Separator and lithium battery including the same

By using porous substrates and coatings of high melting point organic particles, boehmite, and ceramic particles on the lithium battery separator, the stability problem of lithium batteries at high temperature is solved, and the high temperature stability and electrolyte impregnation characteristics of lithium batteries are achieved. promote.

CN115133224BActive Publication Date: 2024-11-01SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210306306.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-26
Filing Date
2022-03-25
Publication Date
2024-11-01
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

Lithium batteries have short circuit problems due to the low strength and rapid heat shrinkage of olefin polymers at high temperatures. In the prior art, such as the partitions added with polyethylene wax melting at high temperatures, and cannot maintain stability.

Method used

The first binder has a glass transition temperature of 50°C or higher to form a mesh structure, including organic particles with melting points between 100°C and 130°C. To improve high temperature stability.

Benefits of technology

The rapid increase in temperature and heat value at high temperatures is delayed, the coating structure is maintained, the high temperature stability of lithium batteries and electrolyte impregnation characteristics are improved, and the heat resistance and durability of the partition are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115133224B_ABST
    Figure CN115133224B_ABST
Patent Text Reader

Abstract

The present application provides a separator and a lithium battery including the separator, wherein the separator includes: a porous substrate; a first coating disposed on the surface of the porous substrate, the first coating including a melting point (T m ) in the range of about 100°C to about 130°C, organic particles, granular boehmite, needle-shaped ceramic particles and a first binder; a first binder layer disposed on the other surface of the porous substrate, the first binder layer having a glass transition temperature (Tg) of 50°C or higher and including a granular second binder; and a second binder layer disposed on the first coating layer, the second binder layer having a glass transition temperature (Tg) of 50°C or higher and including a granular second binder.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2021-0039489 filed on March 26, 2021 in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0003] One or more embodiments relate to a separator and a lithium battery including the separator. Background Art

[0004] In order to meet the miniaturization and high performance of various devices, the miniaturization and weight reduction of lithium batteries have become more important. In addition, the discharge capacity, energy density and cycle characteristics of lithium batteries have become increasingly important for applications in fields such as electric vehicles. In order to meet the use, lithium batteries with large unit volume discharge capacity, high energy density and excellent life characteristics are required.

[0005] In a lithium battery, a separator is provided between a positive electrode and a negative electrode to prevent a short circuit (or reduce the possibility of a short circuit or the occurrence of a short circuit). An electrode assembly including a positive electrode, a negative electrode, and a separator provided between the positive electrode and the negative electrode is wound to have a jelly roll shape, and in the electrode assembly, the jelly roll is heat-pressed to improve adhesion between the positive electrode / negative electrode and the separator.

[0006] Olefin polymers are widely used as separators for lithium batteries. Although olefin polymers have excellent elasticity, they have low strength when immersed in an electrolyte, and the battery may short-circuit due to rapid thermal shrinkage at high temperatures of 100°C or higher. For this reason, for example, a separator that adds a shutdown function using polyethylene wax on a porous olefin polymer member is proposed. However, in a separator coated with polyethylene wax, the polyethylene wax melts at high temperatures and may not maintain the coating, so that the contact surface of the electrode plate increases, and thermal runaway increases.

[0007] Therefore, there is a need for separators that can improve battery stability at high temperatures. Summary of the invention

[0008] One or more embodiments include a separator having a coating that can maintain a network structure and ensure battery stability.

[0009] One or more embodiments include a lithium battery including a separator.

[0010] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the presented embodiments of the disclosure.

[0011] According to aspects of the embodiments,

[0012] The separator may include: a porous substrate; a first coating layer disposed on a surface of the porous substrate, the first coating layer including a melting point (T m ) organic particles, particulate boehmite, acicular ceramic particles, and a first binder in a range of about 100° C. to about 130° C.;

[0013] a first adhesive layer disposed on the other surface of the porous substrate, the first adhesive layer having a glass transition temperature (Tg) of 50° C. or higher and including a particle-type second binder; and

[0014] A second adhesive layer is disposed on the first coating layer, the second adhesive layer having a glass transition temperature (Tg) of 50° C. or higher and including a particle-type second binder.

[0015] According to another aspect of the embodiment,

[0016] A lithium battery may include: a positive electrode; a negative electrode; and a separator between the positive electrode and the negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and other aspects, features and advantages of certain embodiments of the present disclosure will become more apparent from the following description taken in conjunction with the accompanying drawings, in which:

[0018] Figure 1 A schematic diagram showing an embodiment of a lithium battery;

[0019] Figure 2 A schematic diagram showing an embodiment of a laminate structure and coating form of a separator;

[0020] Figure 3 A schematic diagram showing another embodiment of a laminate structure and coating form of a separator;

[0021] Figure 4 shows changes in ionic conductivity of separators prepared in Examples 1 to 5 and Comparative Examples 1 and 2 according to the content of needle-shaped ceramic particles in the coating layer of the separator;

[0022] Figure 5 is a scanning electron microscope (SEM) image of the separator prepared in Example 1 before being placed at high temperature;

[0023] Figure 6 This is a SEM image of the separator prepared in Example 1 after being placed at high temperature;

[0024] Figure 7 This is a SEM image of the separator prepared in Comparative Example 1 after being placed at high temperature. DETAILED DESCRIPTION

[0025] Reference will now be made in detail to the embodiments illustrated in the accompanying drawings, examples of which are shown in the accompanying drawings, wherein the same reference numerals refer to the same elements throughout. In this regard, the present embodiments may have different forms and should not be construed as being limited to the description set forth herein. Accordingly, the embodiments are described below simply by reference to the various figures to explain the various aspects of this description. As used herein, the term "and / or" includes any and all combinations of one or more related enumerated items. Expressions such as "at least one" when preceding a list of elements modify the entire list of elements, without modifying the individual elements of the list.

[0026] Hereinafter, a separator and a lithium battery including the separator according to embodiments will be described in detail.

[0027] According to an embodiment, the separator may include: a porous substrate; a first coating layer disposed on a surface of the porous substrate, the first coating layer including a melting point (T m ) in the range of about 100°C to about 130°C, organic particles, granular boehmite, needle-shaped ceramic particles and a first binder; a first binder layer disposed on the other surface of the porous substrate, the first binder layer having a glass transition temperature (Tg) of 50°C or higher and including a granular second binder; and a second binder layer disposed on the first coating layer, the second binder layer having a glass transition temperature (Tg) of 50°C or higher and including a granular second binder.

[0028] The particle-type boehmite includes spherical or non-spherical shapes.

[0029] The needle-shaped ceramic particles may be at least one selected from alumina (Al2O3), boehmite, BaSO4, MgO, Mg(OH)2, clay, SiO2, TiO2, ZnO, CaO, attapulgite, and 10SiO2-2Al2O3-Fe2O3-2MgO. Here, attapulgite is an aluminum magnesium silicate, which is a mineral belonging to the monoclinic (orthorhombic) crystal system.

[0030] Since the separator includes a coating layer on the surface of the porous substrate, the coating layer includes a melting point (T m ) organic particles having a range of about 100° C. to about 130° C. and a first binder having a melting point at least 30° C. higher than the melting point of the organic particles, even when the organic particles of the coating are at a high temperature, the shape of the coating can be maintained due to the network structure of the first binder having a higher melting point. Therefore, once shutdown occurs, a rapid increase in temperature and calorific value can be delayed. Therefore, a lithium battery with improved stability at high temperatures can be provided.

[0031] In the case of a coated separator in the prior art, for example, in order to solve the short circuit problem of the battery due to rapid thermal shrinkage at high temperature, a method of adding a shutdown function using polyethylene wax on a porous substrate has been proposed. However, the coated polyethylene wax melts at high temperatures and may not maintain the coating, so the contact surface of the separator may increase, thereby increasing thermal runaway.

[0032] To this end, the following separator is provided: wherein the separator is provided by mixing organic particles, the melting point of which is higher than the melting point (T m ) of the first binder, granular boehmite and needle-shaped ceramic particles to form a first coating on the surface of the porous substrate.

[0033] The first binder may coat the organic particles, the particulate boehmite, and the needle-shaped ceramic particles, or the first binder may embed the organic particles, the particulate boehmite, and the needle-shaped ceramic particles therein.

[0034] The first coating layer contains particulate boehmite and needle-shaped ceramic particles to improve the electrolyte impregnation characteristics, durability and safety of the separator.

[0035] The needle-shaped ceramic particles may be, for example, at least one selected from alumina (Al2O3), boehmite, BaSO4, MgO, Mg(OH)2, clay, SiO2, TiO2, ZnO, CaO, attapulgite, and 10SiO2-2Al2O3-Fe2O3-2MgO.

