Manufacturing method of alignment liquid crystal film

By coating and irradiating an active energy ray-cured adhesive in a roll-to-roll manner under specific temperature and tension conditions, the problem of optical property changes in aligned liquid crystal films under high temperature conditions was solved, and more stable optical properties were achieved.

CN115113440BActive Publication Date: 2026-11-17NITTO DENKO CORP
View PDF 24 Cites 0 Cited by

Patent Information

Application Number
CN202210244594.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-18
Filing Date
2022-03-14
Publication Date
2026-11-17
Estimated Expiration
2042-03-14

AI Technical Summary

Technical Problem

In high-temperature environments, the optical properties of oriented liquid crystal films in existing technologies are prone to change, especially when they are bonded to optical layers via roll-to-roll bonding with an active energy ray-cured adhesive, resulting in a significant increase in delay characteristics.

Method used

A manufacturing method that uses a roll-to-roll method to bond an oriented liquid crystal layer and an optical layer with an active energy ray curable adhesive. By applying the adhesive within a specific temperature range and irradiating it with active energy rays under specific tension, the curing shrinkage and residual stress of the adhesive are controlled, thus ensuring the stability of the optical layer.

Benefits of technology

An oriented liquid crystal film with minimal changes in optical properties even after prolonged exposure to high temperatures was manufactured, thus improving the film's heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115113440B_ABST
    Figure CN115113440B_ABST
Patent Text Reader

Abstract

This invention provides a method for manufacturing an aligned liquid crystal film capable of producing an aligned liquid crystal film with minimal changes in optical properties even after prolonged exposure to high-temperature environments. The method involves bonding an aligned liquid crystal layer and an optical layer using an active energy beam-curable adhesive in a roll-to-roll manner. The method includes a bonding step in which the aligned liquid crystal layer and the optical layer are bonded using an active energy beam-curable adhesive in a roll-to-roll manner. The bonding step includes a coating step and an irradiation step. In the coating step, an adhesive, uncured and at a temperature of 0°C to 45°C, is coated onto at least one surface of the aligned liquid crystal layer and the optical layer. In the irradiation step, the laminate formed by stacking the aligned liquid crystal layer and the optical layer with the uncured adhesive is irradiated with an active energy beam along the transport direction of the laminate, while a tension of 70 N / 1000 mm width to 550 N / 1000 mm width is applied to the laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing an aligned liquid crystal film having an aligned liquid crystal layer having an aligned liquid crystal compound. Background Technology

[0002] As an optical film (optical anisotropic element) with functions such as optical compensation for liquid crystal display devices and prevention of external light reflection in organic EL display devices, a liquid crystal film (aligned liquid crystal film) is used, which has an aligned liquid crystal layer in which the liquid crystal compound is aligned along a predetermined direction. Compared with polymer stretched films, aligned liquid crystal films have a larger birefringence Δn, which is beneficial for the thinning and lightening of image display devices (more specifically, liquid crystal display devices, organic EL display devices, etc.). In image display devices, the aligned liquid crystal film is bonded to the organic EL panel or liquid crystal display panel in the form of a laminate integrally stacked with an adhesive or bonding agent and a polarizer, etc. (see, for example, Patent Document 1).

[0003] Liquid crystal compounds can be oriented in a specified direction by shear forces when coated onto a substrate and orientation-restricting forces of alignment films. By oriented liquid crystal compounds, aligned liquid crystal films with various optical anisotropies can be obtained. For example, a uniformly aligned liquid crystal layer in which nematic liquid crystal molecules with positive refractive index anisotropy are aligned parallel to each other on a substrate surface can be used as a positive A-plate with refractive index anisotropy of nx > ny = nz.

[0004] When using a thermotropic liquid crystal, a solution containing a liquid crystal compound (liquid crystal composition) is coated onto a substrate, and the substrate is heated so that the liquid crystal compound contained in the composition is in a liquid crystal state, thereby orienting the liquid crystal compound. When the liquid crystal composition contains a photopolymerizable liquid crystal compound (liquid crystal monomer), after orienting the liquid crystal compound, the liquid crystal composition is cured by light irradiation, thereby fixing the orientation state.

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-7700 Summary of the Invention

[0008] The problem that the invention aims to solve

[0009] For image display devices, higher durability is required, and the optical components that make up the image display device must also have minimal changes in optical properties (more specifically, delay, etc.) when exposed to high temperatures for a long time.

[0010] On the other hand, due to the influence of layers disposed adjacent to the alignment liquid crystal layer, the optical properties of the alignment liquid crystal film may change under high temperature conditions. For example, when the alignment liquid crystal layer and the optical layer (more specifically, the polarizer, transparent film, other alignment liquid crystal layers, etc.) are bonded together by an adhesive layer, there is almost no delay change under high temperature conditions. In contrast, when the alignment liquid crystal layer and the optical layer are bonded together by an active energy ray curable adhesive, there is a tendency for the delay to increase under high temperature conditions.

[0011] Furthermore, through the research of the inventors, it has been determined that the trend of delay in rising under the aforementioned high-temperature environment becomes particularly significant when the alignment liquid crystal layer and the optical layer are bonded together by means of an active energy ray curing adhesive in a roll-to-roll manner.

[0012] In view of this problem, the object of the present invention is to provide a method for manufacturing an oriented liquid crystal film that can produce an oriented liquid crystal film with minimal changes in optical properties even when exposed to high temperature environments for a long time, wherein the oriented liquid crystal layer and the optical layer are bonded together in a roll-to-roll manner using an active energy ray curable adhesive.

[0013] means for solving problems

[0014] The method for manufacturing an oriented liquid crystal film of the present invention is a method for manufacturing an oriented liquid crystal film having an oriented liquid crystal layer having an oriented liquid crystal compound, comprising a bonding step of bonding the oriented liquid crystal layer and an optical layer together by means of an active energy ray curable adhesive in a roll-to-roll manner. The bonding step comprises a coating step and an irradiation step. In the coating step, the adhesive, before curing, and at a temperature of 0°C to 45°C is coated on at least one surface of the oriented liquid crystal layer and the optical layer. In the irradiation step, the laminate formed by laminating the oriented liquid crystal layer and the optical layer with the adhesive before curing is irradiated with active energy rays along the transport direction of the laminate with a tension of 70 N / 1000 mm width to 550 N / 1000 mm width.

[0015] In one embodiment of the method for manufacturing the alignment liquid crystal film of the present invention, in the above-mentioned irradiation step, the cumulative light intensity is 450 mJ / cm. 2 ~1200mJ / cm 2 The above-mentioned laminated body was irradiated with the above-mentioned active energy rays under the specified conditions.

[0016] In one embodiment of the method for manufacturing the alignment liquid crystal film of the present invention, in the above-mentioned coating process, the above-mentioned adhesive at a temperature of 0°C to 10°C is coated on the above-mentioned surface.

[0017] In one embodiment of the method for manufacturing the alignment liquid crystal film of the present invention, the thickness of the layer formed by the adhesive after the above-mentioned irradiation process is 0.1 μm to 3.0 μm.

[0018] In one embodiment of the method for manufacturing the alignment liquid crystal film of the present invention, the liquid crystal compound is uniformly aligned in the alignment liquid crystal layer described above.

[0019] In one embodiment of the method for manufacturing the alignment liquid crystal film of the present invention, the birefringence Δn of the alignment liquid crystal layer after the above-mentioned bonding process is 0.03 or more.

[0020] In one embodiment of the method for manufacturing the oriented liquid crystal film of the present invention, the optical layer is a polarizer, a transparent film, or other oriented liquid crystal layer.

[0021] Invention Effects

[0022] The method for manufacturing an oriented liquid crystal film according to the present invention includes a bonding step in which an oriented liquid crystal layer and an optical layer are bonded together by means of an active energy ray curable adhesive in a roll-to-roll manner, and it is possible to manufacture an oriented liquid crystal film whose optical properties change little even when exposed to a high temperature environment for a long time. Attached Figure Description

[0023] Figure 1 This is an explanatory diagram illustrating an example of the method for manufacturing the alignment liquid crystal film of the present invention.

[0024] Figure 2 This is a cross-sectional view showing an example of an aligned liquid crystal film formed by laminating an aligned liquid crystal layer and an optical layer together with an adhesive.

[0025] Figure 3 A, B, C, and D are shown Figure 2 A cross-sectional view showing an example of a method for manufacturing an alignment liquid crystal film, divided by process steps.

