifunctional acrylic groups such as methacrylate, acrylate, or aromatic groups such as styrene. In one embodiment, the spacer group is a compound including a hydrophobic chain, a hydrophilic chain, an amphiphilic chain, or any combination thereof. In one embodiment, the carbon material is selected from the group including graphite, graphene, carbon black, activated carbon, nanodiamond, carbon nanotubes, and fullerenes. The free radical polymerization initiator includes one of benzoyl peroxide (BP), 2,2-azobisisobutyronitrile (AIBN), 2-hydroxy-2-methylpropiophenone, and diphenyliodonium nitrate.

[0048] The viscous slurry should have sufficient flow to pass through or push through a metering pressure pump, where the viscosity of the viscous slurry depends on the type of carbon material. For example, a graphite material slurry mixture requires a viscosity of 206.5 mPa·s. It was found that any viscosity above this value is semi-solid in nature and difficult to push through a microchannel or metering pressure pump. Liquid forms of adhesives or cross-linking agents are considered ideal, and solvents such as dodecane and hexane can be added, up to 10 ml / mg of sample, to dilute the mixture to achieve flow conditions. As used herein, the term "dispersed phase" refers to a phase composed of particles distributed in another phase. The dispersed phase herein is a discontinuous phase. In one embodiment, the metering pressure pump may include a syringe pump.

[0049] In an optional embodiment of the present invention, in step 102, a viscous slurry is prepared in a polar solvent ( Figure 1 The viscous slurry prepared in the polar solvent is configured to be used as a dispersed phase, wherein the dispersed phase flows as an inner phase. The polar solvent used herein can be selected from water, methanol, ethanol, and the like.

[0050] In one embodiment, one or more hydrocolloids are used to prepare a viscous gel in step 104. The viscous gel is configured to be used as a continuous phase. The continuous phase flows as an external phase. The viscous gel is prepared in a polar medium, which is immiscible with a non-polar solvent. One or more hydrocolloids are selected from the group consisting of xanthan gum, gum arabic, polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG) or its derivatives or combinations. One or more hydrocolloids are configured to protect newly formed droplets from flocculation and coalescence and increase the viscosity of the continuous phase. As used herein, the term "continuous phase" refers to a phase in which particles are dispersed.

[0051] In an alternative embodiment of the present invention, the viscous gel is formed in step 104 ( Figure 1 The microfluidic droplet generator (not shown) is prepared in a non-polar solvent that is immiscible with the polar solvent. The viscous gel is configured to be used as a continuous phase, wherein the continuous phase flows as the external phase. In one embodiment, in step 106, the dispersed phase and the continuous phase enter the microfluidic droplet generator to obtain spherical droplets of a predetermined size. The predetermined size of the spherical droplets includes a size range of 10 mm to 100 nm. In a preferred embodiment, the predetermined size range of the spherical droplets is between 10 μm and 90 μm. The diameter of the spherical droplets and the size of the microbeads can be controlled (reduced or increased) by adjusting the phase flow rate and reducing the size of the internal phase slurry reservoir. Once non-polar carbon slurry droplets are formed in the polar continuous phase, they will automatically assume a spherical conformation due to the thermodynamic principle of minimum interfacial energy. The contents within the spherical droplets need to be completely combined together to achieve the desired mechanical stability, separated from the high viscosity continuous phase, washed and dried to produce usable hard beads.

[0052] In the present invention, the theoretical value of the radius r of the spherical droplet is formed using the equation given by Thorsen et al., where the equation is as follows:

[0053]

[0054] Where γ = interfacial tension between water and oil,

[0055] μ = viscosity of the continuous phase,

[0056] Where U = fluid velocity, r c = channel radius.

[0057] A two-fold discrepancy between the actual and predicted droplet sizes was noted.