[0036] In one embodiment, the needle-shaped ceramic particles may be attapulgite, for example, a compound represented by the formula 3MgO-1.5Al2O3-8SiO2-9H2O.

[0037] The acicular ceramic particles may be, for example, ATTAGEL 40 commercially available in the art. ATTAGEL 40 is a finely ground attapulgite clay that provides excellent thickening and thixotropic properties in high quality aqueous systems such as latex. Another type of ATTAGEL brand clay product is ATTAGEL 30 or ATTAGEL 50.

[0038] The average particle size of the needle-shaped ceramic particles may be in the range of about 1 μm to about 20 μm, about 1.1 μm to about 18 μm, about 3 μm to about 16 μm, or about 5 μm to about 15 μm, and the aspect ratio of the needle-shaped ceramic particles may be in the range of about 1 to about 100, about 10 to about 95, about 15 to about 90, about 20 to about 85, about 30 to about 80, or about 30 to about 65. Here, the average particle size of the needle-shaped ceramic particles refers to the average length of the needle-shaped ceramic particles. The average particle size and aspect ratio can be identified by a scanning electron microscope (SEM). As a SEM analysis device, an ultra-high resolution field emission scanning electron microscope (S-4700 manufactured by Hitachi High-Technologies Co., Ltd.) is used. Images are taken using a SEM analysis device, and image analysis is performed by randomly selecting 50 particles to determine the average length or average particle size.

[0039] In addition, also for the aspect ratio, 50 particles are selected from the SEM image for image analysis and the average value is determined. Specifically, 50 particle images are selected in order from the largest, their entire images can be observed at 100 times magnification, and each image is observed at 1000 times magnification, and the average value of the aspect ratio is calculated. From the printed image, the average values ​​of the minor axis length, major axis length and aspect ratio of the needle-shaped ceramic particles can be obtained. The aspect ratio is determined as the ratio of the major axis length to the minor axis length (aspect ratio = major axis length / minor axis length).

[0040] When the needle-shaped ceramic particles have an average size and aspect ratio within these ranges, a separator having excellent ion conductivity, excellent air permeability characteristics, and excellent shutoff function can be manufactured.

[0041] The density of the needle-shaped ceramic particles according to one or more embodiments may be, for example, about 0.2 g / cm 2 To about 0.5g / cm 2 , about 0.25g / cm 2 To about 0.45g / cm 2 , about 0.3g / cm 2 To about 0.4g / cm 2 or about 0.35g / cm 2 To about 0.37g / cm 2 within the range.

[0042] The particle-type boehmite may have excellent heat absorption characteristics and have a hydroxyl group. Therefore, the particle-type boehmite may be controlled to have high hydrophilicity and a high specific surface area. The particle-type boehmite may contain primary particles, secondary particles as aggregates of primary particles, or any combination thereof.

[0043] The particle-type boehmite may be specifically spherical, plate-like, cubic or amorphous. The specific surface area may be 3 m 2 / g or more, 10m 2 / g or more, 30m 2 / g or more or 30m 2 / g to 50m 2 / g. The density can be about 0.1g / cm 3 About 30g / cm 3 The density can be calculated based on "Test methods for electrical insulating ceramic materials" (JIS C2141) according to JIS (Japanese Industrial Standards).

[0044] The average particle size of the particulate boehmite indicates the average particle diameter when the particulate boehmite is spherical or the major axis length when the particulate boehmite is non-spherical. The average particle size of the particulate boehmite may be in the range of about 0.1 μm to about 1.0 μm, about 0.2 μm to about 0.9 μm, about 0.3 μm to about 0.8 μm, or about 0.4 μm to about 0.6 μm.

[0045] In this specification, the term "average particle size" means D50 by volume. The average particle size can be measured, for example, using a measuring device and a measuring method such as a laser diffraction method or a dynamic light scattering method. The average particle size can be a value measured by using, for example, a laser scattering particle size distribution meter (e.g., Horiba LA-920), and is a median particle size (D50) corresponding to 50% in the cumulative particle size distribution curve from small particles.

[0046] The content of the needle-shaped ceramic particles may be in the range of about 1 part by weight to about 30 parts by weight, about 2 parts by weight to about 30 parts by weight, about 3 parts by weight to about 30 parts by weight, or about 5 parts by weight to about 30 parts by weight, based on 100 parts by weight of the total weight of the particulate boehmite and the needle-shaped ceramic particles. When the content of the needle-shaped ceramic particles is within any of these ranges, electrolyte impregnation characteristics are improved, and ionic conductivity is increased.

[0047] Based on 100 parts by weight of the inorganic particles, the total content of the particulate boehmite and the acicular ceramic particles may be in the range of about 20 parts by weight to about 50 parts by weight, about 20 parts by weight to about 40 parts by weight, or about 25 parts by weight to about 40 parts by weight. Herein, the term "inorganic particles" refers to a mixture of particulate boehmite and acicular ceramic particles.

[0048] Figure 2 Schematic diagram showing an embodiment of the laminate structure and coating form of the separator.

[0049] A first coating layer 11 may be formed on the porous substrate 10, which includes a melting point (T m) ranges from about 100° C. to about 130° C., organic particles, granular boehmite, needle-shaped ceramic particles, and a first binder, and a first binder layer 12 having a glass transition temperature (Tg) of 50° C. or higher, which contains a granular second binder, may be provided on the other surface of the porous substrate 10. A second binder layer 13 having a glass transition temperature (Tg) of 50° C. or higher, which includes a granular second binder, may be formed on the first coating layer 11.

[0050] like Figure 3 As shown in FIG. 1 , a second coating layer 11′ may be further included between the porous substrate 10 and the first adhesive layer 12, which includes a melting point (T m ) organic particles having a temperature ranging from about 100° C. to about 130° C., particulate boehmite, needle-shaped ceramic particles, and a second binder. The organic particles may be, for example, PE wax.

[0051] When the separator is exposed to high temperature, the organic particles dissolve and penetrate into the porous substrate, blocking the pores of the porous substrate, thereby inhibiting the flow of current and improving thermal stability. In addition, the needle-shaped ceramic particles can act as fillers together with the granular boehmite. Due to the large specific surface area of ​​the needle-shaped ceramic particles and the granular boehmite, the electrolyte impregnation can be improved, thereby increasing the ionic conductivity. The granular boehmite can improve the heat resistance and durability of the separator by giving the coating appropriate strength.

[0052] When the separator is exposed to high temperature, the organic particles dissolve or melt and penetrate into the porous substrate, which may cause the closure of the holes that block the porous substrate. Even when the organic particles dissolve or melt, the first binder with a high melting point in the coating can also maintain the matrix form of the mesh structure (retaining gaps where the organic particles dissolve or melt and disappear), thereby preventing the collapse of the coating. Therefore, in the separator according to the embodiment, by suppressing the increase of the contact surface of the electrode plate and delaying the rapid increase of the temperature and calorific value, the coating can be maintained when the shutdown occurs at high temperature. Therefore, the lithium battery can have improved stability at high temperatures.

[0053] The first coating layer 11 may be a closable shutdown layer, and may be coated on one surface or both surfaces of the porous substrate 10 .

[0054] The melting point (T m) may be in the range of about 100°C to about 130°C, for example, about 110°C to about 125°C. When the melting point of the organic particles is less than 100°C, unexpected heat and changes in the external environment may cause the organic particles to melt and block the pores of the separator, thereby reducing the output and usability of the battery. Therefore, the battery performance may be adversely affected. In addition, when the melting point of the organic particles exceeds 130°C, the separator may melt away, and therefore, it may be difficult to exert a shutdown effect by the organic particles. The organic particles may have a melting point, for example, in a range similar to the melting point of the porous substrate.

[0055] Melting point (T m ) Organic particles having a temperature range of about 100° C. to about 130° C. melt after being exposed to a high temperature, for example, a temperature of 120° C., the pores of the porous substrate may be blocked, and the flow of current may be suppressed, thereby improving the stability of the lithium battery. The organic particles may be, for example, selected from polyethylene (PE) wax, polypropylene (PP) wax, polystyrene (PS), polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA), acrylate compounds, polyacrylonitrile (PAN), azodicarbonamide compounds, derivatives thereof, and copolymers thereof. For example, the organic particles may be selected from at least one of polyethylene wax, polypropylene wax, polystyrene, and polymethyl methacrylate, but the embodiment is not limited thereto. For example, the organic particles may include polyethylene wax.