[0026] Figure 4 This is a cross-sectional view showing an example of an aligned liquid crystal film formed by laminating an aligned liquid crystal layer and an optical layer together with an adhesive.

[0027] Figure 5 This is a cross-sectional view showing an example of an oriented liquid crystal film having an adhesive layer.

[0028] Figure 6 This is a cross-sectional view showing an example of an aligned liquid crystal film formed by laminating an aligned liquid crystal layer and an optical layer together with an adhesive.

[0029] Figure 7 This is a cross-sectional view showing an example of the layer configuration of an image display device.

[0030] Symbol Explanation

[0031] 17-layered structure

[0032] 19, 40 Adhesive layers

[0033] 21-aligned liquid crystal layer

[0034] Optical layers 22 and 41

[0035] Alignment liquid crystal films 100, 101, 102, 103, 104 Detailed Implementation

[0036] The preferred embodiments of the present invention will be described below. First, the terminology used in this specification will be explained. The thickness of the alignment liquid crystal layer, the thickness of the optical layer, and the thickness of the layer formed by the adhesive after irradiation with active energy rays (after curing) (hereinafter sometimes referred to simply as "adhesive layer") are obtained by observing a cross-section of the layer cut along the thickness direction using a transmission electron microscope (TEM), randomly selecting 10 measurement locations from the cross-sectional image, and measuring the thickness at the selected 10 measurement locations.

[0037] Hereafter, the term "system" is sometimes used after the compound name to collectively refer to the compound and its derivatives. When "system" is used after the compound name to indicate a polymer, it means that the repeating unit of the polymer is derived from the compound or its derivatives. Sometimes acrylate and methacrylate are collectively referred to as "(meth)acrylate". Sometimes acrylate and methacrylate are collectively referred to as "(meth)acrylate". Sometimes acryloyl and methacryloyl are collectively referred to as "(meth)acryloyl".

[0038] <Method for Manufacturing Alignment Liquid Crystal Film>

[0039] The method for manufacturing an oriented liquid crystal film according to this embodiment is a method for manufacturing an oriented liquid crystal film having an oriented liquid crystal layer oriented with a liquid crystal compound, which includes a bonding step in which the oriented liquid crystal layer and an optical layer are bonded together by means of an active energy ray curable adhesive in a roll-to-roll manner. The bonding step includes a coating step and an irradiation step. In the coating step, an adhesive, which is to be cured and is at a temperature of 0°C to 45°C, is coated on at least one surface of the oriented liquid crystal layer and the optical layer. In the irradiation step, the laminate formed by laminating the oriented liquid crystal layer and the optical layer with the adhesive before curing is irradiated with active energy rays while the laminate is subjected to a tension of 70 N / 1000 mm width to 550 N / 1000 mm width along the transport direction of the laminate.

[0040] According to the method for manufacturing an alignment liquid crystal film of this embodiment, there is a bonding step in which the alignment liquid crystal layer and the optical layer are bonded together by means of an active energy ray curable adhesive in a roll-to-roll manner, and it is possible to manufacture an alignment liquid crystal film in which the optical properties change little even when exposed to a high temperature environment for a long time. The reason for this is speculated as follows.

[0041] Generally, when manufacturing membrane products from membrane materials using a roll-to-roll method, the membrane material is processed under tension along the conveying direction in order to transport it. Therefore, membrane products manufactured using this method tend to exhibit anisotropy in shrinkage stress between the length direction (the conveying direction during manufacturing) and the width direction, and are prone to residual stress. Consequently, membrane products manufactured using this method tend to have optical properties (e.g., retardation) that easily change under high-temperature conditions. As mentioned above, this trend is particularly pronounced when an aligned liquid crystal layer and an optical layer are bonded using an active energy radiation-cured adhesive via a roll-to-roll method.

[0042] In contrast, in this embodiment, by setting the temperature of the adhesive in the coating process to a specific range and setting the tension applied to the laminate in the irradiation process to a specific range, the volume change (curing shrinkage) of the adhesive during curing is suppressed. As a result, the generation of residual stress caused by the curing shrinkage of the adhesive is suppressed, and therefore, it is possible to manufacture an aligned liquid crystal film with minimal changes in optical properties even when exposed to high temperatures for extended periods (hereinafter sometimes referred to as "excellent heat durability").

[0043] Hereinafter, this embodiment will be described in detail with reference to the accompanying drawings. Furthermore, for ease of understanding, the referenced... Figures 1 to 7 The figures mainly illustrate the various components schematically. For ease of preparation, the size, number, and shape of the components shown may sometimes differ from the actual figures. Furthermore, for clarity, sometimes in subsequent figures, components identical to those described in earlier figures are labeled with the same symbols, and their descriptions are omitted.

[0044] Figure 1 This is an explanatory diagram used to illustrate an example of the method for manufacturing the alignment liquid crystal film of this embodiment. For example... Figure 1 As shown, an adhesive is applied to the surface of the alignment liquid crystal layer film 10 (more specifically, the surface of the alignment liquid crystal layer in the alignment liquid crystal layer film 10) being transported in a roll-to-roll manner, forming a coating layer 12 (coating process). Furthermore, in Figure 1 In this invention, a die-coating machine is used as the coating device 11. However, the coating device is not limited in this invention. A gravure coating machine, a reverse coating machine, a bar coating machine, or other coating devices can be used depending on the viscosity of the adhesive.

[0045] Next, the optical layer film 13, which is guided by the guide roller 14 and conveyed between the first bonding roller 15 and the second bonding roller 16, and the alignment liquid crystal layer film 10 are stacked between the first bonding roller 15 and the second bonding roller 16, thereby being deposited through the coating layer 12 to form a laminate 17. At this time, the laminate 17 is formed in a state where the optical layer in the optical layer film 13 is in contact with the coating layer 12.

[0046] Next, the laminate 17 is irradiated with active energy rays (more specifically, ultraviolet rays, electron rays, etc.) using an active energy irradiation device 18 (irradiation process). During the irradiation process, the adhesive in the coating layer 12 is cured, thereby forming an adhesive layer 19, resulting in an aligned liquid crystal film 100 formed by bonding an aligned liquid crystal layer film 10 and an optical layer film 13 together via the adhesive layer 19. Examples of light sources for the active energy rays include: low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, LEDs, black lights, and chemical lamps. The illuminance of the active energy ray light source is, for example, 100 mW / cm². 2 ~1000mW / cm 2 The preferred value is 400mW / cm. 2 ~800mW / cm 2 The active energy rays can irradiate the surface containing the oriented liquid crystal film 10, the surface containing the optical film 13, or both surfaces of the laminate 17, depending on the transmittance of the active energy rays containing the oriented liquid crystal film 10 and the optical film 13.

[0047] To manufacture an alignment liquid crystal film with superior heat resistance, the thickness of the adhesive layer 19 is preferably 3.0 μm or less, more preferably 2.8 μm or less. Furthermore, to manufacture an alignment liquid crystal film with excellent adhesion reliability, the thickness of the adhesive layer 19 is preferably 0.1 μm or more, more preferably 0.5 μm or more. To ensure both adhesion reliability and superior heat resistance in the manufacture of an alignment liquid crystal film, the thickness of the adhesive layer 19 is preferably 0.1 μm to 3.0 μm, more preferably 0.5 μm to 2.8 μm. The thickness of the adhesive layer 19 can be adjusted by changing the thickness of the coating layer 12.

[0048] In reference Figure 1 In the bonding process described, tension is applied to the alignment liquid crystal film 10, the optical film 13, and the laminate 17, for example, by a jumping roller (not shown). The direction of tension application is the transport direction for any of the alignment liquid crystal film 10, the optical film 13, and the laminate 17.

[0049] In order to stably transport the laminate 17 while manufacturing an alignment liquid crystal film with better heat resistance, it is preferable to irradiate the laminate 17 with active energy rays while imbuing it with a tension of 77 N / 1000 mm width to 550 N / 1000 mm width.

[0050] To manufacture an alignment liquid crystal film with superior heat resistance, it is preferable to apply a cumulative light intensity of 450 mJ / cm² to the laminate 17. 2 ~1200mJ / cm 2 Irradiation with active energy rays under suitable conditions, preferably with a cumulative light intensity of 450 mJ / cm². 2 ~1100mJ / cm 2 Under conditions of irradiation with active energy rays, further optimized with a cumulative light intensity of 450 mJ / cm 2 ~800mJ / cm 2 Irradiation with active energy rays under specific conditions, with a further preferred cumulative light intensity of 450 mJ / cm². 2 ~600mJ / cm 2 Irradiation with active energy rays under certain conditions.