[0058] In the present invention, various empirical experiments were performed in the absence of reliable guidance from the prior art due to the unpredictability and number of variables. Optimization of droplet formation showed that spherical droplets can be achieved by varying the phase velocity parameters. It was observed that the external phase must flow much faster than the internal phase to produce the desired monodisperse spherical droplets. Such results provide an insight that the droplet diameter and therefore the microbead size can be controlled (reduced or increased) by adjusting the phase flow rates and reducing the internal phase slurry reservoir size. Carbon beads were synthesized using Equation 1 and the expected droplet diameter was calculated to be 776 μm, where the actual droplet diameter obtained was equal to 90 μm, with an error of 762%.

[0059] In one embodiment, the spherical droplets are subjected to heat treatment or UV radiation to obtain carbon bead spherical particles in step 108. Subjecting the droplets to UV radiation or heat treatment helps the slurry mixture to polymerize and harden in situ as they flow into the capture container. In one embodiment, a temperature oven is used for heat treatment.

[0060] Furthermore, the carbon bead spherical particles are dried in step 110 to obtain carbon beads of a predetermined size. The predetermined size of the carbon beads includes at least one of a submicron size, a micron size, and a millimeter size. The post-synthesis treatment of the carbon bead spherical particles is adjusted to enhance their physical and chemical properties. Examples of post-synthesis treatments include temperature annealing to enhance the conductivity and mechanical properties of the particles to withstand extreme pH values ​​and high temperatures, and to adjust the pore size and porosity of the carbon beads.

[0061] In an exemplary embodiment, post-synthesis treatment of the carbon beads includes temperature annealing to enhance the conductivity and mechanical properties of the particles to withstand extreme acidic and alkaline pH ranges from pH 1 to pH 14, and high temperatures from room temperature to 100°C. In a further embodiment of the method 100 for synthesizing carbon beads, a first additive is also added to the viscous slurry to enhance the physicochemical properties of the carbon bead spherical particles. The first additive includes one or more free radical promoters, one or more porogens, and one or more atoms and one or more molecules, which can control one of the following items of the carbon bead spherical particles: one of optical properties, electrical properties, acoustic properties, thermal properties, and magnetic properties. Adding free radical promoters, porogens, atoms or molecules to the viscous slurry can adjust the pore size of the carbon bead spherical particles between 0.1nm and 500μM, and the porosity range is between 1% and 99%.

[0062] One or more free radical promoters are added to improve the mechanical properties of the spherical particulate carbon beads. In one embodiment, the free radical promoter is selected from the group consisting of methyl ethyl ketone hydroperoxide, tert-butyl hydroperoxide, cumyl hydroperoxide, p-isopropyl cumyl hydroperoxide, cobalt naphthenate and cobalt acetylacetonate.

[0063] One or more porogens are added to adjust the pore size and porosity of the spherical particle carbon beads. In one embodiment, the porogen is selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1,4-butanediol, cyclohexane, benzene, toluene and NaCl crystals.

[0064] In one embodiment, in order to adjust the optical properties of the carbon bead spherical particles, one or more atoms and one or more molecules can be selected from the group including nanotubes (e.g., Vana black), nanodiamonds, silica, aluminum, silver, gold, organic fluorophores, lanthanides or their derivatives or combinations thereof.

[0065] In another embodiment, in order to adjust the electrical properties of the carbon bead spherical particles, one or more atoms and one or more molecules may be selected from the group consisting of copper, gold, silver and aluminum.

[0066] In yet another embodiment, in order to adjust the acoustic properties of the carbon bead spherical particles, one or more atoms and one or more molecules may be selected from the group consisting of sulfur hexafluoride and barium.

[0067] In one embodiment, in order to adjust the thermal or magnetic properties of the carbon bead spherical particles, one or more atoms and one or more molecules may be selected from the group consisting of iron, nickel, cobalt and oxides thereof.

[0068] In another embodiment of the method 100 for synthesizing carbon beads, the method 100 includes adding a second additive to the viscous gel to control the size of the spherical droplets. The second additive includes a group selected from ammonium sulfate and sodium chloride. Ammonium sulfate and sodium chloride are added to increase the order of polar medium cages formed around the hydrophobic slurry, thereby enhancing hydrophobic interactions.