[0056] According to an embodiment, the organic particles may have at least one shape selected from a spherical shape, a particle shape, a plate shape, and a sheet shape, for example, the organic particles may be spherical. The organic particles may be, for example, selected from polyethylene (PE) wax, polypropylene (PP) wax, polystyrene (PS), polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA), acrylate compounds, polyacrylonitrile (PAN), azodicarbonamide compounds, derivatives thereof, and copolymers thereof. For example, the organic particles may be polyethylene (PE) wax.

[0057] The first binder included in the first coating layer may have a melting point that is at least 30°C higher than the melting point of the organic particles. For example, the first binder may have a melting point that is 30°C or more, 40°C or more, 50°C or more, 60°C or more, 70°C or more, 80°C or more, 90°C or more, or 100°C or more higher than the melting point of the organic particles. For example, the melting point of the first binder may be in the range of about 160°C to about 180°C, about 165°C to about 175°C, for example, about 170°C. By having such a high melting point in any of these ranges, the first binder having high heat resistance can maintain the matrix form of the network structure even when the separator is exposed to high temperature.

[0058] The first binder may be highly heat-resistant and include, for example, sulfonate compounds, acrylamide compounds, (meth) acrylic compounds, acrylonitrile compounds, derivatives thereof, copolymers thereof, mixtures thereof, or any combination thereof. The first binder may include, for example, sulfonate compounds or derivatives thereof, acrylamide compounds or derivatives thereof, and acrylonitrile compounds or derivatives thereof, copolymers thereof, or any combination thereof.

[0059] The first binder may include a (meth)acrylic copolymer including: a first repeating unit derived from (meth)acrylamide; a repeating unit derived from at least one selected from (meth)acrylic acid and (meth)acrylate; and a second repeating unit including at least one of (meth)acrylamide sulfonic acid and a salt thereof.

[0060] Based on 100 mol% of the (meth) acrylic copolymer, the first repeating unit in the range of about 55 mol% to about 95 mol%, about 60 mol% to about 90 mol% or about 65 mol% to about 85 mol% may be included. Based on 100 mol% of the (meth) acrylic copolymer, the second repeating unit in the range of about 5 mol% to about 45 mol%, about 10 mol% to 40 mol% or 15 mol% to about 35 mol% may be included. Based on 100 mol% of the (meth) acrylic copolymer, the repeating unit derived from (meth) acrylamide sulfonic acid and its salt in the second repeating unit may be 10 mol% or less, in the range of about 0.01 mol% to about 10 mol% or about 0.01 mol% to about 5 mol%. When the content of the repeating unit is in any of these ranges, the heat resistance and bonding strength of the separator can be further improved.

[0061] The first repeating unit derived from (meth) acrylamide may include an -NH2 functional group in the repeating unit. The -NH2 functional group may increase the bonding force between the porous substrate and the electrode, and, for example, form a hydrogen bond between the -OH functional group of the needle-shaped ceramic particles and the particle-type boehmite. The needle-shaped ceramic particles and the particle-type boehmite are used as inorganic particles. Therefore, the inorganic particles in the coating layer may be firmly fixed, and accordingly, the heat resistance of the separator may be further improved.

[0062] The repeating unit derived from at least one selected from (meth) acrylic acid and (meth) acrylic acid ester can be used to fix the inorganic particles on the porous substrate and provide a bonding force between the coating and the porous substrate and the electrode, thereby improving the heat resistance and air permeability of the separator. The repeating unit derived from at least one selected from (meth) acrylic acid and (meth) acrylic acid ester can include a carboxyl functional group (-C(=O)O-) in the repeating unit, and the carboxyl functional group can help improve the dispersibility of the coating slurry.

[0063] In addition, the repeating unit derived from (meth)acrylamidesulfonic acid or its salt includes a bulky functional group, thereby reducing the mobility of the copolymer including the (meth)acrylamidesulfonic acid or its salt, thereby enhancing the heat resistance of the separator.

[0064] The first repeating unit derived from (meth)acrylamide may, for example, be represented by Formula 1:

[0065] Formula 1

[0066]

[0067] In Formula 1, R 1 It can be hydrogen or a C1 to C6 alkyl group.

[0068] The repeating unit derived from at least one selected from (meth)acrylic acid and (meth)acrylic acid ester may be represented by, for example, any one of Formula 2, Formula 3, and any combination thereof:

[0069]

[0070] Among them, in formula 2 and formula 3, R 2 and R 3 may each independently be hydrogen or C1 to C6 alkyl, and R 7 It may be substituted or unsubstituted C1 to C 20 alkyl.

[0071] The repeating unit derived from (meth)acrylate may be derived from alkyl (meth)acrylate, perfluoroalkyl (meth)acrylate, or (meth)acrylate having a functional group in a side chain, for example, alkyl (meth)acrylate. In addition, the number of carbons in the alkyl or perfluoroalkyl group bonded to the non-carbonyl oxygen atom of the alkyl (meth)acrylate or perfluoroalkyl (meth)acrylate may be specifically 1 to 20, more specifically 1 to 10, for example, 1 to 5.

[0072] Examples of alkyl (meth)acrylates having 1 to 5 carbons in the alkyl or perfluoroalkyl group bonded to the non-carbonyl oxygen atom may include: alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, and tert-butyl acrylate; 2-(perfluoroalkyl)ethyl acrylates such as 2-(perfluorobutyl)ethyl acrylate and 2-(perfluoropentyl)ethyl acrylate; alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, and tert-butyl methacrylate; and 2-(perfluoroalkyl)ethyl methacrylates such as 2-(perfluorobutyl)ethyl methacrylate, 2-(perfluoropentyl)ethyl methacrylate, and 2-(perfluorohexyl)ethyl methacrylate.

[0073] Examples of the alkyl (meth)acrylates may include: alkyl acrylates having 6 to 18 carbons in the alkyl group bound to the non-carbonyl oxygen atom, such as n-hexyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, dodecyl acrylate, octadecyl acrylate, cyclohexyl acrylate, and isobornyl acrylate; alkyl methacrylates having 6 to 18 carbons in the alkyl group bound to the non-carbonyl oxygen atom, such as n-hexyl methacrylate, 2-ethylhexyl methacrylate, octyl methacrylate, isodecyl methacrylate, dodecyl methacrylate, tridecyl methacrylate, octadecyl methacrylate, and cyclohexyl methacrylate; 2-(perfluoroalkyl)ethyl acrylates having 6 to 18 carbons in the perfluoroalkyl group bound to the non-carbonyl oxygen atom, such as 2-(perfluorohexyl)ethyl acrylate; )ethyl acrylate, 2-(perfluorooctyl)ethyl acrylate, 2-(perfluorononyl)ethyl acrylate, 2-(perfluorodecyl)ethyl acrylate, 2-(perfluorododecyl)ethyl acrylate, 2-(perfluorotetradecyl)ethyl acrylate, and 2-(perfluorohexadecyl)ethyl acrylate; and 2-(perfluoroalkyl)ethyl methacrylates having 6 to 18 carbons in the perfluoroalkyl group bound to the non-carbonyl oxygen atom, such as 2-(perfluorohexyl)ethyl methacrylate, 2-(perfluorooctyl)ethyl methacrylate, 2-(perfluorononyl)ethyl methacrylate, 2-(perfluorodecyl)ethyl methacrylate, 2-(perfluorododecyl)ethyl methacrylate, 2-(perfluorotetradecyl)ethyl methacrylate, and 2-(perfluorohexadecyl)ethyl methacrylate.

[0074] For example, the repeating unit derived from at least one selected from (meth)acrylic acid and (meth)acrylate may include a repeating unit represented by Formula 2 and a repeating unit represented by Formula 3. When the repeating unit includes both the repeating unit represented by Formula 2 and the repeating unit represented by Formula 3, a molar ratio of the repeating unit represented by Formula 2 to the repeating unit represented by Formula 3 may be in the range of about 10:1 to about 1:1, about 6:1 to about 1:1, or about 3:1 to about 1:1.

[0075] The repeating unit including at least one of (meth)acrylamidosulfonic acid and its salt may be derived from (meth)acrylamidosulfonic acid or (meth)acrylamidosulfonic ester, and the (meth)acrylamidosulfonic ester may be a conjugate base of (meth)acrylamidosulfonic acid, (meth)acrylamidosulfonic acid salt or a derivative thereof. The repeating unit derived from (meth)acrylamidosulfonic acid or (meth)acrylamidosulfonic ester may be represented by one of Formula 4, Formula 5, Formula 6 and any combination thereof.