[0051] In order to manufacture an alignment liquid crystal film with better heat resistance, the temperature of the adhesive applied in the coating process is preferably 0°C to 25°C, more preferably 0°C to 10°C.

[0052] In order to stably transport the liquid crystal film 10 containing the alignment layer 10, the optical layer 13 containing the optical layer 13 and the laminate 17, their transport speed is preferably 1 m / min to 100 m / min, more preferably 5 m / min to 50 m / min.

[0053] The time from the application of the adhesive on the alignment liquid crystal film 10 in the coating process to the irradiation of the laminate 17 with active energy rays in the irradiation process is, for example, 0 seconds to 300 seconds.

[0054] In order to manufacture an alignment liquid crystal film with better heat resistance, it is preferable to satisfy the following condition 1, more preferably to satisfy the following condition 2, further preferably to satisfy the following condition 3, and even more preferably to satisfy the following condition 4.

[0055] Condition 1: The temperature of the adhesive to be coated in the coating process is 0℃~25℃, and in the irradiation process, the cumulative light intensity is 450mJ / cm. 2 ~1200mJ / cm 2 The conditions were such that the laminate 17 was irradiated with active energy rays.

[0056] Condition 2: The temperature of the adhesive to be coated in the coating process is 0℃~25℃, and in the irradiation process, the cumulative light intensity is 450mJ / cm. 2 ~800mJ / cm 2The conditions were such that the laminate 17 was irradiated with active energy rays.

[0057] Condition 3: The temperature of the adhesive to be coated in the coating process is 0℃~10℃, and in the irradiation process, the cumulative light intensity is 450mJ / cm. 2 ~1200mJ / cm 2 The conditions were such that the laminate 17 was irradiated with active energy rays.

[0058] Condition 4: The temperature of the adhesive to be coated in the coating process is 0℃~10℃, and in the irradiation process, the cumulative light intensity is 450mJ / cm. 2 ~800mJ / cm 2 The following conditions were applied to irradiate the laminate 17 with active energy rays.

[0059] Above, refer to Figure 1 An example of a method for manufacturing an alignment liquid crystal film according to this embodiment has been described, but the present invention is not limited to the above example. For example, in the above example, an adhesive is coated on the alignment liquid crystal layer, but in the present invention, the adhesive can be coated on the optical layer, or the adhesive can be coated on both the alignment liquid crystal layer and the optical layer.

[0060] Next, an example of the configuration of the alignment liquid crystal film obtained by the manufacturing method of this embodiment will be described.

[0061] Figure 2 This is a cross-sectional view showing an example of an aligned liquid crystal film obtained by the manufacturing method of this embodiment. Figure 2 The alignment liquid crystal film 101 shown includes: a support substrate 20, an alignment liquid crystal layer 21 stacked on the support substrate 20, and an optical layer 22 stacked on the alignment liquid crystal layer 21 by an adhesive layer 19.

[0062] Reference Figure 1 and Figure 3 A~D pairs Figure 2 An example of the manufacturing method of the alignment liquid crystal film 101 shown will be described. Figure 3 A through D are shown Figure 2 A cross-sectional view showing an example of a manufacturing method for the alignment liquid crystal film 101, divided by process steps.

[0063] First, prepare a liquid crystal film 10 containing an alignment liquid crystal layer 21, which is stacked on a support substrate 20. Figure 3 A). The oriented liquid crystal layer film 10 is obtained, for example, by coating a liquid crystal composition containing a liquid crystal compound onto a support substrate 20, oriented the liquid crystal compound in a predetermined direction, and then fixing the orientation state.

[0064] Next, through the coating device 11 (refer to...) Figure 1An adhesive is applied to the surface of the alignment liquid crystal layer 21 to form a coating layer 12. Figure 3 B).

[0065] Next, between the first bonding roller 15 and the second bonding roller 16 (refer to...) Figure 1 A laminate 17 is formed by stacking an alignment liquid crystal film 10 with a coating layer 12 and an optical film 13 having a support substrate 23 and an optical layer 22, thereby forming a laminate 17. Figure 3 C). At this point, a laminate 17 is formed with the optical layer 22 in contact with the coating layer 12.

[0066] Next, the device 18 (reference) is used for irradiation with active energy rays. Figure 1 The laminate 17 is irradiated with active energy rays, causing the adhesive in the coating layer 12 to cure, forming the adhesive layer 19. Then, the support substrate 23 is peeled off from the optical layer 22. Through the above processes, a product can be obtained. Figure 3 The alignment liquid crystal film 101 shown in D. Furthermore, the support substrate 23 can be used directly as an alignment liquid crystal film while it is attached to the optical layer 22 without peeling it off.

[0067] In order to manufacture alignment liquid crystal films with better heat resistance, Figure 3 The retardation of the alignment liquid crystal layer 21 of A Figure 3 The absolute value of the retardation difference of the alignment liquid crystal layer 21 of D is preferably 3.2 nm or less. There is no particular limitation on the lower limit of the absolute value of the above difference, which can be 0 nm, but from the viewpoint of reducing manufacturing costs, the absolute value of the above difference is preferably 1.5 nm or more. The absolute value of the above difference can be adjusted, for example, by changing at least one of the following: the temperature of the adhesive to be coated in the coating process, the tension applied to the laminate 17 in the irradiation process, and the cumulative amount of active energy rays irradiating the laminate 17 in the irradiation process.

[0068] The aligned liquid crystal film 101 can be used directly as an optical component. In this case, the support substrate 20 constitutes part of the aligned liquid crystal film 101. Alternatively, it can be used like... Figure 4 As shown in the alignment liquid crystal film 102, the support substrate 20 is peeled off from the alignment liquid crystal layer 21. This can be done as follows: Figure 5 As shown in the diagram 103, a suitable adhesive layer 30 can be laminated on the surface of the alignment liquid crystal layer 21 exposed by peeling off the support substrate 20. Figure 6 The optical layer 41 is stacked in the manner shown by the oriented liquid crystal film 104 through an adhesive layer 40.

[0069] There are no particular limitations on the adhesive constituting the adhesive layer 30; adhesives based on polymers such as acrylic polymers, silicone polymers, polyesters, polyurethanes, polyamides, polyethers, fluoropolymers, and rubber polymers can be appropriately selected. Acrylic adhesives and rubber adhesives, which exhibit excellent transparency, moderate wetting properties, cohesiveness and adhesion, weather resistance, and heat resistance, are particularly preferred. The thickness of the adhesive layer 30 can be appropriately set according to the type of substrate being adhered to, for example, from 5 μm to 500 μm.

[0070] The adhesive layer 30 is laminated onto the alignment liquid crystal layer 21, for example, by attaching a pre-formed sheet adhesive to the surface of the alignment liquid crystal layer 21. Alternatively, after applying the adhesive composition to the alignment liquid crystal layer 21, solvent drying, crosslinking, photocuring, etc., can be performed to form the adhesive layer 30. To improve the adhesion (anchoring force) between the alignment liquid crystal layer 21 and the adhesive layer 30, the adhesive layer 30 can be laminated after forming a surface treatment or easy-to-adhere layer such as corona treatment or plasma treatment on the surface of the alignment liquid crystal layer 21.

[0071] like Figure 5 As shown, a release liner 31 is preferably temporarily attached to the surface of the adhesive layer 30. The release liner 31 is used, for example, to bond the adhesive-coated alignment liquid crystal film 103 to the image display unit 50 described later (see reference 100). Figure 7 The adhesive layer 30 is protected during the bonding process. As a component of the release liner 31, a plastic film formed of acrylic, polyolefin, cyclic polyolefin, polyester, etc., can be suitably used. The thickness of the release liner 31 is, for example, 5 μm to 200 μm. It is preferable to perform a release treatment on the surface of the release liner 31. Examples of release agents used for the release treatment include silicone-based materials, fluorine-based materials, long-chain alkyl-based materials, and fatty acid amide-based materials.