[0069] In another embodiment of the method 100 for synthesizing carbon beads, the method 100 further comprises functionalizing the internal structure and / or external surface of the carbon beads with at least one of atoms, molecules, and macromolecules through covalent or non-covalent bonds. In such an embodiment, the internal structure comprises at least one of micropores, mesopores, and macropores. The covalent or non-covalent functionalization of the internal and external surfaces of the spherical carbon beads is modulated by atoms, molecules, and macromolecules to change the hydrophobicity, surface charge, or affinity for a specific analyte.

[0070] In another embodiment of the present invention, a composition 200 for synthesizing carbon beads is provided. The composition 200 includes a viscous slurry as a dispersed phase and a viscous gel as a continuous phase. The viscous slurry includes 0.1-20 wt% of a carbon material, 50-99 wt% of a binder or crosslinker molecule, and 1-3 wt% of a suitable free radical polymerization initiator.

[0071] In one embodiment, the carbon material is selected from the group consisting of graphite, graphene, carbon black, activated carbon, carbon nanotubes, fullerenes, nanodiamonds, or combinations thereof.

[0072] In another embodiment, the binder and crosslinker molecules each contain one or more terminal carbon double bond groups and a spacer group. One or more terminal carbon double bond groups include but are not limited to multifunctional acrylic groups such as methacrylate, acrylate or aromatic groups such as styrene. The spacer group is a compound comprising at least one of a hydrophobic chain, a hydrophilic chain, an amphiphilic chain or a combination thereof.

[0073] In yet another embodiment, the free radical polymerization initiator comprises one of 2-hydroxy-2-methyl-propiophenone and diphenyliodonium nitrate. The free radical polymerization initiator allows rapid crosslinking of double bonds in situ. The free radical polymerization initiator is used as a UV photoinitiator. The photoinitiator used for UV curing has an absorbance in the 250-400nm spectral range, so it is necessary to initiate UV light initiation by direct irradiation without obstruction by glass tubes or closed containers.

[0074] In one embodiment, the composition 200 includes 0.05-5wt% of a viscous gel. In such an embodiment, the viscous gel includes one or more hydrocolloids. The one or more hydrocolloids are selected from the group including xanthan gum, gum arabic, polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG) or a derivative or combination thereof. The one or more hydrocolloids are configured to protect the newly formed droplets from flocculation and coalescence and increase the viscosity of the continuous phase. The use of one or more hydrocolloids to increase the viscosity of the continuous phase can perform three basic functions, such as suspending the resulting spherical droplets to "hold" their material contents; significantly slowing their migration to the surface to prevent rupture due to surface tension imbalance, facilitating the formation of spherical droplets due to more deformation of the interface boundary between the merged immiscible phases due to the increase in shear force, and controlling the size of the droplets. The hydrocolloid is added to the continuous phase, i.e., the polar or aqueous phase.

[0075] In an alternative embodiment, to produce moisture-free carbon beads in applications such as active materials for battery electrode applications, one or more hydrocolloids are added to other protic polar media (immiscible with the organic dispersed phase) such as ethanol, ether or acetone.

[0076] In a further embodiment of the composition 200 for synthesizing carbon beads, the viscous slurry also includes a first additive. The first additive is selected from a group including one or more free radical promoters, one or more porogens, one or more atoms and one or more molecules. One or more free radical promoters are added to improve the mechanical properties of the spherical particle carbon beads. One or more porogens are added to adjust the pore size and porosity of the spherical particle carbon beads. One or more atoms or molecules are added to control the optical, electrical, acoustic, thermal or magnetic properties of the carbon bead spherical particles. Adding free radical promoters, porogens, atoms or molecules to the viscous slurry can adjust the pore size of the carbon bead spherical particles to between 0.1nm-500μm and the porosity range to between 1%-99%.

[0077] In a further embodiment of the composition 200 for synthesizing carbon beads, the viscous gel also includes a second additive for controlling the size of the spherical droplets. The second additive is selected from a group including ammonium sulfate and sodium chloride. Ammonium sulfate and sodium chloride are added to strengthen hydrophobic interactions by increasing the magnitude of the polar medium cage formed around the hydrophobic slurry. The first additive allows the internal structure and external surface of the carbon beads to be covalently and non-covalently functionalized with at least one of one or more atoms, one or more molecules and one or more macromolecules to change the hydrophobicity, surface charge and affinity for specific analytes of the carbon beads. The internal structure includes micropores, mesopores and macropores.

