CMP polishing pad with improved rate
By using a polymer matrix and hierarchically structured layered particles in a polishing pad for chemical mechanical polishing, combined with a slurry with positive surface charge, the problems of low removal rate and high defect rate in the existing technology are solved, and high efficiency is achieved. polishing process.
Patent Information
- Application Number
- CN202210341643.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-29
AI Technical Summary
Existing chemical mechanical polishing technology has a low removal rate in high-capacity multi-layer memory manufacturing, resulting in a long 3D NAND manufacturing process, and increasing the removal rate may increase the defect rate of the polished substrate.
Using a polishing pad comprising a polymer matrix and rate-enhancing layered particles, the layered particles being hydrogen phosphates or hydrogen arsenates of Group III-A or Group IV-A metals having a layered and lamellar structure, It is used for chemical mechanical polishing of substrates. During polishing, the pH of the slurry is controlled within the positive surface charge range.
The polishing rate is significantly increased while reducing the occurrence of polishing defects. Especially when using ceria-based slurries, the removal rate is increased by 10% to more than 50% and the defect rate is reduced by 10% to 50%.
Smart Images

Figure CN115139219B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates generally to polishing pads for chemical mechanical polishing of substrates, particularly including polishing using ceria-based slurries such as during pre-metal dielectric formation. Background Art
[0002] In the manufacture of integrated circuits and other electronic devices, multiple layers of conductive materials, semiconductive materials, and dielectric materials are deposited on or partially or selectively removed from the surface of a semiconductor wafer. Many deposition techniques can be used to deposit thin layers of conductive materials, semiconductive materials, and dielectric materials. In addition, in a damascene process, materials are deposited to fill the recessed areas produced by patterned etching of trenches and vias. Since the filling is conformal, this may result in irregular surface morphology. In addition, in order to avoid insufficient filling, additional materials can be deposited. Therefore, it is necessary to remove materials outside the recesses. Common deposition techniques in modern wafer processing include, in particular, physical vapor deposition (PVD) (also known as sputtering), chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), and electrochemical deposition (ECD). Common removal techniques include, in particular, wet etching and dry etching; isotropic etching and anisotropic etching.
[0003] As materials are sequentially deposited and removed, the topography of the substrate may become uneven or non-planar. Because subsequent semiconductor processing (such as lithography, metallization, etc.) requires the wafer to have a flat surface, the wafer needs to be planarized. Planarization is used to remove undesirable surface topography and surface defects, such as rough surfaces, agglomerated materials, lattice damage, scratches, and contaminated layers or materials.
[0004] Chemical mechanical planarization (also known as chemical mechanical polishing (CMP)) is a common technique for planarizing or polishing workpieces (such as semiconductor wafers) and removing excess material in a damascene process, a front-end of line (FEOL) process, or a back-end of line (BEOL) process. In conventional CMP, a wafer carrier or polishing head is mounted on a carrier assembly. The polishing head holds the wafer and positions the wafer to contact the polishing surface of a polishing pad, which is mounted on a table or platen within the CMP equipment. The carrier assembly provides a controllable pressure between the wafer and the polishing pad. At the same time, a slurry or other polishing medium is dispensed onto the polishing pad and drawn into the gap between the wafer and the polishing layer. To perform polishing, the polishing pad and the wafer are typically rotated relative to each other. As the polishing pad rotates under the wafer, the wafer passes over a typically annular polishing track or polishing area, in which the surface of the wafer directly faces the polishing layer. The surface of the wafer is polished and made flat by the chemical and mechanical action of the polishing surface and the polishing medium (e.g., slurry) on the surface.
[0005] The removal rate is important for the efficiency of the process of manufacturing electronic devices. For example, in a high-capacity multi-layer memory device (e.g., 3D NAND flash memory), the manufacturing process may include a multilayer stack of SiO2 and Si3N4 films stacked in an alternating manner in the form of a pyramidal staircase. Once completed, the stack is covered with a thick SiO2 capping layer. This must be flattened before the device structure is completed. The device capacity is proportional to the number of layers in the layered stack. Commercial devices typically use 32 or 64 layers, and the industry is rapidly moving to 128 layers. The thickness of each oxide / nitride pair in the stack is about 125nm. Therefore, the thickness of the stack increases directly with the number of layers (32 layers with a thickness of about 4,000nm, 64 layers with a thickness of about 8,000nm, and 128 layers with a thickness of about 16,000nm). The total amount of the covering dielectric to be removed can be about 1.5 times the thickness of the stack (e.g., up to about 24,000nm). Conventional dielectric CMP slurries have a removal rate of about 250 nm / min, resulting in undesirably long CMP process times, which can create bottlenecks in 3D NAND manufacturing processes. Much of the work to develop faster CMP processes has focused on process conditions, such as higher pressures, higher contact speeds, pad conditioning, slurry composition. However, increasing the removal rate cannot be at the expense of increasing the defectivity of the polished substrate. Therefore, methods to increase the removal rate, preferably without increasing defects, are desired. Summary of the invention
[0006] Disclosed herein is a polishing pad for chemical mechanical polishing having a polishing material comprising a polymer matrix material and layered particles for increasing the polishing rate, the layered particles comprising a hydrogen phosphate or hydrogen arsenate of a Group III-A or Group IV-A metal, preferably having the formula
[0007] M(HYO4)2n(H2O),
[0008] Wherein M is a metal ion of Group III-A or Group IV-A, preferably Zr +4 、Ti +4 or Ce +4 , the most preferred +4 , Y is P or As, preferably P, and n is 0, 1 or 2, preferably 1.
[0009] Also disclosed herein is a method comprising providing a substrate; providing a polishing pad as described above; providing a slurry between the polishing pad and the substrate; polishing the substrate with the pad and the slurry, preferably wherein the polishing is performed at a pH where the slurry contains particles having an overall positive surface charge in an aqueous medium such as deionized water. For the purposes of this specification, a positive surface charge means that the pH of the polishing slurry is below its isoelectric point. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is a schematic diagram showing the chemical structure of one example of a rate-enhancing layered particulate additive as disclosed herein. DETAILED DESCRIPTION
[0011] Disclosed herein is a polishing pad having a polishing portion comprising a polymer matrix and rate-enhancing lamellar particles.