[0072] In manufacturing Figure 6 When aligning the liquid crystal film 104 as shown, the alignment liquid crystal layer 21 can be bonded to the optical layer 22 with an adhesive, and then the alignment liquid crystal layer 21 can be bonded to the optical layer 41 with an adhesive. Alternatively, the alignment liquid crystal layer 21 can be bonded to the optical layer 41 with an adhesive, and then the alignment liquid crystal layer 21 can be bonded to the optical layer 22 with an adhesive. Furthermore, the alignment liquid crystal layer 21 can be bonded to the optical layer 22, and the alignment liquid crystal layer 21 can be bonded to the optical layer 41 simultaneously with an adhesive. An adhesive layer (not shown) can be further laminated on the optical layer 22 or the optical layer 41, and a release liner (not shown) can be temporarily adhered to the surface of the adhesive layer.

[0073] Next, the materials used in the manufacturing method of the alignment liquid crystal film of this embodiment will be described.

[0074] [Liquid Crystalline Composition]

[0075] Examples of liquid crystal compounds included in liquid crystal compositions include rod-shaped and disc-shaped liquid crystal compounds. Rod-shaped liquid crystal compounds are preferred because they are easily and uniformly oriented by the orientation restraint force of the supporting substrate 20. The rod-shaped liquid crystal compound can be a polymer. For example, it can be a liquid crystal polymer (more specifically, a main-chain liquid crystal polymer, a side-chain liquid crystal polymer, etc.) or a polymer of a polymerizable liquid crystal compound. If the liquid crystal compound (monomer) exhibits liquid crystal properties before polymerization, it may not exhibit liquid crystal properties after polymerization.

[0076] The liquid crystal compound is preferably a thermotropic liquid crystal that exhibits liquid crystal properties upon heating. Thermotropic liquid crystals undergo phase transitions between a crystalline phase, a liquid crystal phase, and an isotropic phase with temperature changes. The liquid crystal compound contained in the liquid crystal composition can be any of a nematic liquid crystal, a smectic liquid crystal, or a cholesterol-type liquid crystal. A chiral agent can also be added to a nematic liquid crystal to impart cholesterol-type orientation.

[0077] Examples of thermotropic rod-shaped liquid crystal compounds include: methylimine compounds, oxoazo compounds, cyanobiphenyl compounds, cyanophenyl ester compounds, benzoate compounds, cyclohexanecarboxylic acid phenyl ester compounds, cyanophenylcyclohexane compounds, cyano-substituted phenylpyrimidine compounds, alkoxy-substituted phenylpyrimidine compounds, phenyldioxane compounds, diphenylacetylene compounds, and alkenylcyclohexylbenzonitrile compounds.

[0078] Examples of polymerizable liquid crystal compounds include: polymerizable liquid crystal compounds in which the orientation state of rod-shaped liquid crystal compounds can be fixed using a polymer binder; and polymerizable liquid crystal compounds having polymerizable functional groups that can fix the orientation state of liquid crystal compounds through polymerization. Among these, photopolymerizable liquid crystal compounds having photopolymerizable functional groups are preferred.

[0079] The photopolymerizable liquid crystal compound (liquid crystal monomer) has a mesocrystalline group and at least one photopolymerizable functional group in one molecule. The temperature at which the liquid crystal monomer exhibits liquid crystal properties (liquid crystal phase transition temperature) is preferably 40°C to 200°C, more preferably 50°C to 150°C, and even more preferably 55°C to 100°C.

[0080] Examples of mesocrystalline groups that can serve as monomers for liquid crystals include: biphenyl, phenylbenzoate, phenylcyclohexyl, oxazophenyl, azophenyl, phenylpyrimidinyl, diphenylethynyl, diphenylbenzoate, bicyclohexyl, cyclohexylphenyl, and triphenyl, among other cyclic structures. The ends of these cyclic units can be substituted with cyano, alkyl, alkoxy, or halogen groups.

[0081] Examples of photopolymerizable functional groups include (meth)acryloyl, epoxy, and vinyl ether groups. Among these, (meth)acryloyl is preferred. The liquid crystal monomer preferably has two or more photopolymerizable functional groups in one molecule. By using a liquid crystal monomer containing two or more photopolymerizable functional groups, a cross-linking structure is introduced into the photocured liquid crystal layer, thus leading to an improvement in the durability of the oriented liquid crystal film.

[0082] As the liquid crystal monomer, any suitable liquid crystal monomer can be used. For example, International Patent Publication No. 00 / 37585, US Patent No. 5211877, US Patent No. 4388453, International Patent Publication No. 93 / 22397, European Patent No. 0261712, German Patent No. 19504224, German Patent No. 4408171, British Patent No. 2280445, Japanese Patent Application Publication No. 2017-206460, International Patent Publication No. 2014 / 126113, International Patent Publication No. 2016 / 114348, International Patent Publication No. 2014 / 010325, and Japanese Patent Application Publication No. 2015-200 Compounds described in Japanese Publication No. 877, Japanese Patent Application Publication No. 2010-31223, International Publication No. 2011 / 050896, Japanese Patent Application Publication No. 2011-207765, Japanese Patent Application Publication No. 2010-31223, Japanese Patent Application Publication No. 2010-270108, International Publication No. 2008 / 119427, Japanese Patent Application Publication No. 2008-107767, Japanese Patent Application Publication No. 2008-273925, International Publication No. 2016 / 125839, and Japanese Patent Application Publication No. 2008-273925 are used as liquid crystal monomers. By selecting the liquid crystal monomer, the birefringence performance and the delayed wavelength dispersion can also be adjusted.

[0083] In addition to liquid crystal monomers, liquid crystal compositions may also contain compounds (orientation control agents) that control the orientation of liquid crystal monomers in a predetermined direction. For example, by including a side-chain type liquid crystal polymer in the liquid crystal composition, the liquid crystal compound (monomer) can be vertically oriented. Furthermore, by adding a chiral agent to the liquid crystal composition, the liquid crystal compound can be oriented in a cholesterol-type manner.

[0084] The liquid crystal composition may contain a photopolymerization initiator. In cases where liquid crystal monomers are cured by ultraviolet irradiation, to promote photocuring, the liquid crystal composition preferably contains a photoradical polymerization initiator (photoradical generator) that generates free radicals upon light irradiation. Depending on the type of liquid crystal monomer (the type of photopolymerizable functional group), a photocation generator or a photoanion generator may be used. The amount of photopolymerization initiator used is, for example, 0.01 parts by weight to 10 parts by weight relative to 100 parts by weight of the liquid crystal monomer. In addition to photopolymerization initiators, sensitizers, etc., may also be used.

[0085] Liquid crystal compositions can be prepared by mixing liquid crystal monomers and various orientation control agents, polymerization initiators, etc., as needed, with solvents. As a solvent, there are no particular limitations as long as it can dissolve the liquid crystal monomers and does not corrode the supporting substrate 20 (or has low corrosivity). Examples include: halogenated hydrocarbon compounds such as chloroform, dichloromethane, carbon tetrachloride, dichloroethane, tetrachloroethane, trichloroethylene, tetrachloroethylene, chlorobenzene, and o-dichlorobenzene; phenolic compounds such as phenol and p-chlorophenol; aromatic hydrocarbon compounds such as benzene, toluene, xylene, methoxybenzene, and 1,2-dimethoxybenzene; acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and cyclopentanone. Ketone solvents such as 2-pyrrolidone and N-methyl-2-pyrrolidone; ester solvents such as ethyl acetate and butyl acetate; alcohol solvents such as tert-butanol, glycerol, ethylene glycol, triethylene glycol, ethylene glycol monomethyl ether, diethylene glycol dimethyl ether, propylene glycol, dipropylene glycol, and 2-methyl-2,4-pentanediol; amide solvents such as dimethylformamide and dimethylacetamide; nitrile solvents such as acetonitrile and propionitrile; ether solvents such as diethyl ether, dibutyl ether, and tetrahydrofuran; and cellosolver solvents such as ethyl cellosolver and butyl cellosolver. Mixed solvents of two or more solvents can also be used.

[0086] The concentration of solid components in the liquid crystal composition is, for example, 5% to 60% by weight. The liquid crystal composition may contain additives such as surfactants and leveling agents.

[0087] [Supporting Substrate]

[0088] As for the support substrates 20 and 23, there are no particular limitations as long as they can be transported in a roll-to-roll manner. From the viewpoint of ease of transport, film substrates (more specifically, resin film substrates, etc.) are preferred. Support substrates 20 and 23 can be made of the same material or of different types of materials. The thickness of support substrate 20 and 23 is not particularly limited, and for example, is 1 μm to 500 μm. The thickness of support substrate 20 and 23 can be the same or different. Support substrate 20 has a first main surface and a second main surface, and a liquid crystal composition is coated on the first main surface.