[0076]

[0077] Among them, in equations 4 to 6, R 4 , R 5 and R 6 may be independently hydrogen or C1 to C6 alkyl, L 1 , L 2 and L 3 may be independently substituted or unsubstituted C1 to C 10 Alkylene, substituted or unsubstituted C3 to C 20 Cycloalkylene, substituted or unsubstituted C6 to C 20 Arylene or substituted or unsubstituted C3 to C 20 The heterocyclic group, a, b and c may each independently be an integer of 0 to 2, M may be an alkali metal, and the alkali metal may be, for example, lithium, sodium, potassium, rubidium or cesium.

[0078] In equations 4 to 6, L 1 , L 2 and L 3 may be independently substituted or unsubstituted C1 to C 10 alkylene, and a, b and c may each be 1.

[0079] The repeating unit including at least one of (meth)acrylamide sulfonic acid and its salt may include each or at least two of the repeating unit represented by Formula 4, the repeating unit represented by Formula 5, and the repeating unit represented by Formula 6. For example, the repeating unit including at least one of (meth)acrylamide sulfonic acid and its salt may include the repeating unit represented by Formula 5. For example, the repeating unit including at least one of (meth)acrylamide sulfonic acid and its salt may include the repeating unit represented by Formula 5 and the repeating unit represented by Formula 6.

[0080] When the repeating unit including at least one of (meth)acrylamide sulfonic acid and a salt thereof includes both the repeating unit represented by Formula 5 and the repeating unit represented by Formula 6, the molar ratio of the repeating unit represented by Formula 5 to the repeating unit represented by Formula 6 may be in the range of about 10:1 to about 1:2, about 5:1 to about 1:1, or about 3:1 to about 1:1.

[0081] The sulfonate in the repeating unit derived from (meth)acrylamidosulfonic acid or its salt may be a functional group derived from, for example, vinylsulfonic acid, allylsulfonic acid, styrenesulfonic acid, anetholesulfonic acid, acrylamidoalkanesulfonic acid, sulfoalkyl(meth)acrylate or its salt. Here, the alkane may be C1 to C 20 Alkanes, C1 to C 10 Alkanes or C1 to C6 alkanes, and the alkyl group may be C1 to C 20 Alkyl, C1 to C 10 Alkyl or C1 to C6 alkyl. Salt means a salt including the aforementioned sulfonate or a suitable ion. The ion may be, for example, an alkali metal ion, and the salt may be a sulfonate alkali metal salt.

[0082] The acrylamidoalkanesulfonic acid may be, for example, 2-acrylamido-2-methylpropanesulfonate, and the sulfoalkyl(meth)acrylate may be, for example, 2-sulfoethyl(meth)acrylate or 3-sulfopropyl(meth)acrylate.

[0083] An example of a (meth)acrylic copolymer can be represented by Formula 7:

[0084] Formula 7

[0085]

[0086] Among them, in formula 7, R 8 To R 10 can be independently hydrogen or methyl, R 11 It can be hydrogen or C1 to C6 alkyl, L 2 It may be substituted or unsubstituted C1 to C 10 Alkylene, substituted or unsubstituted C3 to C 20 Cycloalkylene, substituted or unsubstituted C6 to C 20Arylene or substituted or unsubstituted C3 to C 20 The heterocyclic group, b may be an integer of 0 to 2, M may be an alkali metal such as lithium, sodium, potassium, rubidium or cesium, and l, m and n may each indicate a molar ratio per unit.

[0087] In Formula 7, l+m+n=1. In some embodiments, 0.05≤(l+n)≤0.45 and 0.55≤m≤0.95, for example, 0≤l≤0.4 and 0≤n≤0.1, or for example, 0.9≤m≤0.95, 0≤l≤0.05, and 0≤n≤0.05.

[0088] For example, in Formula 7, L 2 It may be substituted or unsubstituted C1 to C 10 alkylene, and b may be 1.

[0089] Based on 100 mol% of the total amount of the (meth)acrylamide sulfonic acid repeating units, the (meth)acrylic copolymer containing the alkali metal (M + The amount of the repeating unit substituted with methyl methacrylate may be in the range of about 50 mol % to about 100 mol %, for example, about 60 to about 90 mol %, or for example, about 70 to about 90 mol %. When any of these ranges are satisfied, the (meth)acrylic copolymer and the separator including the (meth)acrylic copolymer may have excellent bonding strength, heat resistance and oxidation resistance.

[0090] The (meth)acrylic copolymer may further include other units in addition to the aforementioned units. For example, the (meth)acrylic copolymer may further include units derived from (meth)acrylic acid alkyl esters, units derived from dienes, units derived from styrene groups, units containing ester groups, units containing carbonate groups, or any combination thereof.

[0091] The (meth)acrylic copolymer may be in various forms such as an alternating polymer in which the units are alternately distributed, a random polymer in which the units are randomly distributed, or a graft polymer in which some structural units are grafted.

[0092] The weight average molecular weight of the (meth) acrylic copolymer may be in the range of about 350,000 Daltons to about 970,000 Daltons, about 450,000 Daltons to about 970,000 Daltons, or about 450,000 Daltons to about 700,000 Daltons. When the weight average molecular weight of the (meth) acrylic copolymer satisfies any of these ranges, the (meth) acrylic copolymer and the separator including the (meth) acrylic copolymer may exhibit excellent bonding, heat resistance and air permeability. The weight average molecular weight may be an average molecular weight according to polystyrene measured using gel permeation chromatography.

[0093] The (meth)acrylic copolymer can be prepared by various known methods such as emulsion polymerization, suspension polymerization, solution polymerization or bulk polymerization.

[0094] The first binder may be at least one selected from the group consisting of poly(acrylic acid-co-acrylamide-co-2-acrylamido-2-methylpropanesulfonic acid) sodium salt, poly(acrylic acid acryl amide acrylamido sulfonic acid) and a salt of poly(acrylic acid acryl amide acrylamido sulfonic acid).

[0095] The first binder may be present in an amount ranging from about 1 to about 15 parts by weight, about 3 to about 12 parts by weight, about 3 to about 10 parts by weight, or about 3 to about 8 parts by weight, based on 100 parts by weight of the total weight of the organic particles, the particulate boehmite, the needle-shaped ceramic particles, and the first binder. The first binder may effectively coat the surface of the organic particles within any of these ranges to form a matrix of a network structure surrounding the organic particles.

[0096] The first coating layer may include needle-shaped ceramic particles. Since the first coating layer includes needle-shaped ceramic particles, the possibility of short circuit between the positive electrode and the negative electrode can be reduced, the stability of the battery can be improved, the reduction of the separator area at high temperature can be further suppressed, a relatively high porosity can be ensured, and the characteristics after evaluating the permeability of the lithium battery can be improved.

[0097] Based on the total weight of the organic particles, the particulate boehmite, the needle-shaped ceramic particles, and the first binder, the content of the organic particles in the first coating layer may be in the range of about 50 wt % to about 80 wt %, about 55 wt % to about 80 wt %, or about 60 wt % to about 80 wt %. When the content of the organic particles is within any of these ranges, the battery may have improved stability at high temperatures.

[0098] According to an embodiment, the thickness of the first coating layer may be in the range of about 0.1 μm to about 5 μm, about 0.5 μm to about 5 μm, about 1 μm to about 5 μm, or about 3 μm to about 5 μm. When the thickness of the first coating layer is within any of these ranges, the separator may provide an improved shutdown function and air permeability, and reduce the thickness of the electrode assembly, thereby maximizing the battery capacity per unit volume.

[0099] According to an embodiment, the particle-type second binder may be an aqueous binder, which may exist in a particle form after coating and drying. For example, the aqueous binder may include an acrylate group and / or a styrene group.

[0100] The aqueous binder has a glass transition temperature (Tg) of 50° C. or higher.

[0101] As the particle type second binder, a binder with a common bonding force can be used. For example, the particle type second binder may include at least one selected from acrylic resin, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, polymethyl methacrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, ethylene vinyl acetate copolymer, polyethylene oxide, cellulose acetate, butyl cellulose acetate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile styrene butadiene copolymer and polyimide, but embodiments are not limited thereto. Acrylic resin may be, for example, poly (2-ethylhexyl acrylate).

[0102] The particle-type second binder in the embodiment may include a particle-type acrylic resin, a particle-type polyvinylidene fluoride, or any combination thereof. Here, the acrylic resin may be, for example, poly(2-ethylhexyl acrylate).

[0103] The average particle size of the particulate second binder may be in the range of about 100 nm to about 800 nm, about 150 nm to about 800 nm, or about 200 nm to about 800 nm. When the average particle size of the particulate second binder is within any of these ranges, a separator having excellent bonding strength may be manufactured.