[0012] The layered particles that increase the rate can be metal hydrogen phosphate or metal hydrogen arsenate. The layered particles that increase the rate can have a layered structure. Without wishing to be restricted, it is assumed that the layered structure can reduce the possibility of large particles that may scratch and form defects in the substrate to be polished. The layered particles that increase the rate can have a lamella structure (particularly a layered lamella structure). The average size of the particles in the main direction (i.e., length and / or width, substantially perpendicular to the thickness) can be at least 0.5 micron, or at least 1 micron, or at least 2 microns and can be at most 20 microns, or at most 10 microns, or at most 5 microns at the same time. The particles can have an aspect ratio (length or width: thickness) of 3 to 20 or 3 to 10.
[0013] The rate-enhancing lamellar particles may have a crystalline structure. Figure 1 An example of a molecular structure of such a layered particle is shown, showing zirconium as the metal and phosphate groups. Each layer can have a plane of metal ions bonded to (e.g., bridged by) hydrogen phosphate (or hydrogen arsenate) groups above and below the plane of the metal ions. The outer surface of the hydrogen phosphate (or hydrogen arsenate) bridged layer can be terminated by P-OH groups (or As-OH groups). The metal ion Zr is shown. +4 , which may be bound to phosphate or arsenate groups (phosphate groups are shown), preferably phosphate groups, on either side of the alternating or layered structure. Water may be bound to the hydroxyl groups. The metal ion may be a Group III-A or Group IV-A metal ion, such as a zirconium ion (e.g., Zr +4 ), titanium ions (such as Ti +4 ), or cerium ions (e.g. Ce +4 ).
[0014] The particles may have several layers of metal ions (e.g. Zr +4), typically in the form of metal oxides and associated phosphate groups (or arsenate groups). Above the isoelectric pH in aqueous solution (about 3 for zirconium hydrogen phosphate), the surface is highly negatively charged due to the large number of surface hydroxyl groups. These particles are also hydrophilic, but chemically inert and insoluble in water. These particles can be highly brittle, making it unlikely that large particles will produce scratch defects during polishing. In addition, these particles can break apart to form flakes that can improve polishing performance, such as by increasing removal rates.
[0015] The metal phosphate or metal arsenate may have the formula:
[0016] M(HYO4)2n(H2O),
[0017] Wherein M is a metal ion of Group III-A or Group IV-A, preferably Zr +4 、Ti +4 or Ce +4 , the most preferred +4 , Y is P or As, preferably P, and n is 0, 1 or 2, preferably 1.
[0018] The amount of rate-enhancing layered particles for use in the polishing portion of a pad as disclosed herein can be at least 0.1 weight percent, or at least 1 weight percent, or at least 2 weight percent, or at least 3 weight percent, or at least 5 weight percent and up to 20 weight percent, or up to 15 weight percent, or up to 10 weight percent based on the total weight of the polishing portion. The amount of rate-enhancing layered particles can be 0.1 to 20 volume percent, or 1 to 18 volume percent, or 2 to 15 volume percent based on the total volume of the polishing portion.
[0019] The polishing portion may include any polymer matrix material commonly used in polishing pads. The polishing portion may include thermoplastic or thermosetting polymers. Among the polymer materials that can be used in the base pad or the polishing portion, examples of polymers that can be used in the polishing portion include polycarbonate, polysulfone, nylon, epoxy resin, polyether, polyester, polystyrene, acrylic polymers, polymethyl methacrylate, polyvinyl chloride, polyvinyl fluoride, polyethylene, polypropylene, polybutadiene, polyethyleneimine, polyurethane, polyethersulfone, polyamide, polyetherimide, polyketone, epoxy, silicone, copolymers thereof (such as polyether-polyester copolymers), and combinations or blends thereof. The polymer may be polyurethane.
[0020] According to ASTM D412-16, the Young's modulus of the polished portion can be at least 2 MPa, at least 2.5 MPa, at least 5 MPa, at least 10 MPa, or at least 50 MPa, at most 900 MPa, at most 700 MPa, at most 600 MPa, at most 500 MPa, at most 400 MPa, at most 300 MPa, or at most 200 MPa. The polished portion can be opaque to the signal used for endpoint detection.
[0021] The polishing portion may also contain other particles. For example, such as, in particular, hollow microelements, in particular flexible hollow polymer microelements, such as microspheres. For example, a plurality of microelements may be uniformly dispersed throughout the polishing layer. A plurality of microelements may be only pores in the matrix (e.g., trapped bubbles), or may be hollow polymer materials, liquid-filled hollow polymer materials, water-soluble materials, or insoluble phase materials (e.g., mineral oil). A plurality of microelements provide porosity for the polishing element, for example, when the microelements are selected from trapped bubbles and hollow polymer materials uniformly distributed throughout the polishing layer. The microelements may have a weighted average diameter of at most 150 microns or at most 50 microns, while having a diameter of at least 10 microns. The weighted average diameter may be measured using laser diffraction, such as low-angle laser light scattering (LALLS). A plurality of microelements may include polymer microspheres having a shell wall of polyacrylonitrile or a polyacrylonitrile copolymer (e.g., from Akzo Nobel). Microspheres). A plurality of microelements may be incorporated into the polishing layer in an amount of 0 volume percent, or at least 5 volume percent, or at least 10 volume percent, at most 50 volume percent, at most 45 volume percent, at most 40 volume percent, or at most 35 volume percent. When the microelements provide porosity, the porosity of the polishing portion may be a porosity of 0 to 50, 5 to 45, or 10 to 35 volume percent. The volume percent of porosity may be determined by dividing the difference between the specific gravity of the unfilled polishing layer and the specific gravity of the polishing layer containing the microelements by the specific gravity of the unfilled polishing layer. Alternatively, the porosity percentage is determined by dividing the density of the polishing layer by the weighted average density of the unfilled portion of the polishing layer. Metal phosphates are particularly suitable for machining non-porous polishing pads. For example, metal phosphate particles can improve machining grooves from a vertical lathe operated with a fixed cutting tool or cutting grooves with a rotating tool.