[0089] As a resin material constituting the resin film substrate, there are no particular limitations as long as it is not soluble in the solvent of the liquid crystal composition and has heat resistance when heated to orient the liquid crystal composition. Examples include: polyesters such as polyethylene terephthalate and polyethylene naphthalate; polyolefins such as polyethylene and polypropylene; cyclic polyolefins such as norbornene polymers; cellulose polymers such as cellulose diacetate and cellulose triacetate; acrylic polymers; styrene polymers; polycarbonate; polyamide; polyimide, etc.

[0090] The support substrate 20 can have the orientation capability to orient the liquid crystal compound along a predetermined direction. For example, by using a stretched film as the support substrate 20, the liquid crystal compound can be uniformly oriented along its stretching direction. The stretching ratio of the stretched film is only required to achieve the orientation capability, for example, 1.1 to 5 times. The stretched film can be a biaxial stretched film. Even with a biaxial stretched film, if a film with different stretching ratios in the longitudinal and transverse directions is used, the liquid crystal compound can be oriented along the direction with the larger stretching ratio. The stretched film can also be an inclined stretched film. By using an inclined stretched film as the support substrate 20, the liquid crystal compound can be oriented along a direction that is not parallel to any direction in the length or width direction of the support substrate 20.

[0091] The support substrate 20 may have an alignment film on its first main surface. The alignment film can be selected appropriately based on the type of liquid crystal compound and the material of the support substrate 20. As an alignment film used to uniformly align the liquid crystal compound along a predetermined direction, an alignment film obtained by rubbing a polyimide-based or polyvinyl alcohol-based alignment film can be appropriately used. Alternatively, a photo-alignment film can be used. Alternatively, an alignment film may not be provided, and the resin film serving as the support substrate 20 may be rubbed.

[0092] The support substrate 20 may have an alignment film for vertically aligning the liquid crystal compound. Examples of alignment agents for forming the vertically oriented alignment film include: lecithin, stearic acid, hexadecyltrimethylammonium bromide, octadecylamine hydrochloride, chromium monocarboxylic acid complexes, organosilanes (more specifically, silane coupling agents, siloxane compounds, etc.), perfluorodimethylcyclohexane, tetrafluoroethylene, polytetrafluoroethylene, etc.

[0093] [Orientation liquid crystal layer]

[0094] When the liquid crystal compound is a thermotropic liquid crystal, a liquid crystal composition is coated on the first main surface of the support substrate 20, and the liquid crystal compound is oriented in a liquid crystal state by heating.

[0095] The method for coating the liquid crystal composition onto the support substrate 20 is not particularly limited, and methods such as spin coating, die coating, kiss roll coating, gravure coating, reverse coating, spray coating, Mayer rod coating, knife roller coating, and air knife coating can be used. After coating the liquid crystal composition, the solvent is removed, thus forming a liquid crystal composition layer on the support substrate 20. The thickness of the coating layer formed by coating the liquid crystal composition is preferably adjusted so that the thickness of the liquid crystal composition layer after solvent removal is 0.1 μm to 20 μm.

[0096] A liquid crystal phase is formed by heating a liquid crystal composition layer formed on a support substrate 20, and the liquid crystal compound is oriented to form an oriented liquid crystal layer 21. Specifically, the liquid crystal composition is coated onto the support substrate 20, and then heated to above the N (nematic)-I (isotropic liquid phase) transition temperature of the liquid crystal composition, so that the liquid crystal composition becomes an isotropic liquid state. Then, it is slowly cooled as needed to make it exhibit a nematic phase. At this time, it is desirable to temporarily maintain the temperature of exhibiting a liquid crystal phase to allow the liquid crystal phase domains to grow into single domains. Alternatively, the liquid crystal composition can be coated onto the support substrate 20, and then the temperature can be maintained within the temperature range of exhibiting a nematic phase for a certain period of time to oriented the liquid crystal compound in a predetermined direction.

[0097] The heating temperature for aligning the liquid crystal compound in a specified direction can be appropriately selected according to the type of liquid crystal composition, for example, 40°C to 200°C. If the heating temperature is too low, the transition to the liquid crystal phase tends to be insufficient; if the heating temperature is too high, orientation defects may increase. The heating time can be adjusted to ensure sufficient growth of the liquid crystal phase domains, for example, 30 seconds to 30 minutes.

[0098] Preferably, the liquid crystal compound is oriented by heating and then cooled to a temperature below the glass transition temperature. The cooling method is not particularly limited; for example, simply removing it from the heated atmosphere to room temperature is sufficient. Forced cooling, such as air cooling or water cooling, can also be used.

[0099] Photocuring is achieved by irradiating the oriented photopolymerizable liquid crystal compound with light, allowing the compound (liquid crystal monomer) to maintain its liquid crystal regularity. The irradiation light only needs to be sufficient to polymerize the photopolymerizable liquid crystal compound; ultraviolet or visible light with wavelengths of 250 nm to 450 nm is typically used. If the liquid crystal composition contains a photopolymerization initiator, light of a wavelength to which the initiator has sensitivity can be selected. As the irradiation source, low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, LEDs, black lights, chemical lamps, etc., can be used. To promote the photocuring reaction, irradiation is preferably carried out in an atmosphere of inert gas such as nitrogen.

[0100] During the photocuring of the liquid crystal composition, the liquid crystal compound can be oriented along a predetermined direction by using polarized light in a predetermined direction. As described above, when the liquid crystal compound is oriented by the orientation-restricting force of the supporting substrate 20, the irradiation light can also be unpolarized light (natural light).

[0101] The intensity of the irradiation light can be adjusted appropriately based on the composition of the liquid crystal composition and the amount of photopolymerization initiator added. For example, the irradiation energy (cumulative light intensity) is 20 mJ / cm². 2 ~10000mJ / cm2 The preferred value is 50 mJ / cm. 2 ~5000mJ / cm 2 More preferably 100 mJ / cm 2 ~800mJ / cm 2 To promote the photocuring reaction, light irradiation can be applied under heating conditions.

[0102] The polymer cured by photocuring liquid crystal monomers by light irradiation is non-liquid crystal and does not undergo phase transitions caused by temperature changes. Therefore, liquid crystal layers cured by photocuring with liquid crystal monomers aligned in a specified direction are generally less prone to changes in molecular orientation. Furthermore, compared to films formed from non-liquid crystal materials, oriented liquid crystal films have a much larger birefringence Δn, thus significantly reducing the thickness of optical anisotropic elements with the desired retardation. The thickness of the oriented liquid crystal layer 21 can be set accordingly to the target retardation value, for example, 0.1 μm to 20 μm, preferably 0.2 μm to 10 μm, and more preferably 0.5 μm to 7 μm.

[0103] The optical properties of the alignment liquid crystal layer 21 are not particularly limited. The in-plane retardation and thickness direction retardation of the alignment liquid crystal layer 21 can be appropriately set according to the application. In the case of uniform alignment of the liquid crystal compound, the in-plane retardation of the alignment liquid crystal layer 21 is, for example, 20 nm to 1000 nm. In the case of a quarter-wave plate, the in-plane retardation is preferably 100 nm to 180 nm, more preferably 120 nm to 150 nm. In the case of a half-wave plate, the in-plane retardation is preferably 200 nm to 340 nm, more preferably 240 nm to 300 nm. In the case of vertical alignment of the liquid crystal compound, the in-plane retardation of the alignment liquid crystal layer 21 is approximately 0 (for example, 5 nm or less, preferably 3 nm or less), and the absolute value of the thickness direction retardation is, for example, 30 nm to 500 nm.

[0104] When the liquid crystal compound in the alignment liquid crystal layer 21 is uniformly aligned, in order to reduce the thickness of the optical anisotropic element, it is preferable that the birefringence Δn of the alignment liquid crystal layer 21 after the bonding process is 0.03 or more. Furthermore, when the liquid crystal compound in the alignment liquid crystal layer 21 is uniformly aligned, in order to easily adjust the in-plane retardation of the alignment liquid crystal layer 21, it is preferable that the birefringence Δn of the alignment liquid crystal layer 21 after the bonding process is 0.5 or less. The birefringence Δn of the alignment liquid crystal layer 21 can be adjusted, for example, by changing the type of liquid crystal compound used to form the alignment liquid crystal layer 21.