[0078] In yet another embodiment of the present invention, a microfluidic droplet generator for synthesizing carbon beads having at least one of a submicron size, a micron size, and a millimeter size is provided. Figure 2a is a schematic diagram of a microfluidic droplet generator according to an embodiment of the present invention.

[0079] As used herein, the term "microfluidic droplet generator" refers to a device for generating highly reproducible micro-sized droplets. Compared with traditional methods, a microfluidic droplet generator is able to generate droplets with much higher precision and repeatability. A microfluidic droplet generator provides droplets of a desired size at a desired flow rate and volume.

[0080] In one embodiment, the microfluidic droplet generator includes a continuous phase pressure tank 305 configured to maintain the viscous gel as a continuous phase. After loading the viscous gel, the continuous phase pressure tank is pressurized to enable the viscous gel to flow. The continuous phase pressure tank 305 is also called a continuous phase storage tank.

[0081] In one embodiment, the microfluidic droplet generator further includes a continuous phase pressure regulator 315, with or without a pulse solenoid fluidically coupled to the continuous phase pressure tank 305. The continuous phase pressure regulator 315 is configured to control the flow rate and pattern of the continuous phase. The continuous phase pressure regulator 315 is also referred to as a continuous phase pressure regulator.

[0082] In one embodiment, the microfluidic droplet generator also includes a metering pressure pump 320, which is fluidically connected to a slurry reservoir 310 filled with a viscous slurry. In one embodiment, the metering pressure pump may include a syringe pump. The metering pressure pump 320 is configured to control the flow of the viscous slurry as a dispersed phase loaded into the slurry reservoir 310. In one embodiment, the pump 320 includes an HPLC pump. The HPLC pump is capable of providing a high pressure within the range of 5000-7000psi. High pressure produces a uniform flow rate. In one embodiment, the slurry reservoir 310 is configured to optimize the snap-off of droplets manufactured with various inner diameters (i.e., 300μM to <20μM).

[0083] refer to Figure 2b , showing that the microfluidic droplet generator also includes a hydrophilic co-flow nozzle 330, which is fluidically connected to the continuous phase pressure tank 305 through a continuous phase pressure regulator 315 and a slurry reservoir 310. The hydrophilic co-flow nozzle 330 is configured to allow the continuous phase and the dispersed phase to mix at a converging portion 335. The continuous phase and the dispersed phase meet at the hydrophilic co-flow nozzle 330 and the shear force between the flowing immiscible fluids causes the droplets to snap off in an area 340 formed by a plurality of glass capillaries used as a hydrophilic container. The hydrophilic surface chemistry and reaction chamber 345 of the hydrophilic nozzle ensure that the continuous phase as the "external phase" keeps the hydrophobic dispersed phase as a separate droplet in the center of the hydrophilic nozzle. The microfluidic droplet generator is able to replace commercially available nozzles and allows the size of individual droplets to be controlled. Control of the shear force between the fluid phases in the hydrophilic co-flow nozzle 330 provides precise control of the droplet snap-off, so that the droplet volume can be set.

[0084] In one embodiment, the microfluidic droplet generator includes a hydrophilic reaction chamber 345, which includes a UV lamp and is fluidically coupled to a hydrophilic co-flow nozzle 330. In such an embodiment, the hydrophilic reaction chamber 345 is configured to have a pre-designed inclination angle θ relative to the axis 350. The hydrophilic reaction chamber 345 is configured to perform a hydrophilic reaction to synthesize spherical carbon bead particles. In an exemplary embodiment, the droplets obtained by the microfluidic droplet generator include a size of 90 μm. The droplet diameter can be controlled (reduced or increased) by adjusting the phase flow rate and reducing the size of the internal phase slurry reservoir (the inner diameter of the slurry reservoir 310) to control the size of the carbon bead spherical particles. Unlike traditional microfluidic systems, microfluidic droplet generators mainly use polar solutions as continuous phases and non-polar solutions as dispersed phases.