[0022] The polished portion may have a g / cm 2 as measured according to ASTM D1622 (2014) of 0.4 to 1.15 or 0.7 to 1.0 g / cm 2. 3 density.
[0023] The polished portion may have a Shore D hardness of 28 to 75 as measured according to ASTM D2240 (2015).
[0024] The polishing portion can have an average thickness of 20 to 150 mils, 30 to 125 mils, 40 to 120 mils, or 50 to 100 mils (0.5-4, 0.7-3, 1-3, or 1.3-2.5 mm).
[0025] The polishing pad of the present invention optionally further comprises at least one additional layer bonded to the polishing layer. For example, the polishing pad may further comprise a compressible base layer adhered to the polishing layer. The compressible base layer preferably improves the conformability of the polishing layer to the surface of the substrate being polished. A base pad (also referred to as a sublayer or base layer) can be used below the polishing portion. The base pad can be a single layer or can include more than one layer. The top surface of the base pad can define a plane in an xy Cartesian coordinate system. For example, the polishing portion can be attached to the base pad by a mechanical fastener or by an adhesive. The base layer can have a thickness of at least 0.5 mm or at least 1 mm. The base layer can have a thickness of no more than 5 mm, no more than 3 mm, or no more than 2 mm.
[0026] The base pad or base layer may include any material known to be used as a base layer of a polishing pad. For example, the material may include a polymer, a blend of polymers, or a composite material of a polymer material and other materials, such as ceramic, glass, metal, or stone. Polymers and polymer composites may be used as base pads, particularly for top layers when more than one layer is used, because they are compatible with the material that may form the polishing portion. Examples of such composite materials include polymers filled with carbon or inorganic fillers, and fiber felts such as glass or carbon fibers impregnated with polymers. The base of the pad can be made of a material having one or more of the following properties: a Young's modulus of at least 2 MPa, at least 2.5 MPa, at least 5 MPa, at least 10 MPa, or at least 50 MPa, up to 900 MPa, up to 700 MPa, up to 600 MPa, up to 500 MPa, up to 400 MPa, up to 300 MPa, or up to 200 MPa, as determined, for example, by ASTM D412-16; a Poisson's ratio of at least 0.05, at least 0.08, or at least 0.1, up to 0.6, or up to 0.5, as determined, for example, by ASTM E132; a hardness of at least 0.4, at least 0.5, up to 1.7, up to 1.5, or up to 1.3 grams per cubic centimeter (g / cm 3 ) density.
[0027] Examples of such polymeric materials that can be used in the base pad or polishing portion include polycarbonate, polysulfone, nylon, epoxy resin, polyether, polyester, polystyrene, acrylic polymer, polymethyl methacrylate, polyvinyl chloride, polyvinyl fluoride, polyethylene, polypropylene, polybutadiene, polyethyleneimine, polyurethane, polyethersulfone, polyamide, polyetherimide, polyketone, epoxy, ethylene vinyl acetate (EVA or PEVA), ethylene propylene diene monomer rubber (EPDM rubber), silicone, copolymers thereof (such as polyether-polyester copolymers), or combinations or blends thereof.
[0028] The polymer may be a polyurethane. The polyurethane may be used alone or may be a matrix of carbon or inorganic fillers and fiber mats such as glass or carbon fibers.
[0029] For the purposes of this specification, "polyurethane" is a product derived from a difunctional or multifunctional isocyanate, such as polyether urea, polyisocyanurate, polyurethane, polyurea, polyurethane urea, copolymers thereof, and mixtures thereof. The CMP polishing pad can be manufactured by a method comprising providing an isocyanate-terminated urethane prepolymer; separately providing a curing agent component; and mixing the isocyanate-terminated urethane prepolymer and the curing agent component to form a combination, and then reacting the combination to form a product. The base pad or base layer can be formed by cutting the cast polyurethane cake into a desired thickness. Optionally, preheating the cake mold with IR radiation, induced current or direct current when casting the porous polyurethane matrix can reduce the variability of the product. Optionally, thermoplastic or thermosetting polymers can be used. The polymer can be a cross-linked thermosetting polymer.