[0105] [Optical layer]

[0106] Optical layer 22 and optical layer 41 are not particularly limited. For example, commonly used optical isotropic or optical anisotropic films can be used without limitation as optical layer 22 and optical layer 41. Specific examples of optical layer 22 and optical layer 41 include: transparent films (more specifically, retardation films, polarizer protective films, etc.), functional films (more specifically, polarizers, viewing angle widening films, viewing angle limiting (anti-spy) films, brightness enhancing films, etc.). Optical layer 22 and optical layer 41 can be single layers or laminates. Optical layer 22 and optical layer 41 can be oriented liquid crystal layers (other oriented liquid crystal layers). Furthermore, optical layer 22 can be a polarizer with a transparent protective film bonded to one or both sides of the polarizer. When the polarizer has a transparent protective film on one side, the polarizer can be bonded to the oriented liquid crystal layer 21, or the transparent protective film can be bonded to the oriented liquid crystal layer 21. Optical layer 22 and optical layer 41 can be made of the same material or of different types of materials. The thicknesses of optical layer 22 and optical layer 41 can be adjusted appropriately according to the required optical performance, for example, from 0.1 μm to 1000 μm, preferably from 0.1 μm to 100 μm. The thicknesses of optical layer 22 and optical layer 41 can be the same or different.

[0107] [Adhesive layer]

[0108] The adhesive constituting adhesive layer 19 and adhesive layer 40 is not particularly limited as long as it is an active energy ray curable type and optically transparent; examples include epoxy resin adhesives, silicone resin adhesives, acrylic resin adhesives, polyurethane adhesives, polyamide adhesives, and polyether adhesives. Adhesive layer 19 and adhesive layer 40 can be composed of the same type of adhesive or different types of adhesives. The preferred range for the thickness of adhesive layer 40 is the same as the preferred range for the thickness of adhesive layer 19 described above. The thicknesses of adhesive layer 19 and adhesive layer 40 can be the same or different.

[0109] Active energy radiation-cured adhesives are adhesives that can undergo free radical polymerization, cationic polymerization, or anionic polymerization by irradiation with active energy rays such as electron beams or ultraviolet rays. Among them, photoradioactive adhesives, photocationic adhesives, or hybrid adhesives that combine photocationic and photoradioactive polymerization are preferred because they can cure at low energy levels.

[0110] Monomers for photoradical polymerizable adhesives include compounds having a (meth)acryloyl group and compounds having a vinyl group. Compounds having a (meth)acryloyl group are preferred. Examples of compounds having a (meth)acryloyl group include (meth)acrylic acid C. 1-20Alkyl esters, cyclic alkyl esters of (meth)acrylate, polycyclic alkyl esters of (meth)acrylate, and other alkyl esters of (meth)acrylate; hydroxyl-containing (meth)acrylates; glycidyl esters of (meth)acrylate and other epoxy-containing (meth)acrylates, etc. Photoradical polymerizable adhesives may contain nitrogen-containing monomers such as hydroxyethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, (meth)acrylamide, and (meth)acryloylmorpholine. Photoradical polymerizable adhesives may contain multifunctional monomers such as tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecanediethanol diacrylate, cyclic trimethylolpropane formal acrylate, dioxane glycol diacrylate, and polyoxyethylene glycol diacrylate as crosslinking components.

[0111] Compounds having epoxy groups or oxobutyl groups can be listed as curing components in photocationic polymerizable adhesives. There are no particular limitations on the epoxy group composition, as long as it has at least two epoxy groups within the molecule; various generally known curable epoxy compounds can be used. Preferred epoxy compounds include compounds having at least two epoxy groups and at least one aromatic ring within the molecule (aromatic epoxy compounds), and compounds having at least two epoxy groups within the molecule, with at least one of them formed between two adjacent carbon atoms constituting an alicyclic ring (alicyclic epoxy compounds). Hybrid adhesives can also be prepared by containing free radical polymerizable compounds such as compounds having (meth)acryloyl groups in the cationic polymerizable adhesive.

[0112] To obtain an adhesive with low curing shrinkage, it is preferable to adjust the adhesive formulation in a way that reduces the number of bonds formed during curing. To reduce the number of bonds, monomers with high molecular weight per reactive functional group (e.g., (meth)acryloyl group) are preferred. Examples of monomers with high molecular weight per reactive functional group include alkyl (meth)acrylates (e.g., isostearyl acrylate) having 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more carbon atoms, and polyoxyethylene glycol diacrylates having 5 or more, 7 or more, or 9 or more oxyethylene groups per molecule.

[0113] Furthermore, when the adhesive before curing contains oligomers with a weight-average molecular weight of 1000 or more, an adhesive with low curing shrinkage can also be obtained. Examples of oligomers with a weight-average molecular weight of 1000 or more (hereinafter sometimes referred to as "specific oligomers") include oligomers formed from monomers having (meth)acryloyl groups (acrylic oligomers). Acrylic oligomers may have cationic polymerizable functional groups (e.g., epoxy groups).

[0114] The weight-average molecular weight of a specific oligomer can be determined by gel permeation chromatography (GPC). In this specification, unless otherwise specified, the weight-average molecular weight of a specific oligomer is a standard polystyrene equivalent measured under the following conditions.

[0115] (Conditions for molecular weight determination)

[0116] GPC measuring device: Tosoh Corporation "HLC-8120GPC"

[0117] Sample concentration: 2.0 g / L (tetrahydrofuran solution)

[0118] Sample injection volume: 20 μL

[0119] Column: Tosoh Corporation "TSKgel, SuperAWM-H+superAW4000"

[0120] +superAW2500”

[0121] Column dimensions: 6.0mm I.D. × 150mm each

[0122] Eluent: Tetrahydrofuran

[0123] Flow rate: 0.4 mL / min

[0124] Detector: Differential refractometer (RI)

[0125] Column temperature (measurement temperature): 40℃

[0126] Photocurable adhesives preferably contain a photopolymerization initiator. The photopolymerization initiator can be selected appropriately based on the type of reaction. For example, it is preferable to use a photoradical polymerization initiator that generates free radicals through light irradiation in a photoradical polymerization adhesive. It is preferable to use a photocationic polymerization initiator (photoacid generator) that generates cationic species or Lewis acids through light irradiation in a photocationic polymerization adhesive. It is preferable to combine a photocationic polymerization initiator and a photoradical polymerization initiator in a mixed adhesive.

[0127] The content of the photopolymerization initiator relative to 100 parts by weight of the monomer is, for example, 0.1 parts by weight to 10 parts by weight, preferably 0.5 parts by weight to 3 parts by weight. If necessary, a photosensitizer may also be incorporated into the photocurable adhesive. The amount of the photosensitizer relative to 100 parts by weight of the monomer is, for example, 0.001 parts by weight to 10 parts by weight, preferably 0.01 parts by weight to 3 parts by weight.

[0128] Adhesives may contain appropriate additives as needed. Examples of additives include: silane coupling agents, titanium coupling agents, and other coupling agents; ethylene oxide and other adhesion promoters; ultraviolet absorbers; deterioration inhibitors; dyes; processing aids; ion scavengers; antioxidants; tackifiers; fillers; plasticizers; leveling agents; foaming inhibitors; antistatic agents; heat stabilizers; and hydrolysis stabilizers.

[0129] [use]

[0130] The oriented liquid crystal film obtained by the manufacturing method of this embodiment can, for example, be used as an optical film for displays for purposes such as improving visual recognizability.

[0131] The alignment liquid crystal film obtained by the manufacturing method of this embodiment can be a circular polarizer to which a polarizer serving as an optical layer 22 is bonded to one side of the alignment liquid crystal layer 21 via an adhesive layer 19. The circular polarizer may have two or more alignment liquid crystal layers.

[0132] Polarizing films can consist of only one polarizer layer, or, as described above, a transparent protective film can be laminated to one or both sides of the polarizer. Examples of polarizers include: polarizers made by uniaxially stretching hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films after adsorbing dichroic substances such as iodine and dichroic dyes; and polyene-based oriented films such as dehydrated polyvinyl alcohol products and dehydrochlorinated polyvinyl chloride products.

[0133] From the perspective of achieving a high degree of polarization, a polyvinyl alcohol (PVA)-based polarizer is preferred, which adsorbs iodine and dichroic substances such as dichroic dyes onto a polyvinyl alcohol film, such as polyvinyl alcohol or partially formalized polyvinyl alcohol, and orients it in a specified direction. For example, a PVA-based polarizer can be obtained by iodizing and stretching a polyvinyl alcohol film. Alternatively, a PVA-based resin layer can be formed on a resin substrate, and iodine-dyeing and stretching can be performed in a laminated state.