[0104] In some embodiments, the average particle size of the particulate second binder in the first adhesive layer and the second adhesive layer may be in the range of about 100 nm to about 500 nm, for example, it may be a particulate acrylic resin having an average particle size range of about 400 nm to about 500 nm or a particulate polyvinylidene fluoride having an average particle size range of about 100 nm to about 300 nm.

[0105] The first adhesive layer and the second adhesive layer may each include a fluorine-based adhesive. A fluorine-based adhesive is an adhesive in which some or all of the hydrogen bonded to the carbon is replaced by fluorine. For example, the fluorine-based adhesive may be a polymer comprising repeating units derived from at least one monomer selected from vinylidene fluoride monomers, tetrafluoroethylene monomers, and hexafluoropropylene. The fluorine-based adhesive may be, for example, a fluorine-based homopolymer or a fluorine-based copolymer.

[0106] The thickness of the first adhesive layer and the second adhesive layer may each be in the range of about 0.1 μm to about 5 μm, about 0.1 μm to about 3 μm, about 0.3 μm to about 2 μm, or about 0.5 μm to about 1 μm. When the thickness of each of the first adhesive layer and the second adhesive layer is within any of these ranges, the first adhesive layer and the second adhesive layer may effectively provide bonding between the coating and the electrode plate.

[0107] The porous substrate included in the separator may be a porous film containing polyolefin. Polyolefin may have an excellent anti-short circuit effect, and battery stability may be improved by a shutdown effect. For example, the porous substrate may be a film including a resin (such as a polyolefin, such as polyethylene, polypropylene, polybutylene or polyvinyl chloride, and mixtures or copolymers thereof). For example, a porous film including a polyolefin resin, a porous film woven with polyolefin fibers, an aggregate of nonwoven fabrics or insulating material particles including polyolefins, etc. may be used as a porous substrate. For example, a porous film containing polyolefin may have excellent applicability for preparing a binder solution for a coating formed on a porous substrate, and by thinning the thickness of the film of the separator to increase the proportion of active materials in the battery, the capacity per unit volume may be increased.

[0108] The polyolefin used as the material of the porous substrate may be, for example, a homopolymer, such as polyethylene or polypropylene, a copolymer, or a mixture thereof. Polyethylene may be low-density, medium-density or high-density polyethylene, and in terms of mechanical strength, polyethylene may be high-density polyethylene. In addition, polyethylene may be a mixture of at least two types of polyethylene to impart elasticity. The polymerization catalyst for preparing polyethylene is not particularly limited, and Ziegler-Natta catalysts, Phillips catalysts or metallocene catalysts may be used. Considering the coordination of mechanical strength and high permeability, the weight-average molecular weight of polyethylene may be in the range of about 100,000 daltons to about 12,000,000 daltons, or, for example, about 200,000 daltons to about 3,000,000 daltons. Polypropylene may be a homopolymer, a random copolymer or a block copolymer, and polypropylene may be used alone or in a mixture of at least two thereof. In addition, the polymerization catalyst is not particularly limited, and Ziegler-Natta catalysts or metallocene catalysts may be used. In addition, stereoregularity is not particularly limited, and the polypropylene stereoregularity can be isotactic, syndiotactic or atactic. Cheap isotactic polypropylene can be used. In addition, although it will not have an adverse effect on one or more embodiments, additives such as polyolefins and antioxidants other than polyethylene and polypropylene can be added to the polyolefin.

[0109] The porous substrate included in the separator may include, for example, polyolefins such as polyethylene or polypropylene, and a multilayer film of at least two layers may be used. For example, a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator or a polypropylene / polyethylene / polypropylene three-layer separator may be used, but the embodiment is not limited thereto. Any suitable material and composition available in the art for the porous substrate may be used. The porous substrate included in the separator may include, for example, a diene polymer prepared by polymerizing a monomer composition including a diene monomer. The diene monomer may be a conjugated diene monomer or a non-conjugated diene monomer. For example, the diene monomer may include at least one selected from the group consisting of: 1,3-butadiene, isoprene, 2-chloro-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, vinylpyridine, vinyl norbornene, dicyclopentadiene and 1,4-hexadiene, but the embodiment is not limited thereto. Any suitable diene monomer available in the art may be used.

[0110] The thickness of the porous substrate included in the separator may be in the range of about 1 μm to about 100 μm, about 1 μm to about 30 μm, about 5 μm to about 20 μm, about 5 μm to about 15 μm, or about 5 μm to about 10 μm. When the thickness of the porous substrate is less than 1 μm, it may be difficult to maintain the mechanical properties of the separator, and when the thickness of the porous substrate exceeds 100 μm, the internal resistance of the lithium battery may increase. The porosity of the porous substrate included in the separator may be in the range of about 5% to about 95%. When the porosity is less than 5%, the internal resistance of the lithium battery may increase, and when the porosity is greater than 95%, it may be difficult to maintain the mechanical properties of the porous substrate. The pore size of the porous substrate in the separator may be in the range of about 0.01 μm to about 50 μm. For example, the pore size of the porous substrate in the separator may be in the range of about 0.01 μm to about 20 μm. For example, the pore size of the porous substrate in the separator may be in the range of about 0.01 μm to about 10 μm. When the pore size is less than 0.01 μm, the internal resistance of the lithium battery may increase, and when the pore size is greater than 50 μm, it may be difficult to maintain the mechanical properties of the porous substrate.

[0111] Any suitable method of preparing separators available in the art may be used.

[0112] For example, the composition for forming the first coating layer can be applied on the surface of the porous substrate and dried to form the first coating layer, and the composition for forming the first adhesive layer can be applied on the other surface of the porous substrate and dried to form the first adhesive layer. Subsequently, after applying the composition for forming the second adhesive layer on the first coating layer, the composition can be dried to form the second adhesive layer, thereby manufacturing the separator.

[0113] The method for coating each of the composition for forming the first coating, the composition for forming the first adhesive layer and the composition for forming the second adhesive layer is not particularly limited. Any suitable method available in the art can be used. For example, each layer can be formed by methods such as printing, roller coating, scraping, dipping or spraying.

[0114] A lithium battery according to an embodiment may include a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode. According to an embodiment, a lithium battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode, wherein the electrode assembly is wound into a jelly roll shape. Since the lithium battery includes the above-mentioned separator, the stability of the lithium battery can be ensured by maintaining a coating of a mesh structure at high temperatures.

[0115] A lithium battery can be manufactured, for example, as follows.

[0116] A negative electrode active material, a conductive agent, a binder, and a solvent are mixed to prepare a negative electrode active material composition. In one or more embodiments, the negative electrode active material composition may be directly coated on a metal current collector to prepare a negative electrode plate. In one or more embodiments, the negative electrode active material composition may be cast on a separate support to form a negative electrode active material film, which may then be separated from the support and laminated on a metal current collector to prepare a negative electrode plate. The negative electrode is not limited to the above examples and may have various other shapes.

[0117] The negative electrode active material may be, for example, a carbonaceous material, a non-carbonaceous material, or any combination thereof.

[0118] The example of carbonaceous material can include crystalline carbon, amorphous carbon and mixture thereof. The example of crystalline carbon can include graphite, such as natural graphite or artificial graphite in shapeless, plate-like, flaky, spherical or fibrous form. The example of amorphous carbon can include soft carbon (low temperature sintered carbon), hard carbon, mesophase pitch carbide and sintered coke.

[0119] As the non-carbonaceous material, for example, the negative electrode active material may include at least one selected from the group consisting of a metal that can form an alloy with lithium, an alloy of a metal that can form an alloy with lithium, and an oxide of a metal that can form an alloy with lithium.

[0120] Examples of metals that can form alloys with lithium include silicon (Si), tin (Sn), aluminum (Al), germanium (Ge), lead (Pb), bismuth (Bi), antimony (Sb), Si-Y alloys (wherein Y is an alkali metal, an alkaline earth metal, an element of Groups 13 to 16, a transition metal, a rare earth element, or any combination thereof, and Y is not Si) and Sn-Y alloys (wherein Y is an alkali metal, an alkaline earth metal, an element of Groups 13 to 16, a transition metal, a rare earth element, or any combination thereof, and Y is not Sn). Y can be magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), (Rf), vanadium (V), niobium (Nb), tantalum (Ta), (Db), chromium (Cr), molybdenum (Mo), tungsten (W), (Sg), technetium (Tc), rhenium (Re), (Bh), iron (Fe), lead (Pb), ruthenium (Ru), osmium (Os), (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), aluminum (Al), gallium (Ga), tin (Sn), indium (In), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), or any combination thereof.

[0121] For example, the transition metal oxide may be lithium titanium oxide, vanadium oxide, or lithium vanadium oxide.