[0030] When polyurethane is used in the base pad and / or the polishing layer, it can be the reaction product of a polyfunctional isocyanate and a polyol. For example, a polyisocyanate-terminated urethane prepolymer can be used. The polyfunctional isocyanate used to form the polishing layer of the chemical mechanical polishing pad of the present invention can be selected from the group consisting of: aliphatic polyfunctional isocyanates, aromatic polyfunctional isocyanates and mixtures thereof. For example, the polyfunctional isocyanate used to form the polishing layer of the chemical mechanical polishing pad of the present invention can be a diisocyanate selected from the group consisting of: 2,4 toluene diisocyanate; 2,6 toluene diisocyanate; 4,4' diphenylmethane diisocyanate; naphthalene 1,5 diisocyanate; toluidine diisocyanate; p-phenylene diisocyanate; xylene diisocyanate; isophorone diisocyanate; hexamethylene diisocyanate; 4,4' dicyclohexylmethane diisocyanate; cyclohexane diisocyanate; and mixtures thereof. The polyfunctional isocyanate may be an isocyanate-terminated urethane prepolymer formed by reacting a diisocyanate with a prepolymer polyol. The isocyanate-terminated urethane prepolymer may have 2 to 12 wt%, 2 to 10 wt%, 4-8 wt%, or 5 to 7 wt% of unreacted isocyanate (NCO) groups. The prepolymer polyol used to form the polyfunctional isocyanate-terminated urethane prepolymer may be selected from the group consisting of diols, polyols, polyol diols, copolymers thereof, and mixtures thereof. For example, the prepolymer polyol can be selected from the group consisting of: polyether polyols (e.g., poly(oxytetramethylene) glycol, poly(oxypropylene) glycol, and mixtures thereof); polycarbonate polyols; polyester polyols; polycaprolactone polyols; mixtures thereof; and mixtures thereof with one or more low molecular weight polyols selected from the group consisting of: ethylene glycol; 1,2-propylene glycol; 1,3-propylene glycol; 1,2-butylene glycol; 1,3-butylene glycol; 2-methyl-1,3-propylene glycol; 1,4-butylene glycol; neopentyl glycol; 1,5-pentanediol; 3-methyl-1,5-pentanediol; 1,6-hexanediol; diethylene glycol; dipropylene glycol; and tripropylene glycol. For example, the prepolymer polyol can be selected from the group consisting of: polytetramethylene ether glycol (PTMEG); ester-based polyols (such as ethylene glycol adipate, butylene adipate); polypropylene ether glycol (PPG); polycaprolactone polyols; copolymers thereof; and mixtures thereof. For example, the prepolymer polyol can be selected from the group consisting of: PTMEG and PPG. When the prepolymer polyol is PTMEG, the unreacted isocyanate (NCO) concentration of the isocyanate-terminated urethane prepolymer can be 4 to 12 wt% (more preferably 6 to 10 wt%; most preferably 8 to 10 wt%). Examples of commercially available PTMEG-based isocyanate-terminated urethane prepolymers include Prepolymers (available from COIM USA, Inc., such as PET 80A, PET 85A, PET 90A, PET 93A, PET 95A, PET 60D, PET 70D, PET 75D); prepolymers (available from Chemtura, such as LF 800A, LF 900A, LF 910A, LF 930A, LF 931A, LF 939A, LF 950A, LF952A, LF 600D, LF 601D, LF 650D, LF 667, LF 700D, LF750D, LF751D, LF752D, LF753D, and L325); Prepolymers (available from Anderson Development Company, such as 70APLF, 80APLF, 85APLF, 90APLF, 95APLF, 60DPLF, 70APLF, 75APLF). When the prepolymer polyol is PPG, the unreacted isocyanate (NCO) concentration of the isocyanate-terminated urethane prepolymer can be 3 to 9 wt% (more preferably 4 to 8 wt%; most preferably 5 to 6 wt%). Examples of commercially available PPG-based isocyanate-terminated urethane prepolymers include Prepolymer (available from American Ke Yi Company, such as PPT 80A, PPT 90A, PPT95A, PPT 65D, PPT 75D); prepolymers (available from Lanxess, such as LFG 963A, LFG 964A, LFG 740D); and Prepolymer (available from Anderson Development Company, such as 8000APLF, 9500APLF, 6500DPLF, 7501DPLF). The isocyanate-terminated urethane prepolymer can be a low-free isocyanate-terminated urethane prepolymer having a free toluene diisocyanate (TDI) monomer content of less than 0.1 wt%. Non-TDI-based isocyanate-terminated urethane prepolymers can also be used. For example, isocyanate-terminated urethane prepolymers include those formed by reacting 4,4' diphenylmethane diisocyanate (MDI) with a polyol such as polytetramethylene glycol (PTMEG) (wherein optional diols such as 1,4-butanediol (BDO) are acceptable). When such isocyanate-terminated urethane prepolymers are used, the concentration of unreacted isocyanate (NCO) is preferably 3 to 10 wt% (more preferably 4 to 10 wt%, most preferably 5 to 10 wt%). Examples of commercially available isocyanate-terminated urethane prepolymers in this category include Prepolymer (available from American Ke Yi Company, such as 27 85A, 27 90A, 27 95A); Prepolymers (available from Anderson Development as IE75AP, IE80AP, IE 85AP, IE90AP, IE95AP, IE98AP); and Prepolymer (available from Chemtura, such as B625, B635, B821).
[0031] The polishing pad of the present invention in its final form may include a texture of one or more sizes combined on its upper surface. These may be classified as macrotextures or microtextures according to their size. Conventional types of macrotextures for controlling fluid dynamic response and / or slurry transmission for CMP include, but are not limited to, grooves of many configurations and designs, such as annular, radial, and cross-line. These may be formed into uniform sheets by machining processes, or may be formed directly on the pad surface by a net-shape molding process. Common types of microtextures are finer-scale features that produce a large number of surface roughnesses, which are points of contact with the substrate wafer being polished. Common types of microtextures include, but are not limited to, textures formed by grinding with hard particle arrays such as diamond (commonly referred to as pad conditioning) before, during, or after use, as well as microtextures formed during pad manufacturing.
[0032] The polishing pad of the present invention can be adapted to engage with a platen of a chemical mechanical polisher. The polishing pad can be secured to the platen of the polisher. The polishing pad can be secured to the platen using at least one of a pressure sensitive adhesive and a vacuum.
[0033] The CMP pads of the present invention can be made by a variety of methods that are compatible with the properties of the pad polymer used. These methods include mixing the above ingredients and pouring them into a mold, annealing, and cutting into sheets of desired thickness. Alternatively, they can be made in a more precise net shape form. Manufacturing methods include: 1. Thermoset injection molding (commonly known as "reaction injection molding" or "RIM"); 2. Thermoplastic or thermoset injection blow molding; 3. Compression molding; or 4. Any similar type of method in which a flowable material is placed and solidified to produce at least a portion of the macrotexture or microtexture of the pad. In the example of forming the polishing pad: 1. The flowable material is forced into or onto a structure or substrate; 2. The structure or substrate can impart surface texture to the material as the material solidifies, and 3. The structure or substrate is then separated from the solidified material.