[0134] In a circular polarizer, at least one oriented liquid crystal layer preferably has a uniformly oriented liquid crystal compound. In the circular polarizer, the orientation direction of the liquid crystal compound in the oriented liquid crystal layer with uniformly oriented liquid crystal compound is neither parallel nor orthogonal to the absorption axis direction of the polarizer.

[0135] When a circular polarizer has only one oriented liquid crystal layer, for example, the oriented liquid crystal layer 21 is a quarter-wave plate, the angle between the absorption axis direction of the polarizer (which serves as the optical layer 22) and the orientation direction of the liquid crystal compound (generally the slow axis direction) is set to 45°. The angle between the absorption axis direction of the polarizer and the orientation direction of the liquid crystal compound can be 35° to 55°, 40° to 50°, or 43° to 47°.

[0136] In a configuration where a polarizer serving as optical layer 22 and a quarter-wave plate serving as alignment liquid crystal layer 21 are stacked at an angle of 45° between their optical axes, an alignment liquid crystal layer with vertically aligned liquid crystal compound is further provided as optical layer 41 (see reference). Figure 6 By sequentially stacking an oriented liquid crystal layer 21, which serves as a quarter-wave plate, and an optical layer 41, which functions as a positive C-plate, on a polarizer, a circular polarizer capable of blocking reflected light from external light coming from an inclined direction can be formed. A vertically oriented liquid crystal layer (positive C-plate) and a uniformly oriented liquid crystal layer (a quarter-wave plate serving as a positive A-plate) can be sequentially stacked on the polarizer.

[0137] exist Figure 6 The oriented liquid crystal film 104 shown is a circular polarizer in which an oriented liquid crystal layer 21 and an oriented liquid crystal layer 41 are sequentially stacked on a polarizer serving as an optical layer 22. Both the oriented liquid crystal layer 21 and the optical layer 41 can be uniformly oriented liquid crystal layers. In this case, it is preferable that the oriented liquid crystal layer 21 disposed near the optical layer 22 is a half-wave plate, and the optical layer 41 disposed away from the optical layer 22 is a quarter-wave plate. In this layer configuration, it is preferable that the angle between the slow axis direction of the half-wave plate and the absorption axis direction of the polarizer is 75°±5°, and the angle between the slow axis direction of the quarter-wave plate and the absorption axis direction of the polarizer is 15°±5°. Circular polarizers with such layer configurations function as circular polarizers over a wide wavelength range of visible light, thus reducing the coloration of reflected light.

[0138] <Image display device>

[0139] Figure 7 This is a cross-sectional view showing an example of the layer configuration of an image display device. An alignment liquid crystal film (obtained by the manufacturing method of this embodiment) having an alignment liquid crystal layer 21 is bonded to the surface of the image display unit 50 via an adhesive layer 30. The alignment liquid crystal film may have two or more alignment liquid crystal layers. Examples of image display units 50 include liquid crystal cells and organic EL cells.

[0140] As described above, the heat durability of the alignment liquid crystal layer 21 of the alignment liquid crystal film obtained by the manufacturing method of this embodiment is improved. Therefore, Figure 7 Even when exposed to high temperatures for extended periods, the image display device 200 exhibits minimal change in the delay of the oriented liquid crystal layer 21, resulting in minimal change in visual recognizability and excellent heat resistance.

[0141] Example

[0142] The present invention will be described in more detail below with examples of the fabrication of alignment liquid crystal films, but the present invention is not limited to the examples described below.

[0143] <Preparation of Adhesive A-1>

[0144] UV-curable adhesive A-1 was prepared by combining the components shown in Table 1 with the proportions shown in Table 1. Furthermore, in Table 1, all proportions are relative to the total amount of adhesive.

[0145] In addition, the meanings of the terms in Table 1 are as follows.

[0146] HEAA: Hydroxyethyl Acrylamide (manufactured by KJ Chemical Company, "HEAA (registered trademark)")

[0147] M-5700: Acrylate monomer (manufactured by Dong-A Synthetic Co., Ltd., "Aronix (registered trademark) M-5700")

[0148] P2H-A: Phenoxy diethylene glycol acrylate (manufactured by Kyoei Chemical Co., Ltd., "Light acrylate (registered trademark) P2H-A")

[0149] M-220: Acrylate monomer (manufactured by Dong-A Synthetic Co., Ltd., "Aronix (registered trademark) M-220")

[0150] 1,9ND-A: 1,9-Nonanediol diacrylate (Kyoei Chemical Co., Ltd., "Light acrylate (registered trademark) 1,9ND-A")

[0151] UP-1190: Acrylic oligomer (manufactured by Dong-A Synthetic Co., Ltd., "ARUFON (registered trademark) UP-1190", weight average molecular weight: 1700)

[0152] Omnirad 907: Photoradical polymerization initiator (manufactured by IGM Resins, "Omnirad 907" (registered trademark)).

[0153] DETX-S: Photoradical polymerization initiator (manufactured by Nippon Kayaku Co., Ltd., "KAYACURE (registered trademark) DETX-S")

[0154] Table 1

[0155]

[0156] <Fabrication of Layer L-1>

[0157] A photopolymerizable liquid crystal compound exhibiting a nematic liquid crystal phase (BASF's "Paliocolor LC242") was dissolved in cyclopentanone to prepare a solution with a solid content concentration of 30% by weight. A surfactant (Big Chemie Japan's "BYK-360") and a photopolymerization initiator (IGM Resins' "Omnirad 907") were added to this solution to prepare a liquid crystal composition. The amounts of surfactant and photopolymerization initiator added were set to 0.01 parts by weight and 3 parts by weight, respectively, relative to 100 parts by weight of the photopolymerizable liquid crystal compound.

[0158] As the film substrate, a transversely stretched film (ZeonoR Film (registered trademark) ZT12-50135 manufactured by Zeon Corporation, Japan, thickness: 52 μm, in-plane retardation: 50 nm) was used. The aforementioned liquid crystal composition was coated onto the surface of the film substrate using a rod coater to a thickness of 1.4 μm after heating. The substrate was then heated at 100°C for 3 minutes to orient the liquid crystal compound. Next, the liquid crystal composition on the film substrate was cooled to room temperature (25°C), and then irradiated with a cumulative light intensity of 400 mJ / cm² in a nitrogen atmosphere. 2 UV light was used for photocuring to obtain a laminate L-1 with a uniformly oriented liquid crystal layer formed on the film substrate.

[0159] The in-plane retardation of the aligned liquid crystal layer in the obtained laminate L-1 was measured. Specifically, firstly, a 15 μm thick acrylic adhesive sheet was bonded to the surface of the aligned liquid crystal layer in laminate L-1, and then the adhesive sheet was bonded to a glass plate, resulting in a laminate with a glass plate. Next, the film substrate was peeled off from the laminate with the glass plate to obtain a test sample. Next, the in-plane retardation of the test sample (aligned liquid crystal layer) at a wavelength of 590 nm was measured using a phase difference meter (KOBRA 21-ADH, manufactured by Oji Measurement Equipment Co., Ltd.). Hereinafter, the in-plane retardation measured here is recorded as Re1. Re1 is 140 nm.

[0160] <Fabrication of Alignment Liquid Crystal Film>

[0161] [Fabrication of the Alignment Liquid Crystal Film in Example 1]

[0162] A film ("MCP-N(100)", hereinafter referred to as "Laminator L-2") with a vertically aligned liquid crystal layer (thickness: 3 μm, in-plane retardation: 0 nm) as an optical layer on a substrate was prepared. In addition, laminate L-1 was fabricated by the above method.

[0163] The aforementioned adhesive A-1 was coated on the surface of the alignment liquid crystal layer of the laminate L-1 with a thickness of 1.0 μm (temperature: 25°C). Next, the alignment liquid crystal layer side of the laminate L-2 was bonded to the coating layer formed by adhesive A-1 to obtain the laminate L-3.

