A two-dimensional confined catalyst with a transition metal-based organic-inorganic metal framework structure and its preparation method and application

By forming transition metal-based MOFs materials on graphite sheets, the problem of insufficient MOF catalyst activity is solved, and efficient electrocatalytic oxygen evolution performance and stability are achieved, which is suitable for industrial production.

CN115198306BActive Publication Date: 2024-10-25QUZHOU RES INST OF ZHEJIANG UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210592961.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-27
Publication Date
2024-10-25
Estimated Expiration
2042-05-27

AI Technical Summary

Technical Problem

Existing MOF system catalysts suffer from insufficient catalytic activity, especially in electrocatalytic oxygen evolution reactions. Low conductivity and micropore size limit the effective utilization of active centers.

Method used

The graphite sheets are opened through the electrochemical intercalation method, and organic ligand intercalation and transition metal salt soaking reactions are performed on them to form transition metal-based MOFs materials, which are confined in the graphite sheets to delay or prevent catalyst loss. to shorten the mass transfer distance.

Benefits of technology

It achieves high electrochemical performance and stability of the catalyst, effectively replaces traditional precious metal catalysts, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115198306B_ABST
    Figure CN115198306B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of confined catalysis, and discloses a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure, a preparation method and an application thereof. The preparation method comprises the following steps: step 1, electrochemically intercalating a graphite sheet in an electrolyte to obtain a graphite sheet with micro-separation between layers; step 2, placing the graphite sheet obtained in step 1 in an organic ligand salt solution containing a carboxylic acid group for further electrochemical intercalation to obtain a graphite sheet with organic ligand intercalation; step 3, placing the graphite sheet obtained in step 2 in a transition metal salt solution for immersion reaction, taking out the graphite sheet for washing and drying to obtain the two-dimensional confined catalyst, wherein a transition metal-based MOFs material is confined between layers of the graphite sheet, has excellent electrocatalytic activity for oxygen evolution reaction at the electrolysis water anode under alkaline conditions, and still has good stability under long-term operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of confined catalysis technology, and in particular to a two-dimensional confined catalyst with a transition metal-based organic-inorganic metal framework structure, and a preparation method and application thereof. Background Art

[0002] As a zero-carbon emission energy carrier, hydrogen energy is considered to be the new energy with the greatest practical application potential and has received widespread attention. Among the many hydrogen production pathways, the electrochemically driven water splitting method to produce hydrogen and oxygen can efficiently and directly convert electrical energy into hydrogen energy. The technical process is simple and environmentally friendly, and it is easy to achieve the immediate production and use of hydrogen. It is currently the energy conversion method with the most practical application potential and an important part of my country's energy conversion strategy. The full water splitting reaction can be divided into two half reactions, namely the hydrogen evolution reaction occurring at the cathode and the oxygen evolution reaction occurring at the anode. Compared with the hydrogen evolution reaction, the oxygen evolution reaction involves a kinetically slow four-electron and four-proton transfer process, which requires overcoming a higher energy barrier to destroy the OH bond, and is a key step in the water splitting reaction.

[0003] So far, commercial water electrolysis oxygen evolution catalysts are still mainly iridium black and iridium oxide, which are expensive and scarce, resulting in a large amount of oxygen evolution catalyst loading in the electrode, high cost, and difficulty in large-scale application. In recent years, metal organic frameworks (MOFs) based on non-precious transition metals have attracted more and more attention due to their characteristics of both homogeneous and heterogeneous catalysts, and have gradually become a type of oxygen evolution reaction catalyst with application prospects.

[0004] For example, CN113430562A discloses an iron boride-based metal organic framework nanocatalyst. This method uses iron foam as the iron source for preparing the catalyst, accelerates the release of iron in the foam iron through hydrochloric acid corrosion, and prepares Fe-MOFs through hydrothermal reaction with ligands. Fe-MOFs can effectively control the internal void environment and pore size, promote the effective entry of reaction molecules, and thus enhance the catalytic activity.

[0005] For example, CN113073350A discloses an iron-based MOFs oxygen evolution electrocatalyst with a high active crystal face ratio. The method first prepares an N,N-dimethylformamide mixed solution at a molar ratio of iron ions and fumaric acid of 1:64-128, then performs a solvent thermal reaction at a certain reaction temperature, and obtains an iron-based MOFs oxygen evolution electrocatalyst after washing and drying. The in-situ synthesized active crystal face exposure ratio is high, so that the catalyst has excellent catalytic activity.