[0034] method
[0035] Polishing pads as disclosed herein can be used to polish substrates. For example, the polishing method may include providing a substrate to be polished, and then polishing using the pad disclosed herein. The substrate may be any substrate that is desired to be polished and / or planarized. Examples of such substrates include magnetic substrates, optical substrates, and semiconductor substrates. A specific example is a pre-metal dielectric stack. The specific material to be polished on the substrate may be a silicon oxide layer. The method may be part of a front-end or back-end processing of an integrated circuit. For example, the process may be used to remove undesirable surface topography and surface defects, such as rough surfaces, agglomerated materials, lattice damage, scratches, and contaminated layers or materials. In addition, in a damascene process, material is deposited to fill a recessed area produced by one or more steps in lithography, patterned etching, and metallization. Some steps may be imprecise, such as overfilling a recess. The method disclosed herein may be used to remove material outside the recess. The process may be chemical mechanical planarization or chemical mechanical polishing, both of which may be referred to as CMP. The bracket may hold the substrate to be polished, such as a semiconductor wafer (with or without layers formed by lithography and metallization), in contact with the polishing element of the polishing pad. A slurry or other polishing medium may be dispensed into the gap between the substrate and the polishing pad. The polishing pad and substrate are moved relative to each other, such as rotated. The polishing pad is typically located below the substrate to be polished. The polishing pad may be rotated. The substrate to be polished may also be moved, such as on a polishing track such as a ring. This relative movement causes the polishing pad to approach and contact the surface of the substrate.
[0036] The pads as disclosed herein can be used with any slurry. The inventors have discovered that using a pad as disclosed herein with a slurry having positively charged (or having a positive surface charge) particles under polishing conditions can provide a significant increase in removal rate. Without wishing to be limited, it is hypothesized that the rate-enhancing layered particles can provide a relatively high concentration of anionic hydroxyl sites to the pad surface, to which the positively charged particles present during polishing can bind.
[0037] The pressure of the platen can be 1 to 5, 1.5 to 4.5, or 2 to 4 pounds per square inch (psi) (about 6-35, 10-30, or 13 to 28 kilopascals (KPa)). The speed of the platen can be about 40 to 150, or 50-130 rpm. The amount of slurry added can be, for example, 50 to 500 ml / min. The pH of the slurry during polishing can be up to 7, or up to 6.8 and as low as 2, 2.5, or 3.
[0038] For example, in slurries based on ceria, the benefits of increased removal rate are particularly evident. In slurries based on ceria, CeO2 can make particles have a positive charge (or positive surface charge) at a pH lower than about 6.5, for example, such slurries based on ceria can include at least 0.01 weight percent, or at least 0.1 weight percent ceria particles based on the total weight of the slurry, up to 20 weight percents, or up to 15 weight percents, or up to 10 weight percents, or up to 5 weight percents, or up to 2 weight percent ceria particles. Slurries based on ceria can only include ceria as the only particle, or can also include additional other particles. These other particles can be, for example, other particles with positive (surface) charge at the pH for polishing. These other particles can be, for example, silica particles or alumina particles, preferably, they have positive surface charge at the pH for polishing. In some slurries based on silica, particularly in those with particles with positive (surface) charge at the pH for polishing, the increase in removal rate can also be observed.
[0039] For example, the method may include: providing a chemical mechanical polishing apparatus having a platen or a bracket assembly; providing at least one substrate to be polished; providing a chemical mechanical polishing pad as disclosed herein; mounting the chemical mechanical polishing pad on the platen; optionally, providing a polishing medium (e.g., a slurry containing an abrasive and / or a reactive liquid composition containing a non-abrasive) at an interface between the polishing portion of the chemical mechanical polishing pad and the substrate; forming a dynamic contact between the polishing portion of the polishing pad and the substrate, wherein at least some material is removed from the substrate. The bracket assembly may provide a controllable pressure between the substrate being polished (e.g., a wafer) and the polishing pad. The polishing medium may be dispensed onto the polishing pad and drawn into the gap between the wafer and the polishing layer. The polishing medium may contain water, a pH adjuster, and optionally (but not limited to) one or more of the following: abrasive particles, an oxidizing agent, an inhibitor, an antimicrobial agent, a soluble polymer, and a salt. The abrasive particles may be oxides, metals, ceramics, or other suitably hard materials. Typical abrasive particles are colloidal silica, fumed silica, ceria, and aluminum oxide. The polishing pad and substrate can rotate relative to each other. As the polishing pad rotates below the substrate, the substrate can sweep a typically annular polishing track or polishing area, wherein the surface of the wafer directly faces the polishing portion of the polishing pad. The surface of the wafer is polished and made flat by the chemical and mechanical action of the polishing layer and the polishing medium on the surface. Optionally, the polishing surface of the polishing pad can be trimmed with an abrasive dresser before polishing begins.
[0040] The use of pads containing rate-enhancing layered particles as described herein can be particularly effective in increasing removal rates while avoiding defects. For example, using a slurry with positively charged particles (e.g., a ceria-based slurry having a pH of up to 7, or up to 6.5, or up to 6), removal rates (e.g., tetraethyl orthosilicate (TEOS) removal rates) can be increased by 10 percent or more, 15 percent or more, or 20 percent or more, while defectivity can be reduced by 10 percent or more, 30 percent or more, or 50 percent or more, compared to polishing an equivalent pad without rate-enhancing layered particles (e.g., ZHP).
[0041] Optionally, the pad may include a window for endpoint detection. In this case, the provided chemical mechanical polishing apparatus may further include a signal source (e.g., a light source) and a signal detector (e.g., a light sensor (preferably a multi-sensor spectrometer)). In this case, the method may further include: determining the polishing endpoint by transmitting a signal (e.g., light from a light source) through the window and analyzing a signal (e.g., light) reflected from the surface of the substrate through the endpoint detection window and incident on a sensor (e.g., a light sensor). The substrate may have a metal or metallized surface, such as a surface comprising copper or tungsten. The substrate may be a magnetic substrate, an optical substrate, and a semiconductor substrate.
[0042] Examples
[0043] Material
[0044] PTMEG polytetramethylene ether glycol blend.