[0122] Examples of non-transition metal oxides include SnO2 and SiO x (where 0 <x≤2)。

[0123] As the non-carbonaceous material, the negative electrode active material may be at least one selected from the group consisting of Si, Sn, Pb, Ge, Al, SiO x (where 0 <x≤2)、SnO y (where 0 <y≤2)、Li4Ti5O 12 , TiO2, LiTiO3 and Li2Ti3O7, but the embodiment is not limited thereto. Any suitable non-carbonaceous material available in the art may be used.

[0124] In addition, a composite of a non-carbonaceous material and a carbonaceous material may be used, and a carbonaceous material may be further included in addition to the non-carbonaceous material.

[0125] The example of carbonaceous material can include crystalline carbon, amorphous carbon and mixture thereof. The example of crystalline carbon can include graphite, such as natural graphite or artificial graphite in shapeless, plate-like, flaky, spherical or fibrous form. The example of amorphous carbon can include soft carbon (low temperature sintered carbon), hard carbon, mesophase pitch carbide and sintered coke.

[0126] The conductive agent may be acetylene black, ketjen black, natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, and metal powders and metal fibers such as copper, nickel, aluminum or silver. In some embodiments, at least one conductive material such as a polyphenylene derivative may be used alone or in combination, but the embodiments are not limited thereto. Any suitable conductive agent available in the art may be used. Any of the above-mentioned crystalline carbonaceous materials may be added as a conductive agent.

[0127] Examples of the binder may include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, and styrene-butadiene rubber polymer may be used as a binder, but the embodiment is not limited thereto. Any suitable material that can be used as a binder in the art may further be used.

[0128] Examples of the solvent include N-methyl-pyrrolidone, acetone, and water, but the embodiment is not limited thereto. Any appropriate material that can be used as a solvent in the art may be used.

[0129] The amounts of the negative electrode active material, the conductive agent, the binder and the solvent may be the same as those generally used in the field of lithium batteries. Depending on the purpose and structure of the lithium battery, at least one of the conductive agent, the binder and the solvent may be omitted.

[0130] A positive electrode active material, a conductive agent, a binder, and a solvent are mixed to prepare a positive electrode active material composition. In one or more embodiments, the positive electrode active material composition may be directly coated on a metal current collector and then dried to prepare a positive electrode plate. In one or more embodiments, the positive electrode active material composition may be cast on a separate support to form a positive electrode active material film, which may then be separated from the support and laminated on a metal current collector to prepare a positive electrode plate.

[0131] The positive electrode active material may further include at least one selected from lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphorus oxide, and lithium manganese oxide, but the embodiment is not limited thereto. Any suitable positive electrode active material available in the art may be used.

[0132] The positive electrode active material may be, for example, a compound represented by one of the following formulae: Li a A 1-b B' bD2, where 0.90≤a≤1.8 and 0≤b≤0.5; Li a E 1-b B' b O 2-c D c , where 0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05; LiE 2-b B' b O 4-c D c , where 0≤b≤0.5 and 0≤c≤0.05; Li a Ni 1-b-c Co b B' c D α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2; Li a Ni 1-b-c Co b B' c O 2-α F' α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2; Li a Ni 1-b-c Co b B' c O 2-α F'2, where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2; Li a Ni 1-b-c Mn b B' c D α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2; Li a Ni 1-b- c Mn b B' c O 2-α F' α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2; Li a Ni 1-b-c Mn b B' c O 2-α F'2, where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2; Li a Ni b E c G dO2, where 0.90≤a≤1.8, 0≤b≤0.9, and 0≤c≤0.5, 0.001≤d≤0.1; Li a Ni b Co c Mn d G e O2, where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1; Li a NeG b O2, where 0.90≤a≤1.8 and 0.001≤b≤0.1; Li a CoG b O2, where 0.90≤a≤1.8 and 0.001≤b≤0.1; Li a MnG b O2, where 0.90≤a≤1.8 and 0.001≤b≤0.1; Li a Mn b O4, where 0.90≤a≤1.8 and 0.001≤b≤0.1; QO2; QS2; LiQS2; V2O5; LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3 -f)Fe2(PO4)3, where 0≤f≤2; and LiFePO4.

[0133] In the aforementioned formula, A may be selected from nickel (Ni), cobalt (Co), manganese (Mn) and any combination thereof; B' may be selected from aluminum (Al), Ni, Co, Mn, chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), rare earth elements and any combination thereof; D may be selected from oxygen (O), fluorine (F), sulfur (S), phosphorus (P) and any combination thereof; E may be selected from Co, Mn and any combination thereof; F' may be selected from F, S, P and any combination thereof; G may be selected from Al, Cr, Mn, Fe, Mg, lanthanum (La), cerium (Ce), Sr, V and any combination thereof; Q may be selected from titanium (Ti), molybdenum (Mo), Mn and any combination thereof; I' may be selected from Cr, V, Fe, scandium (Sc), yttrium (Y) and any combination thereof; and J may be selected from V, Cr, Mn, Co, Ni, copper (Cu) and any combination thereof.

[0134] The compounds listed above as positive active materials may have a surface coating (hereinafter, also referred to as "coating"). Alternatively, a mixture of a compound without a coating and a compound with a coating may be used, the compound being selected from the compounds listed above. In one or more embodiments, the coating may include at least one compound of a coating element selected from the group consisting of oxides, hydroxides, oxyhydroxides, oxycarbonates and basic carbonates of the coating element. In one or more embodiments, the compound for the coating may be amorphous or crystalline. In one or more embodiments, the coating element for the coating may be magnesium (Mg), aluminum (Al), cobalt (Co), potassium (K), sodium (Na), calcium (Ca), silicon (Si), titanium (Ti), vanadium (V), tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr) or a mixture thereof. In one or more embodiments, the coating may be formed using any suitable method, and when a compound of the coating element is used, the method does not adversely affect the physical properties of the positive active material. For example, a coating may be formed using a spraying method or an impregnation method. The coating method is well understood by those of ordinary skill in the art, and therefore a detailed description thereof will be omitted.

[0135] For example, LiNiO2, LiCoO2, LiMn x O 2x (where x = 1 or 2), LiNi 1-x Mn x O2 (where 0 <x<1)、LiNi 1-x-y Co x Mn y O2 (wherein 0≤x≤0.5 and 0≤y≤0.5), LiFeO2, V2O5, TiS or MoS.

[0136] In one or more embodiments, the conductive agent, binder and solvent used for the positive active material composition may be the same as the conductive agent, binder and solvent used for the negative active material composition. A plasticizer may be further added to the positive active material composition and / or the negative active material composition to form pores inside the electrode plate.

[0137] The amounts of the positive electrode active material, the conductive agent, the binder and the solvent may be within the range commonly used in lithium batteries. Depending on the purpose and structure of the lithium battery, at least one of the conductive agent, the binder and the solvent may be omitted.

[0138] The binder used to prepare the positive electrode may be the same as the coating composition contained in the coating layer of the separator.

[0139] Next, a separator may be disposed between the positive electrode and the negative electrode.

[0140] The separator may be separately prepared and disposed between the positive electrode and the negative electrode.

[0141] Next, an electrolyte is prepared.

[0142] The electrolyte may be a liquid or a gel electrolyte.

[0143] For example, the electrolyte may be an organic electrolyte solution. In some embodiments, the electrolyte may be a solid electrolyte. For example, the solid electrolyte may be boron oxide or lithium nitrogen oxide, but the embodiment is not limited thereto. Any suitable material that can be used as a solid electrolyte in the art can be used. The solid electrolyte can be formed on the negative electrode by, for example, sputtering.

[0144] For example, an organic electrolyte solution may be prepared. The organic electrolyte solution may be prepared by dissolving a lithium salt in an organic solvent.

[0145] Any suitable organic solvent available in the art can be used as the organic solvent. For example, the organic solvent can be selected from propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, ethylene dichloride, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, methyl propionate, ethyl propionate, propyl propionate and any combination thereof.

[0146] The lithium salt may be any suitable material that can be used as a lithium salt in the art. For example, the lithium salt may be LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers), LiCl, LiI or a mixture thereof.

[0147] The lithium battery 1 may include a positive electrode 3, a negative electrode 2 and a separator 4, such as Figure 1. The positive electrode 3, the negative electrode 2 and the separator 4 according to one or more embodiments may be wound or folded to form an electrode assembly. The electrode assembly may then be sealed in a battery case 5. The battery case 5 is then filled with an organic electrolyte solution and sealed with a capping assembly 6, thereby completing the manufacture of the lithium battery 1. The battery case 5 may be a cylindrical type, a rectangular type or a film type. In one or more embodiments, the lithium battery 1 may be a lithium ion battery. In one or more embodiments, the lithium battery 1 may be a lithium polymer battery.