[0164] Next, following a roll-to-roll bonding process, adhesive A-1 in laminate L-3 is photocured while under tension. Specifically, in an atmosphere at 25°C, laminate L-3 is subjected to a tension of 538 N / 1000 mm in an in-plane direction orthogonal to the orientation direction of the uniformly aligned liquid crystal layer in laminate L-1, with an illuminance of 600 mW / cm². 2 The high-pressure mercury lamp has a cumulative luminous flux of 600 mJ / cm². 2 The adhesive A-1 was photocured by irradiating it with ultraviolet light. Ultraviolet irradiation was performed from the L-2 side of the laminate. Furthermore, the orientation direction of the uniformly aligned liquid crystal layer in the L-1 is the stretching direction of the film substrate (stretched film) of the L-1. Therefore, in the roll-to-roll bonding process, the direction orthogonal in-plane to the orientation direction of the uniformly aligned liquid crystal layer is the transport direction of the L-3. Next, the substrate of the L-2 was peeled from the L-3 to obtain the aligned liquid crystal film of Example 1.

[0165] [Fabrication of Alignment Liquid Crystal Films in Examples 2-4]

[0166] The cumulative light intensity during photocuring of the adhesive was changed as shown in Table 2 below. Otherwise, alignment liquid crystal films of Examples 2 to 4 were prepared by the same method as in Example 1.

[0167] [Preparation of alignment liquid crystal films in Examples 5-7 and Comparative Example 1]

[0168] The temperature of the adhesive during coating was changed as shown in Table 3 below. Otherwise, alignment liquid crystal films of Examples 5-7 and Comparative Example 1 were prepared using the same method as in Example 1. Furthermore, for reference, details of Example 1 described above are also recorded in Table 3.

[0169] [Fabrication of alignment liquid crystal films in Examples 8, 9 and Comparative Example 2]

[0170] The tension applied to the laminate L-3 was modified as shown in Table 4 below. Otherwise, alignment liquid crystal films of Examples 8, 9, and Comparative Example 2 were prepared using the same method as in Example 1. Furthermore, for reference, details of Example 1 described above are also recorded in Table 4.

[0171] <Evaluation>

[0172] [Changes in adhesion delay before and after bonding]

[0173] An acrylic adhesive sheet with a thickness of 15 μm was bonded to the surface of the vertically aligned liquid crystal layer of the alignment liquid crystal film of the evaluation object (any one of the alignment liquid crystal films of Examples 1-9, Comparative Examples 1 and 2). The adhesive sheet was then bonded to a glass plate to obtain a laminate with a glass plate. Next, the film substrate was peeled off from the laminate with the glass plate to obtain an evaluation sample. The in-plane retardation of the evaluation sample (uniformly aligned liquid crystal layer) at a wavelength of 590 nm was measured using a phase difference meter (KOBRA 21-ADH manufactured by Oji Measurement Equipment Co., Ltd.). Hereinafter, the in-plane retardation measured here is recorded as Re2. Furthermore, the retardation change before and after bonding (unit: nm) was calculated according to the formula "Retardation change before and after bonding = |Re2 - Re1|". In addition, |Re2 - Re1| represents the absolute value of the difference between Re2 and Re1. When the retardation change before and after bonding is 3.2 nm or less, it is evaluated as "capable of suppressing the retardation change before and after bonding". On the other hand, when the delay change before and after bonding exceeds 3.2 nm, it is evaluated as "unable to suppress the delay change before and after bonding".

[0174] Furthermore, for the oriented liquid crystal film of Example 1, the birefringence Δn was calculated using Re2 and the thickness of the uniformly oriented liquid crystal layer according to the formula “birefringence Δn = Re2 / thickness of uniformly oriented liquid crystal layer”, and the result was that the birefringence Δn of the uniformly oriented liquid crystal layer was 0.10.

[0175] [Rate of delayed change before and after heating durability test]

[0176] The evaluation sample used for evaluating the [delay change before and after bonding] was placed in an air-circulating constant-temperature oven at 85°C for 120 hours. Next, the evaluation sample was removed from the oven, and the in-plane delay of the evaluation sample (uniformly aligned liquid crystal layer) at a wavelength of 590 nm was measured using a phase difference meter (KOBRA 21-ADH, manufactured by Oji Measurement Equipment Co., Ltd.). Hereinafter, the in-plane delay measured here is recorded as Re3. Furthermore, the delay change rate (in %) before and after the heat durability test was calculated according to the formula: "Delay change rate before and after heat durability test = 100 × |Re3 - Re2| / Re2". In addition, |Re3 - Re2| represents the absolute value of the difference between Re3 and Re2. When the delay change rate before and after the heat durability test is 3.5% or less, it is evaluated as "able to suppress changes in optical properties even after prolonged exposure to high-temperature environments". On the other hand, if the rate of delayed change before and after the heat durability test exceeds 3.5%, it is evaluated as "unable to suppress changes in optical properties when exposed to high temperature environment for a long time".

[0177] Furthermore, no interlayer delamination occurred in the evaluation samples after the heat durability test, ensuring the reliability of the bond.

[0178] For each of the above embodiments and comparative examples, the delay changes before and after bonding and the delay change rate before and after the heat durability test, along with the manufacturing conditions, are shown in Tables 2 to 4. Furthermore, in Tables 2 to 4, "ΔRe" represents the delay change before and after bonding, and "Re change rate" represents the delay change rate before and after the heat durability test.

[0179] Table 2

[0180]

[0181] Table 3

[0182]

[0183] Table 4

[0184]

[0185] In Examples 1-9, the temperature of the adhesive during coating was 0°C to 45°C, and the tension applied to the laminate L-3 was 70 N / 1000 mm width to 550 N / 1000 mm width. In Examples 1-9, the rate of retardation change before and after the heat durability test was less than 3.5%. Therefore, the alignment liquid crystal films of Examples 1-9 can suppress changes in optical properties even when exposed to high-temperature environments for extended periods.

[0186] In Comparative Example 1, the temperature of the adhesive applied during coating exceeded 45°C. In Comparative Example 2, the tension applied to the laminate L-3 exceeded 550 N / 1000 mm width. In Comparative Examples 1 and 2, the rate of change in retardation before and after the heat durability test exceeded 3.5%. Therefore, the alignment liquid crystal films of Comparative Examples 1 and 2 were unable to suppress changes in optical properties when exposed to high-temperature environments for extended periods.

[0187] The results above demonstrate that the method for manufacturing an oriented liquid crystal film according to the present invention can produce an oriented liquid crystal film whose optical properties change little even when exposed to a high-temperature environment for a long time.

Claims

1. A method for manufacturing an aligned liquid crystal film, comprising a method for manufacturing an aligned liquid crystal film having an aligned liquid crystal layer oriented with a liquid crystal compound. It features a bonding process that uses a roll-to-roll method to bond the oriented liquid crystal layer and the optical layer together with an active energy ray-cured adhesive. The bonding process includes: The adhesive coating process performed at a temperature of 0°C to 10°C before curing on at least one surface of the alignment liquid crystal layer and the optical layer; and An irradiation process in which an irradiation of an active energy ray is performed on a laminate formed by laminating the alignment liquid crystal layer and the optical layer with an adhesive before curing, wherein the laminate is subjected to a tension of 70 N / 1000 mm to 550 N / 1000 mm along the transport direction of the laminate.

2. The method for manufacturing an alignment liquid crystal film according to claim 1, wherein, In the irradiation process, the cumulative light intensity is 450 mJ / cm. 2 ~1200mJ / cm 2 The laminate is irradiated with the active energy rays under the specified conditions.

3. The method for manufacturing the alignment liquid crystal film according to claim 1 or 2, wherein, The thickness of the layer formed by the adhesive after the irradiation process is 0.1 μm to 3.0 μm.

4. The method for manufacturing the alignment liquid crystal film according to claim 1 or 2, wherein, In the oriented liquid crystal layer, the liquid crystal compound is uniformly oriented.

5. The method for manufacturing an alignment liquid crystal film according to claim 4, wherein, The birefringence Δn of the oriented liquid crystal layer after the bonding process is greater than or equal to 0.

03.

6. The method for manufacturing an aligned liquid crystal film according to claim 1 or 2, wherein, The optical layer is a polarizer or an alignment liquid crystal layer different from the alignment liquid crystal layer.

7. The method for manufacturing an aligned liquid crystal film according to claim 1 or 2, wherein, The optical layer is a transparent film.

Citation Information

Patent Citations

  • Liq. crystalline (LC) material

    DE19504224A1

  • Novel polymerizable liquid crystalline compounds

    DE4408171A1

  • Picture display cell, method of forming an orientation layer on a substrate of the picture display cell and monomeric compounds for use in the orientation layer

    EP0261712A1

  • Liquid crystalline copolymer

    GB2280445A

  • Optical film, retardation plate and liquid crystal compound

    JP2008107767A