[0045] Prepolymer H having 8.95 to 9.25 wt% NCO 12 MDI / TDI-PTMEG blend. TDI (toluene diisocyanate) from Dow, trade name Voranate T-80 TM .
[0046] H 12 MDI (alicyclic diisocyanate).
[0047] MBOCA (4,4'-methylenebis(2-chloroaniline).
[0048] Zirconium hydrogen phosphate powder (ZHP, flakes with an average particle size of 1-6 microns).
[0049] Expancel from Nouryon (formerly Akzo Nobel) TM Microporous particles 551DE40d42.
[0050] Synthesis of prepolymer
[0051] The prepolymer can be synthesized in batches, such as 200-1000 grams. The PTMEG components are blended together to form a polyol mixture. Before adding to the polyol mixture, TDI and H 12 MDI was mixed in a ratio of 80:20. Sufficient isocyanate mixture was then added to the polyol mixture to achieve the desired NCO weight percentage. The entire mixture was mixed again and then placed in a preheated oven at 65°C for 4 hours before use. All samples were used on the day of synthesis. Alternatively, prepolymer H can be used directly 12 MDI / TDI-PTMEG blends are used to make pads.
[0052] Pad production
[0053] The synthesized prepolymer or L-325 was heated to 65°C. Mboca was pre-weighed and melted in an oven at 95°C. ZHP was added to the prepolymer to produce different levels of lamellar particles. ZHP and prepolymer were mechanically mixed. Expancel was then TM 551DE40d42 microporous particles are added to the prepolymer-ZHP blend. The prepolymer, ZHP and Expancel hollow microsphere blends are thoroughly mixed and degassed using vacuum. All samples have enough Expancel added to reach the desired final density. After degassing, MBOCA is added to the prepolymer, ZHP and Expancel blends and mixed thoroughly. The sample is then poured onto a hot plate and scraped using a polytetrafluoroethylene (PTFE) coated rod with an interval set to 175 mils. The plate is then transferred to an oven and heated to 104°C and kept at this temperature for 16 hours. The scraped film is then demoulded, flattened and punched into a diameter of 22 inches (55.9 cm) and used to prepare a laminate pad for polishing. All pads were 20 inch (50.8 cm) diameter and 80 mil (0.2 cm) thick top pads, circular (30 mil deep, 20 mil wide and 120 mil pitch or 0.76 mm deep, 0.51 mm wide and 3 mm pitch) grooves, pressure sensitive adhesive, Suba IV subpads, and CR-II press plate adhesive. Control pads were made using a similar process without the ZHP additive. Each material group was also made into panels for characterization testing with and without Expancel filler for characterization testing.
[0054] Example 1
[0055] According to the above procedure, samples of polyurethane formulations were prepared with different levels of ZHP addition. The material properties of the three materials are summarized in Table 1. While the hardness or elastic modulus (G') remained within the operating range, the tensile strength decreased directly with the addition amount. The functional limit of elongation and toughness reduction without undesirable effects on the polishing process is estimated to occur at addition amounts of up to about 15 weight percent by weight.
[0056]
[0057] Table 1
[0058] Example 2
[0059] Pads with 10 weight percent ZHP and pads without ZHP were used to polish TEOS wafers using a commercially available CeO2-based slurry (Asahi CES333). The slurry was prepared using the manufacturer's instructions. The slurry pH was 5.5. Based on previous data, the pH used was well below the isoelectric pH of the particles used so that the particles were at least somewhat positively charged. Each pad was used to polish a 200mm TEOS wafer using a single set of process conditions. The polishing conditions used for each test were a platen speed of 93rpm, a wafer carriage speed of 87rpm, and a slurry flow rate of 200ml / min. The polishing equipment used was a Mirra CMP polishing tool from Applied Materials. Compared to the removal rate of 1604 angstroms / minute for pads without ZHP, a significant increase in polishing rate was observed for the ZHP-10 pad with a removal rate of 1930 angstroms / minute. A reduction in polishing defects was also observed, with an average of 62 scratch defects per wafer for the pad without ZHP and only 15 for the pad with 10 weight percent ZHP. These results indicate that incorporating the hydrogen phosphate layered particles of the present invention into the pads of the present invention is effective in increasing the rate when polishing is performed at a pH where the particles are at least partially cationic.
[0060] Example 3
[0061] Three commercially available CeO2-based slurries (Hitachi H8005, Versum STI2100F and AsahiCES333) were used to polish TEOS wafers with pads having 10 weight percent ZHP and pads without ZHP. All slurries were prepared using the manufacturer's instructions. The pH during use was 5.5. Based on previous data, the pH used was well below the isoelectric pH of the particles used, so that the particles should have at least some positive charge. Each pad was used to polish 200mm TEOS wafers using a single set of process conditions. The polishing conditions used for each test were a platen speed of 93rpm, a wafer carriage speed of 87rpm, and a slurry flow rate of 150ml / min. The polishing equipment used was a Mirra CMP polishing tool from Applied Materials.
[0062] As shown in Table 2, for all slurries tested, significant improvements in polishing rate were observed for the pads of the present invention relative to the reference without ZHP. These results indicate that for a variety of ceria slurry formulations, when the pH criteria described herein are met, the introduction of hydrogen phosphate additives into the pads of the present invention is effective in increasing the rate.
[0063]
[0064] Table 2
[0065] Furthermore, the silicon nitride selectivity of the three slurries increased by an average of 12% for the ZHP-10 pad compared to the control pad without ZHP.
[0066] Example 4
[0067] Pads with 10 weight percent ZHP and no ZHP were used to polish TEOS wafers using a commercially available CeO2-based slurry (Asahi CES333) and a commercial SiO2-based slurry (Dow K1730). The slurries were prepared using the manufacturer's instructions. The pH of the CeO2-based slurry was 5.5 and had a solid content of 1 wt% when used. The SiO2 slurry had a pH of 10.5 (above the isoelectric pH of the slurry so that the particles are not positively charged) and had a solid content of 16 wt% when used. Each of the four slurry / pad combinations was polished at two different polishing speeds at different downforces ranging from 1.5 to 4 psi. Multiple TEOS wafers were polished for each of the combinations, and the coefficient of friction during polishing and the removal rate were measured.