[0148] The lithium battery 1 may have improved lifespan characteristics and high rate characteristics, and thus may be used in electric vehicles (EVs), for example, in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs).

[0149] Hereinafter, exemplary embodiments will be described in detail with reference to Examples and Comparative Examples. These examples are provided for illustrative purposes only and are not intended to limit the scope of the inventive concept.

[0150] (Preparation of separator)

[0151] Example 1

[0152] As organic particles, polyethylene wax (PE wax) having a spherical shape with an average particle size (D50) of 1.0 μm (melting point of 111° C.) was used. As the first binder, poly(acrylic acid-co-acrylamide-co-2-acrylamide-2-methylpropanesulfonic acid) sodium salt, which is a copolymer, was used. Poly(acrylic acid-co-acrylamide-co-2-acrylamide-2-methylpropanesulfonic acid) sodium salt was prepared according to Synthesis Example 7 of KR 10-2020-0032542. Here, the molar ratio of acrylate to acrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 20:75:5. The melting point (T m ) is 170°C. As the granular boehmite, BG611 (Anhui Estone MaterialTechnology Co., Ltd.) with an average particle size range of 0.4μm to 0.6μm (D50 based on volume) is used. As the needle-shaped ceramic particles, ATTAGEL 40 (BASF Co.) (needle-shaped filler with an average size of 11μm and an aspect ratio of 50) is used. Based on 100 parts by weight of organic particles (polyethylene (PE) wax), the total content of inorganic particles (granular boehmite and needle-shaped ceramic particles) is 25 parts by weight, and the mixing weight ratio of granular boehmite to needle-shaped ceramic particles is 95:5.

[0153] Assuming that the polyethylene wax is fully dissolved at a temperature of 150°C, the ratio of organic particles to inorganic particles in the coating is considered to be the porosity, so that the porosity of the coating is 70%, 76.4 parts by weight of organic particles (PE wax), 4.5 parts by weight of the first binder (poly(acrylic acid-co-acrylamide-co-2-acrylamide-2-methylpropane sulfonic acid) sodium salt) and 19.1 parts by weight of inorganic particles (granular boehmite and needle-shaped ceramic particles) are mixed together to prepare a slurry for forming the first coating. Here, a 20wt% slurry is prepared by using deionized water as a solvent. The slurry for forming the first coating is gravure printed on the surface of a polyethylene porous substrate (SK Innovation, PE) having a thickness of 5.5μm to form a first coating (shutdown layer) having a thickness of 4.0μm on the surface of the porous substrate.

[0154] Next, a slurry for forming an adhesive layer is prepared by mixing particulate poly (2-ethylhexyl acrylate) (BM-2570M available from Xeon) (D50 is 400nm to 500nm), a particulate polyvinylidene fluoride filler (D50 is 200nm) and water as a solvent. The slurry for forming an adhesive layer is gravure printed on the surface of the porous substrate and on the first coating, and then the slurry is dried at a temperature of 75°C. Thus, a first adhesive layer having a thickness of 1 μm is formed on the surface of the porous substrate. Next, a second adhesive layer having a thickness of 1 μm is formed on the first coating (shutdown layer). Thus, a separator having a total thickness of about 11.5 μm is manufactured.

[0155] Examples 2 to 5

[0156] The separator was manufactured in the same manner as in Example 1, except that the mixing weight ratio of the particulate boehmite as the inorganic particles and the needle-shaped ceramic particles was changed as shown in Table 1 in forming the slurry for forming the coating layer.

[0157] Example 6

[0158] The separator was manufactured in the same manner as in Example 1, except that in preparing the slurry for forming the coating layer, the average size (long axis length) of the needle-like ceramic particles was 15 μm, and the aspect ratio of the needle-like ceramic particles was 30.

[0159] Example 7

[0160] The separator was manufactured in the same manner as in Example 1, except that the aspect ratio of the needle-like ceramic particles was 80 in the preparation of the slurry for forming the coating layer.

[0161] Comparative Example 1

[0162] The separator was manufactured in the same manner as in Example 1, except that no needle-shaped ceramic particles were used in preparing the slurry for forming the coating layer.

[0163] Comparative Example 2

[0164] The separator was manufactured in the same manner as in Example 1, except that the particulate boehmite was not used in preparing the slurry for forming the coating layer.

[0165] Comparative Example 3

[0166] The separator was manufactured in the same manner as in Example 1, except that plate-like boehmite (having a major axis length of 1 μm and an aspect ratio of 10) was used instead of the needle-like ceramic particles in preparing the slurry for forming the coating layer.

[0167] According to Comparative Example 3, when boehmite having a large particle size was used, as shown in Table 3 below, the coating density decreased.

[0168] Table 1

[0169]

[0170] In Table 1, the loading level refers to the loading level of the first coating layer formed on the porous substrate, and the loading level was adjusted to constantly control the coating thickness at 4 μm. The coating density refers to the coating density of the first coating layer formed on the porous substrate.

[0171] (Manufacturing of lithium batteries)

[0172] Production Example 1

[0173] First, a negative electrode was prepared as follows.

[0174] 97wt% of graphite particles with an average particle size of 25μm, 1.5wt% of styrene-butadiene rubber (SBR) binder and 1.5wt% of carboxymethyl cellulose (CMC) were mixed together to prepare a mixture. Subsequently, distilled water was added to the mixture, followed by stirring with a mechanical stirrer for 60 minutes to prepare a negative electrode active material slurry. The negative electrode active material slurry was coated on a copper current collector having a thickness of 10μm using a scraper. A negative electrode plate was prepared by drying at a temperature of 100°C for 0.5 hours using a hot air dryer and vacuum drying at a temperature of 120 for 4 hours and rolling.

[0175] The positive electrode was prepared as follows.

[0176] 97wt% of LiCoO2, 1.5wt% of carbon black powder as a conductive agent and 1.5wt% of polyvinylidene fluoride (PVdF) were mixed, and the mixture was added to N-methyl-2-pyrrolidone solvent, followed by stirring with a mechanical stirrer for 30 minutes to prepare a positive active material slurry. The positive active material slurry was coated on an aluminum current collector with a thickness of 20μm using a scraper. The positive electrode plate was prepared by drying at a temperature of 100°C for 0.5 hours using a hot air dryer and vacuum drying at a temperature of 120°C for 4 hours and rolling.

[0177] (Electrode accessories)

[0178] The separator prepared in Example 1 was placed between the positive electrode plate and the negative electrode plate prepared above, and then rolled tightly to prepare an electrode assembly jelly roll. After the jelly roll was inserted into a bag and the electrolyte solution was injected therein, the bag was vacuum-sealed.

[0179] An electrolyte solution was used in which 1.3 M LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / diethyl carbonate (DEC) in a volume ratio of 3:5:2.

[0180] The jelly roll inserted into the bag was pre-charged to 50% SOC (state of charge) and simultaneously applied 250 kgf / cm 2 The jelly rolls were heat softened at 70°C for 1 hour while applying pressure.

[0181] Apply 200kgf / cm 2 The jelly roll was hot pressed at 85° C. for 180 seconds while applying a pressure of 1.5 %. During the hot rolling process, as the binder changes from a gel state to a sol state, a bonding force is generated between the positive electrode / negative electrode and the separator.

[0182] Then, 200 kgf / cm 2 The jelly roll is cold pressed at a temperature of 22° C. to 23° C. for 90 seconds while applying a pressure of 1.5° C. During the cold rolling process, the binder changes from a sol state to a gel state.

[0183] Then, the bag was degassed while applying 200 kgf / cm 2 The battery was charged with a constant current at a current rate of 0.2C for 1 hour at a temperature of 45°C until the voltage reached 4.3V, and then, the battery was charged with a constant voltage until the current reached 0.05C rate while maintaining 4.3V. Thereafter, the battery was discharged at a constant current rate of 0.2C until the voltage reached 3.0V. This cycle was repeated 5 times to perform the formation process.

[0184] Comparative Preparation Examples 1 and 2

[0185] Lithium batteries were respectively manufactured in the same manner as in Manufacturing Example 1, except that the separators manufactured in Comparative Examples 1 and 2 were used instead of the separator of Example 1.

[0186] Evaluation Example 1: Air Permeability

[0187] The air permeability per unit thickness of the separators of Examples 1 to 7 and Comparative Examples 1 to 3 was measured by using an air permeation tester (Asahi Seiko OKEN Type Air Permeation Tester: EGO1-55-1MR) according to the following method.