[0085] The carbon bead spherical particles may include micro-sized particles (also called carbon microbeads) synthesized using the method 100, composition 200 and microfluidic droplet generator provided by the present invention, which are examined for properties such as pore size, porosity and mechanical properties. Figure 3 Bright field optical microscope images showing carbon microbeads prepared using various raw carbon materials and decanediol diacrylate or butanediol dimethacrylate as a binder according to an embodiment of the present invention. The first image shows carbon microbeads formed using carbon black. The second image shows fullerenes formed using carbon black. The third image shows carbon microbeads formed using micrographite. The fourth image shows carbon microbeads formed using multi-walled carbon nanotubes.

[0086] Figure 4 Bright field optical microscope image showing carbon microbeads prepared using graphene oxide and polyethylene glycol (PEG) diacrylate as a binder according to an embodiment of the present invention.

[0087] Figure 5 Bright field optical microscope images showing smaller carbon microbeads (<10 μm in diameter) prepared using various pristine micrographites and decanediol dimethacrylate as a binder according to embodiments of the present invention.

[0088] Figure 6 A high resolution scanning electron microscope (SEM) image showing carbon microbeads prepared using micrographite and decanediol dimethacrylate according to an embodiment of the present invention. The carbon microbeads are shown at a scale of 100 μm and 10 μm to highlight the size aspect.

[0089] Figure 7 A scanning electron microscope (SEM) image showing cleaved carbon microbeads according to an embodiment of the present invention.

[0090] Figure 8 High (top) and low (bottom) resolution scanning electron microscope (SEM) images showing carbon microbeads prepared using carbon black according to embodiments of the present invention.

[0091] Fig. 9 Represents high (top) and low (bottom) resolution scanning electron microscope (SEM) images of carbon microbeads prepared using fullerenes according to embodiments of the present invention.

[0092] Fig.10 Shown are low (top) and high (bottom) resolution scanning electron microscope (SEM) images of highly porous carbon microbeads prepared using micrographite according to embodiments of the present invention.

[0093] 11(a), (b) and (c) respectively show scanning electron microscope (SEM) images of carbon microbeads prepared using carbon nanotubes, activated carbon and graphene oxide according to an embodiment of the present invention.

[0094] Table 1 lists the properties of the synthesized carbon microbeads.

[0095]

[0096]

[0097] Table 1 Examples The present invention is further explained in the following specific examples, which are for illustration only and should not be construed as limiting the scope of the present invention.

[0098] Example 1

[0099] 2-Hydroxy-2-methylpropiophenone was added to 1,10-decanediol dimethacrylate at 2 vol%. The solution was vortexed for 30 seconds. Graphite (crushed <5 um) was added at 5-20 wt% and mixed at 2500 rpm for 2 minutes to obtain slurry 1 (viscosity 206.5-400 mPa·s). Next, the vial containing the solution was placed in a 30°C water bath until thermal equilibrium was reached.

[0100] Example 2

[0101] 2-Hydroxy-2-methylpropiophenone was added to 1,4-butanediol dimethacrylate at 2 vol%. The solution was vortexed for 30 seconds. 5-20 wt% of carbon black (mesoporous <500 nm) was added and mixed at 2500 rpm for 2 minutes to obtain slurry 2 (viscosity 110-200 mPa·s). Next, the vial containing the solution was placed in a 30°C water bath until thermal equilibrium was reached.

[0102] Example 3

[0103] The preparation of water-based phase (viscosity 410mPa·s) includes the preparation of water-based external phase, wherein the water-based external phase is compatible with slurry 1 or slurry 2 formulations for microfluidic droplet generators. Xanthan gum is used as a part of the continuous phase to increase phase viscosity and stabilize droplets. The increase in external phase viscosity can enhance the shear force between phases when the phases merge, which produces deformation at the interface boundary, thereby causing droplet snap-off. In addition, the glue can stabilize the droplets so that they will not be reunited, thereby eliminating the need for surfactants. The xanthan gum / water solution was prepared at a concentration of 2g / L.