[0068] Additionally, this experiment can be used to determine the Preston coefficient, k, using the pressure, rate, and speed data by dividing the polishing rate for each sample by the product of the pressure and speed tested. Since the two slurries used had very different solids contents, an additional measure of polishing efficiency can be determined by dividing k by the percent solids for each polished sample. The polishing efficiency for the SiO2-based slurry was the same at 0.5 for both the pad with and without the ZHP. The polishing efficiency for the CeO2-based slurry was 4.9 for the pad without the ZHP, and 6.5 for the pad with the ZHP.
[0069] The coefficient of friction (COF) data calculated from the motor torque and slurry temperature of the polishing station provides additional insight into the improvements achieved by the pads of the present invention. As can be seen in Table 3, all CeO2-based slurry data show significantly higher COF than the SiO2-based slurry data. In addition, the COF of the pads including ZHP is significantly higher than the pads not including ZHP. This demonstrates that there is a higher concentration of CeO2 particles on the pad surface of the pads including ZHP due to the presence of the metal hydrogen phosphate particles. As with the rate, this effect is not observed when using negatively charged particle slurries (e.g., negatively charged SiO2 particles).
[0070]
[0071] Table 3
[0072] Example 5
[0073] Polishing was performed with pads without ZHP and pads with 10 wt% ZHP and a silica-based slurry at a pH above its isopotential such that the particles have a negative charge. The removal rates of TEOS for pads containing ZHP were roughly the same and differed by up to 1.7 percent on average compared to pads without ZHP. The SiN selectivity of pads without ZHP was twice as high as that of pads with ZHP. In addition, pads with ZHP showed significantly more defects (scratches and scratches).
[0074] Example 6
[0075] Polishing was performed with pads without ZHP and pads with 10 wt% ZHP and a silica-based slurry at a pH below its isopotential such that the particles have a positive charge. The TEOS removal rate of the pad with ZHP was 18 percent higher than that of the pad without ZHP ( Relative to ).
[0076] The present disclosure further encompasses the following aspects:
[0077] Aspect 1: A polishing pad for chemical mechanical polishing having a polishing portion comprising a polymer matrix and rate-enhancing layered particles comprising a phosphate or arsenate of a Group III-A or Group IV-A metal.
[0078] Aspect 2: A polishing pad as described in Aspect 1, wherein these rate-enhancing layered particles include a material having the formula M(HYO4)2n(H2O), wherein M is a Group III-A or Group IV-A metal ion, Y is P or As, preferably P, and n is 0, 1 or 2.
[0079] Aspect 3: The polishing pad according to aspect 2, wherein M is Zr +4 、Ti +4 or Ce +4 , Y is P, and n is 1.
[0080] Aspect 4: The polishing pad of any of the preceding aspects, wherein the rate-enhancing lamellar particles have a layered crystal structure.
[0081] Aspect 5: The polishing pad of any of the preceding aspects, wherein the rate-enhancing lamellar particles are zirconium hydrogen phosphate.
[0082] Aspect 6: A polishing pad as described in any of the preceding aspects, wherein the polymer matrix comprises polyurethane, polyolefin, polyethylene, polypropylene, polyester, polyether, nylon, polyvinyl alcohol, polyvinyl acetate, polyacrylate, polycarbonate, polyacrylamide, polyamide, polyimide, polyetherketone, polysulfone and fluoropolymer, copolymer thereof, or mixture thereof, and preferably comprises polyurethane.
[0083] Aspect 7: A polishing pad as described in any of the preceding aspects, wherein the amount of these rate-enhancing layered particles is at least 0.1 weight percent, preferably at least 1 weight percent, more preferably at least 2 weight percent, even more preferably at least 3 weight percent and most preferably at least 5 weight percent and at most 20 weight percent, preferably at most 15 weight percent, and more preferably at most 10 weight percent based on the total weight of the polishing portion.
[0084] Aspect 8: The polishing pad of any of the preceding aspects, wherein the amount of the rate-enhancing laminar particles can be 0.1 to 20 volume percent, or 1 to 18 volume percent, or 2 to 15 volume percent based on the total volume of the polishing layer.
[0085] Aspect 9: The polishing pad of any of the preceding aspects, wherein the rate-enhancing lamellar particles are in the form of flakes.
[0086] Aspect 10: A polishing pad as described in any of the preceding aspects, wherein the average size of the flakes in the direction perpendicular (or substantially perpendicular) to the thickness is at least 0.5 microns, preferably at least 1 micron, more preferably at least 2 microns, and at the same time can be at most 20 microns, preferably at most 10 microns, more preferably at most 7 microns, or most preferably at most 5 microns.
[0087] Aspect 11: The polishing pad of aspect 9 or 10, wherein the flakes have an aspect ratio of 3 to 20, preferably 3 to 10.
[0088] Aspect 12: The polishing pad of any of the preceding aspects, wherein the polishing portion further comprises one or more microelements.
[0089] Aspect 13: The polishing pad of aspect 12, wherein the microelements provide porosity in the polishing portion.
[0090] Aspect 14: The polishing pad of aspect 13, wherein the one or more microelements comprise hollow microelements.
[0091] Aspect 15: The polishing pad of aspect 14, wherein the volume percent amount of the one or more hollow microelements is 0 to 50 volume percent, preferably 5 to 45 volume percent, and more preferably 10 to 35 volume percent.
[0092] Aspect 16: The polishing pad of aspect 14 or 15, wherein the microelements have a weight average diameter of at most 150 microns or at most 50 microns as measured by laser diffraction, while having a diameter of at least 10 microns.
[0093] Aspect 17: The polishing pad of any of the preceding aspects, wherein the polishing portion has a g / cm 2 of 0.4 to 1.15, preferably 0.7 to 1.0 g / cm 2 as measured according to ASTM D1622 (2014). 3 density.