[0188] After preparing 10 samples cut at 10 different points to a size that can fit into a circle with a diameter of 1 inch, an ASAHI SEIKO OKEN air permeation tester EG01-55-1MR (Asahi Seiko) was used to measure the passage time of 100cc of air in each sample. After measuring the time five times, the average value was calculated to measure air permeability.

[0189] [Conditions for setting up the air permeability measurement device]

[0190] Measuring pressure: 0.05mPa, cylinder pressure: 2.5kgf / cm 2 , setting time: 10 seconds

[0191] The 1 m sample was measured at least 10 times at 10 cm intervals and the average of the data was recorded in Table 2.

[0192] Evaluation Example 2: Ionic Conductivity

[0193] The ion conductivities of the separators of Examples 1 to 7 and Comparative Examples 1 to 3 were measured at a temperature of 25° C. by using an EIS measuring device. The results are shown in Tables 2 and 3.

[0194] Table 2

[0195]

[0196] Table 3

[0197]

[0198]

[0199] In Tables 2 and 3, the coating thickness refers to the coating thickness of the first coating layer (shutdown layer) formed on the porous substrate, the loading level refers to the loading level of the first coating layer formed on the porous substrate, and the loading level is adjusted to constantly control the coating thickness at 4 μm.

[0200] As shown in Table 2 and Table 3, compared with the separators of Comparative Examples 1 and 3, it is found that the separators of Examples 1 to 7 all have excellent air permeability, improved coating density, and significant ionic conductivity increase effect. The separator of Comparative Example 2 includes a coating (shutdown layer) containing needle-shaped ceramic particles. Therefore, the coating has an increased density and an increased surface area of ​​the filler, thereby improving electrolyte solution impregnation and ionic conductivity. However, the separator of Comparative Example 2 has degraded heat resistance and durability. Therefore, the penetration characteristics of Evaluation Example 3 are poor, and therefore, the practical application of the separator is difficult.

[0201] In addition, in the separators of Examples 1 to 5 and Comparative Examples 1 and 2, changes in ionic conductivity of the separators according to changes in the content of the needle-shaped ceramic particles during the manufacturing process of the first coating layer were studied, and Figure 4 Displayed in.

[0202] See also Figure 4 , it was found that when the content of needle-shaped ceramic particles increased, the ionic conductivity of the separator improved.

[0203] Evaluation Example 3: Measurement of penetration characteristics

[0204] The jelly rolls were taken out of the bags of Manufacturing Example 1 and Comparative Manufacturing Examples 1 and 2 that had undergone the formation process, each separator was separated, and the permeation characteristics were evaluated. The results are shown in Table 4. After the needle penetration test was performed on each separator, the degree and probability of abnormal occurrence were evaluated based on the observed phenomena. L4-3 and L6 were evaluated as abnormal.

[0205] Table 4

[0206]

[0207] As shown in Table 4, the separator manufactured according to Manufacturing Example 1 has significantly improved permeation characteristics compared to the separators of Comparative Manufacturing Examples 1 and 2.

[0208] Evaluation Example 4: Scanning Electron Microscope (SEM) Analysis

[0209] In order to verify whether the separator prepared in Example 1 maintains a mesh structure when exposed to high temperature, the separator was placed at a high temperature of 120° C. for 1 hour, and then the separator was observed using a scanning electron microscope (SEM). The SEM observation results before and after the high temperature are shown in FIG. Figures 5 to 7 middle. Figure 5 This is a SEM image of the separator prepared in Example 1 before being placed at high temperature. Figure 6 for Figure 5 FIG. 4 is a SEM image of the separator prepared in Example 1 after being placed at high temperature. Figure 7 This is a SEM image of the separator prepared in Comparative Example 1 after being placed at high temperature.

[0210] like Figure 5 As shown in FIG. 1 , it can be seen that a first coating layer (ie, a shutdown layer) containing organic particles or inorganic particles is formed in the separator manufactured in Example 1. Figure 6 It is shown in the figure that in the separator prepared in Example 1, after the separator is placed at high temperature, the organic particles are dissolved or melted in the first coating layer, and the shape of the closed particles (i.e., organic particles) is maintained, thereby maintaining the matrix of the network structure. Since the first coating layer maintains the network structure, the thermal stability is improved and the air permeability is greatly increased.

[0211] Figure 7 : is a SEM image of the separator prepared in Comparative Example 1, which was observed after the separator was left at high temperature under the same conditions as the separator in Example 1. It was found that in the separator prepared in Comparative Example 1, after the separator was left at high temperature, not only the polyethylene wax particles but also the low melting point binder melted. Therefore, the coating was not maintained.

[0212] It is apparent from the foregoing description that the separator according to one aspect can maintain the coating of the mesh structure even at high temperatures. Therefore, when shutdown occurs, the rapid increase in temperature and calorific value can be delayed. Accordingly, the lithium battery can have improved stability at high temperatures.

[0213] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects within each embodiment should generally be considered to be applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the figures, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made herein without departing from the spirit and scope of the present disclosure as defined by the appended claims.

Claims

1. A partition, comprising: porous substrate; a first coating disposed on the surface of the porous substrate, the first coating comprising organic particles having a melting point ranging from 100° C. to 130° C., particulate boehmite, needle-shaped ceramic particles, and a first binder; a first adhesive layer disposed on the other surface of the porous substrate, the first adhesive layer having a glass transition temperature of 50° C. or higher and including a particle-type second binder; and a second adhesive layer disposed on the first coating layer, the second adhesive layer having a glass transition temperature of 50° C. or higher and including the particle-type second binder, The first coating layer includes the first binder in a network structure whose melting point is at least 30° C. higher than that of the organic particles. 2 . The separator of claim 1 , wherein the content of the acicular ceramic particles is in the range of 1 to 30 parts by weight based on 100 parts by weight of the total weight of the particulate boehmite and the acicular ceramic particles.

3. The separator as described in claim 1, wherein the needle-shaped ceramic particles are at least one selected from alumina, boehmite, BaSO4, MgO, Mg(OH)2, clay, SiO2, TiO2, ZnO, CaO, attapulgite and 10SiO2-2Al2O3-Fe2O3-2MgO. 4 . The separator of claim 1 , wherein an average size of the acicular ceramic particles is in the range of 1 μm to 20 μm, and an aspect ratio of the acicular ceramic particles is in the range of 1 to 100. 5 . 5 . The separator of claim 1 , wherein an average particle size of the granular boehmite is in the range of 0.1 μm to 1.0 μm.

6. The separator of claim 1, further comprising a second coating layer between the porous substrate and the first adhesive layer, the second coating layer comprising organic particles having a melting point ranging from 100°C to 130°C, particulate boehmite, needle-shaped ceramic particles, and a second binder.

7. The separator as claimed in claim 1, wherein the organic particles are at least one selected from polyethylene wax, polypropylene wax, polystyrene, polyvinylidene fluoride, polymethyl methacrylate, acrylate compounds, polyacrylonitrile, azodicarbonamide compounds, derivatives thereof and copolymers thereof. The separator according to claim 1 , wherein the organic particles are polyethylene wax. 9 . The separator according to claim 1 , wherein the first binder comprises a sulfonate compound, an acrylamide compound, a (meth)acrylic acid compound, an acrylonitrile compound, a derivative thereof, a copolymer thereof, a mixture thereof, or any combination thereof.

10. The separator of claim 1, wherein the first binder is at least one selected from the group consisting of poly(acrylic acid-co-acrylamide-co-2-acrylamido-2-methylpropanesulfonic acid) sodium salt, poly(acrylic acid acrylamide acrylamide sulfonic acid), and a salt of poly(acrylic acid acrylamide acrylamide sulfonic acid). 11 . The separator of claim 1 , wherein a total content of the particulate boehmite and the needle-shaped ceramic particles is in a range of 20 to 50 parts by weight based on 100 parts by weight of the organic particles. 12 . The separator of claim 1 , wherein a thickness of the first coating layer is in a range of 0.1 μm to 5.0 μm. 13 . The separator of claim 1 , wherein a thickness of each of the first adhesive layer and the second adhesive layer is in a range of 0.1 μm to 5 μm. 14 . The separator of claim 1 , wherein an average particle diameter of the particulate second binder in the first adhesive layer and the second adhesive layer is in the range of 100 nm to 800 nm.

15. The separator as claimed in claim 1, wherein the particulate second binder comprises at least one selected from the group consisting of acrylic resin, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, polymethyl methacrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, ethylene vinyl acetate copolymer, polyethylene oxide, cellulose acetate, butyl cellulose acetate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile styrene butadiene copolymer and polyimide.