[0104] Example 4

[0105] The cross-linking process involved collecting 400 ml of the continuous phase containing the droplets for each 1000 ml beaker. The beakers were placed under continuous UV (330 nm) irradiation for 3 hours and then left to stand for 1 hour. This time scale was chosen to achieve close to 100% polymerization of the monomer binder.

[0106] Example 5

[0107] The photopolymerized droplets are separated by transferring the entire contents of the beaker (continuous phase and photopolymerized droplets) to a 450 ml conical base centrifuge tube and centrifuging at 1200 rpm for 20 minutes. The supernatant is then vacuumed off. 200 ml of DI water is added to the remaining solidified bead pellets, and the entire test tube is shaken to break up the pellets for the washing step. In addition, the tube is centrifuged at 1200 RPM for another 20 minutes using a centrifuge, and the washing cycle is repeated three times.

[0108] Example 6

[0109] The washed pellets were pipetted into a separate glass beaker, then decanted and heated in an oven at 110°C for 10 minutes to 2 hours to dry to obtain dry carbon beads.

[0110] The present invention provides submicron-sized, micron-sized or millimeter-sized carbon bead spherical particles. The present invention provides the modulation of a viscous slurry for synthesizing carbon bead spherical particles with improved physicochemical properties. The method improves the ability of carbon bead spherical particles to withstand extreme pH and high temperature. The method and composition are also capable of adjusting the pore size and porosity of carbon bead spherical particles. The method and composition are capable of producing spherical droplets of a specific size using a high viscosity slurry. The combination of materials, additives, and processing steps opens up a way to synthesize customizable and customizable carbon beads, which can be used for separation, filtration, purification, wires and cables, electrodes, sensors, composite materials and additive manufacturing, and drug delivery applications. The present invention also provides a microfluidic droplet generator, which is configured to synthesize carbon bead spherical particles having at least one of submicron-sized, micron-sized, and millimeter-sized.

[0111] Although specific language has been used to describe the invention, no limitation is intended thereby. As will be apparent to those skilled in the art, various working modifications may be made to the method to implement the inventive concepts as taught herein.

[0112] The accompanying drawings and the foregoing description give examples of embodiments. It will be appreciated by those skilled in the art that one or more of the described elements may be well combined into a single functional element. Alternatively, certain elements may be split into multiple functional elements. Elements from one embodiment may be added to another embodiment. For example, the order of the processes described herein may be changed and are not limited to the manner described herein. In addition, the actions of any flow chart do not need to be performed in the order shown; nor do they necessarily need to perform all behaviors. In addition, those behaviors that do not depend on other behaviors may be performed in parallel with other behaviors. The scope of the embodiments is in no way limited by these specific examples.

Claims

1. A method for synthesizing carbon beads by a microfluidic droplet generator, comprising: preparing a viscous slurry in a non-polar solvent configured to serve as a dispersed phase, Wherein 0.1-20wt% of carbon material is used; 50-99 wt% of adhesive or cross-linking agent molecules; 1-3 wt% of free radical polymerization initiator to prepare a viscous slurry; the viscosity of the viscous slurry is greater than 100 mPa·s; wherein the binder and cross-linker molecules each comprise a plurality of terminal carbon double bond groups and a spacer group, the spacer group being a compound comprising at least one of a hydrophobic chain, a hydrophilic chain, and an amphiphilic chain; Adding a first additive to the prepared viscous slurry, wherein the first additive is selected from at least one of one or more free radical promoters, one or more porogens, and one or more atoms and one or more molecules that adjust the optical properties, electrical properties, acoustic properties, thermal properties, and magnetic properties of the carbon bead spherical particles; Using one or more hydrocolloids to prepare a 0.05-5 wt% viscous gel as a continuous phase, adding a second additive to the viscous gel, the second additive comprising ammonium sulfate and sodium chloride; The dispersed phase and the continuous phase are passed into the microfluidic droplet generator to obtain spherical droplets of a predetermined size, wherein the microfluidic droplet generator comprises a continuous phase pressure tank, a continuous phase pressure regulator, a metering pressure pump, a hydrophilic co-flow focusing nozzle and a hydrophilic reaction chamber, wherein the metering pressure pump is fluidly connected to a slurry reservoir, wherein the metering pressure pump is configured to control the flow of the viscous slurry loaded into the slurry reservoir as the dispersed phase, wherein the hydrophilic co-flow focusing nozzle is fluidly connected to the continuous phase pressure regulator and the slurry reservoir, wherein the hydrophilic co-flow focusing nozzle is configured to control droplet breakoff to set droplet volume; and wherein the microfluidic droplet generator is configured to enable a viscous slurry as a dispersed phase and a viscous gel as a continuous phase to flow separately through a microchannel meeting at an intersection where the viscous slurry flow is broken into droplets by the viscous gel flow; subjecting the spherical liquid droplets to one of heat treatment and ultraviolet radiation to obtain spherical particles of carbon beads; drying the carbon bead spherical particles to obtain carbon beads of a predetermined size, wherein the predetermined size of the carbon beads includes submicron size, micron size and millimeter size; and Post-synthesis treatment of carbon bead spherical particles, including temperature annealing.