[0094] Aspect 18: The polishing pad of any of the preceding aspects, wherein the polishing portion has a Shore D hardness of 28 to 75 as measured according to ASTM D2240 (2015).
[0095] Aspect 19: The polishing pad of any of the preceding aspects, wherein the polishing portion has an average thickness of 0.5-4 mm, preferably 0.7-3 mm, more preferably 1-3 mm, and still more preferably 1.3-2.5 mm.
[0096] Aspect 20: The polishing pad of any of the preceding aspects, further comprising at least one additional layer coupled to the polishing layer.
[0097] Aspect 21: The polishing pad of aspect 20, wherein the at least one additional layer comprises a base layer.
[0098] Aspect 22: The polishing pad of aspect 20 or 21, wherein the base layer is adhered to the back side of the polishing portion.
[0099] Aspect 23: The polishing pad of any of Aspects 20-22, wherein the base layer is compressible.
[0100] Aspect 24: The polishing pad as described in any of the preceding aspects, wherein the volume porosity in the polishing portion may be 0 to 50 percent, preferably 5 to 45 percent, and more preferably 10 to 35 percent.
[0101] Aspect 25: The polishing pad of any of the preceding aspects, wherein the polymer matrix comprises polyurethane.
[0102] Aspect 26: A method comprising providing a substrate; providing a polishing pad as described in any of Aspects 1-25; providing a slurry between the polishing pad and the substrate; and polishing the substrate with the pad and the slurry.
[0103] Aspect 27: The method of aspect 26, wherein the slurry comprises particles and wherein the polishing is performed at a pH where at least a portion of the particles have a positive charge or a positive surface charge.
[0104] Aspect 28: The method of aspect 26 or 27, wherein the slurry comprises cerium oxide particles.
[0105] Aspect 29: A method as described in Aspect 28, wherein the slurry contains at least 0.01 weight percent, preferably at least 0.1 weight percent, at most 20 weight percent, preferably at most 10 weight percent, and more preferably at most 5 weight percent of cerium dioxide particles based on the total weight of the slurry.
[0106] Aspect 30: The method of any of Aspects 26-29, wherein the slurry comprises silicon oxide particles.
[0107] Aspect 31: The method of any of Aspects 26-30, wherein the polishing pad is on a press plate and the pressure of the press plate is 6-35, preferably 10-30 kilopascals (kPa).
[0108] Aspect 32: The method according to aspect 31, wherein the speed of the press plate is 40 to 100, preferably 50-90 rpm.
[0109] Aspect 33: The method of any of Aspects 26-32, wherein the pH of the slurry during polishing is 2-7, preferably 2.5-6.8.
[0110] Compositions, methods and articles may alternatively comprise, consist of or consist essentially of any suitable material, step or component disclosed herein. In addition or alternatively, compositions, methods and articles may be formulated to be free of or essentially free of any material (or substance), step or component that is not necessary to achieve the function or purpose of these compositions, methods and articles.
[0111] All ranges disclosed herein include endpoints, and endpoints can be combined independently of each other (e.g., the range of "up to 25 wt.%, or more specifically 5 wt.% to 20 wt.%" includes endpoints and all intermediate values in the range of "5 wt.% to 25 wt.%, etc.). In addition, the upper and lower limits can be combined to form a range (e.g., "at least 1 or at least 2 weight percents" and "up to 10 or 5 weight percents" can be combined into a range of "1 to 10 weight percents", or "1 to 5 weight percents", or "2 to 10 weight percents", or "2 to 5 weight percents"). "Combination" includes blends, mixtures, alloys, reaction products, etc. The terms "first", "second" and similar terms do not indicate any order, quantity, or importance, but are used to distinguish one element from another. The terms "a / an" and "said" do not represent a limit on quantity, and unless otherwise indicated herein or clearly contradictory to the context, are interpreted as including both the singular and the plural. Unless otherwise expressly indicated, "or" means "and / or". References throughout this specification to "some embodiments," "one embodiment," etc. mean that a particular element described with respect to that embodiment is included in at least one embodiment described herein, and may or may not be present in other embodiments. Furthermore, it will be appreciated that the described elements may be combined in any suitable manner in the various embodiments. "Combinations thereof" are open ended and include any combination comprising at least one of the listed components or characteristics, optionally together with unlisted similar or equivalent components or characteristics.
[0112] Unless stated to the contrary herein, all test standards are the most current standards in effect as of the filing date of the present application or, if priority is claimed, as of the filing date of the earliest priority application in which the test standards appear.
Claims
1. A polishing pad for chemical mechanical polishing having a polishing portion comprising a polymer matrix and layered particles for increasing the polishing rate, the layered particles comprising a material having the formula M(HYO4)2n(H2O), wherein M is Zr +4 、Ti +4 or Ce +4 , Y is P or As, and n is 0, 1 or 2, wherein, The lamellar particles have an alternating crystal structure that is broken into thin sheets.
2. The polishing pad according to claim 1, wherein The layered particles are zirconium hydrogen phosphate particles.
3. The polishing pad according to claim 1, wherein The polymer matrix includes polyurethane, polyolefin, polyethylene, polypropylene, polyester, polyether, nylon, polyvinyl alcohol, polyvinyl acetate, polyacrylate, polycarbonate, polyacrylamide, polyamide, polyimide, polyetherketone, polysulfone and fluoropolymer, copolymers thereof, or mixtures thereof.
4. The polishing pad according to claim 1, wherein the polishing portion comprises layered zirconium hydrogen phosphate particles for increasing the polishing rate, the amount of the layered particles being 0.1 to 20 weight percent based on the total weight of the polishing layer, wherein The lamellar particles are in the form of flakes having an average length of 0.5 to 20 microns.
Citation Information
Patent Citations
Structured fixed abrasive articles including surface treated nano-ceria filler, and method for making and using the same
CN102356139A
Tungsten-processing slurry with cationic surfactant
CN108350319A
Ceramic castable nanomaterials
US20040043204A1