2. The method according to claim 1, wherein the carbon material is selected from at least one of graphite, graphene, carbon black, activated carbon, nanodiamond, carbon nanotube and fullerene.

3. The method according to claim 1, wherein the free radical polymerization initiator comprises at least one of benzoyl peroxide, 2,2-azo-bis-isobutyronitrile, 2-hydroxy-2-methyl-propiophenone and diphenyliodonium nitrate.

4. The method of claim 1, wherein the viscous gel is prepared in a polar medium that is immiscible with a non-polar solvent. The method of claim 1 , wherein the predetermined size of the spherical droplet comprises a range from 100 nm to 10 mm. The method of claim 1 , wherein the predetermined size of the spherical droplet comprises a range of 10 μm to 90 μm.

7. The method according to claim 1, wherein the hydrocolloid is selected from at least one of xanthan gum, gum arabic, polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene glycol.

8. The method according to claim 1, wherein the free radical accelerator is selected from at least one of methyl ethyl ketone hydroperoxide, tert-butyl hydroperoxide, cobalt naphthenate and cobalt acetylacetonate.

9. The method according to claim 1, wherein the porogen is selected from at least one of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1,4-butanediol, cyclohexane, benzene and NaCl crystals.

10. The method according to claim 1, wherein in order to adjust the optical properties of the carbon bead spherical particles, the one or more atoms and one or more molecules are selected from at least one of nanotubes, nanodiamonds, silica, aluminum, silver, gold, organic fluorophores, and lanthanides.

11. The method according to claim 1, wherein in order to adjust the electrical properties of the carbon bead spherical particles, the one or more atoms and one or more molecules are selected from at least one of copper, gold, silver and aluminum.

12. The method according to claim 1, wherein the one or more atoms and one or more molecules are selected from at least one of sulfur hexafluoride and barium in order to adjust the acoustic properties of the carbon bead spherical particles.

13. The method according to claim 1, wherein one of thermal properties and magnetic properties of the carbon bead spherical particles is adjusted, and the one or more atoms and one or more molecules are selected from at least one of iron, nickel, cobalt and oxides thereof.

14. The method according to claim 1, further comprising functionalizing at least one of the internal structure and the external surface of the carbon bead with at least one of atoms and molecules through one of covalent bonds and non-covalent bonds, The internal structure includes at least one of micropores, mesopores and macropores.

15. The method of claim 1, wherein the microfluidic droplet generator comprises: the continuous phase pressure tank configured to maintain the viscous gel as the continuous phase; the continuous phase pressure regulator fluidly coupled to the continuous phase pressure tank, wherein the continuous phase pressure regulator is configured to control the flow rate and pattern of the continuous phase; and The hydrophilic reaction chamber is fluidically coupled to the hydrophilic co-flow focusing nozzle, wherein the hydrophilic reaction chamber is configured to perform a hydrophilic reaction to synthesize the carbon bead spherical particles.