[0006] However, although the MOF system has abundant metal centers, its low conductivity and micropore size limit the effective utilization of active centers. Summary of the invention

[0007] In view of the problem of insufficient catalytic activity of MOF system catalysts in the prior art, the present invention provides a method for confining MOFs materials in graphite sheets to prepare a two-dimensional confined catalyst. The catalyst is applied to the electrocatalytic hydrogen evolution reaction and has excellent electrochemical performance and stability.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure, characterized in that it comprises the steps of:

[0010] Step 1, electrochemically intercalating a graphite sheet in an electrolyte to obtain a graphite sheet with micro-separation between layers;

[0011] Step 2, placing the graphite sheet obtained in step 1 in a solution of an organic ligand salt containing a carboxylic acid group for further electrochemical intercalation to obtain an organic ligand intercalated graphite sheet;

[0012] Step 3, placing the graphite sheet obtained in step 2 in a transition metal salt solution for immersion reaction, taking out the graphite sheet, washing, and drying to obtain the transition metal-based organic-inorganic metal framework structured two-dimensional confined catalyst.

[0013] The present invention first opens the tight graphite sheets through electrochemical intercalation, then intercalates the organic ligands into the graphite sheets, realizes material self-assembly through impregnation, reacts the inorganic transition metal salts with the organic ligands, and finally obtains the transition metal-based MOFs material confined in the graphite sheets. This method confines the transition metal-based MOFs material in the graphite sheets, delays or prevents the deactivation of the catalyst through the confinement effect, and greatly reduces the mass transfer distance and time, and is applied to the electrocatalytic oxygen evolution reaction under alkaline conditions, and has good electrochemical performance and stability.

[0014] In step 1, the electrolyte includes any one of dilute sulfuric acid solution, perchloric acid solution, sodium tungstate solution, sodium sulfate solution, potassium sulfate solution, ammonium sulfate solution, and dimethyl sulfoxide solution containing lithium salt and triethylamine hydrochloride; the electrolyte concentration is 0.01-2 mol L -1 If the electrolyte concentration is too high, the intercalation voltage is too large or the time is too long, the graphite sheets will be completely peeled off; if the concentration is too low, the intercalation voltage is too small or the time is too short, the graphite sheets will not expand sufficiently, which is not conducive to the optimization of the catalyst catalytic performance.

[0015] Preferably, the electrolyte is dilute sulfuric acid.

[0016] Step 1: The electrochemical intercalation uses a DC power supply with a voltage of 0.5-8.0V and an intercalation time of 1-180min. Under the above conditions, the intercalated graphite flakes are less likely to fall off, and can maintain the original morphology and size while ensuring the expansion of the graphite flakes. At the same time, the expanded size is easy to be attached to the organic ligand later.

[0017] Preferably, the electrochemical intercalation voltage is 2-3 V and the intercalation time is 10-40 min.

[0018] In step 2, the organic ligand salt includes any one of 1,3,5-benzenetricarboxylate, naphthalene dicarboxylate, terephthalate, and 1,2,3,4-cyclobutane tetracarboxylate. The organic ligand salt needs to contain a carboxyl salt group (-COOX, X is a salt ion) to combine with metal ions such as iron and nickel to form a metal organic framework material.

[0019] Preferably, the organic salt ligand is 1,3,5-benzenetricarboxylate, which contains three carboxyl salt groups and can randomly combine with two or more metal active ions such as iron, nickel, and cobalt to form irregular metal active sites, which is beneficial to the catalytic reaction.

[0020] The organic ligand salt includes soluble salts such as sodium salt and potassium salt thereof. The organic ligand salt may be used directly, or the corresponding organic ligand acid and inorganic base may be used in combination, such as 1,3,5-benzenetricarboxylic acid and sodium hydroxide.

[0021] The molar concentration of the organic ligand salt in the organic ligand salt solution is 0.01-2 mol L -1 The appropriate concentration of organic ligand salt can avoid the blockage between graphite sheets and ensure the amount of organic ligands intercalated between graphite sheets, which is beneficial to the later catalytic reaction. The organic ligand salt has a suitable number of coordinated and uncoordinated carboxylate groups. The coordinated carboxylate groups can connect to transition metal atoms and provide catalytic active sites, while the uncoordinated carboxylate groups can play a role in proton transfer. Preferably, the molar concentration of the organic ligand salt is 0.01-0.05 mol L -1 .

[0022] The solvent used in the organic ligand salt solution includes water and / or ethanol.

[0023] Preferably, the solvent is a mixed solvent of ethanol and deionized water, with a volume ratio of 1:0.5-3.0. More preferably, the volume ratio of ethanol to water is 1:1.

[0024] In step 2, the electrochemical intercalation adopts a direct current power supply, the electrochemical intercalation voltage is 0.5-8V, and the time is 1-180min; the intercalation voltage and time determine the amount of organic ligand intercalation in the graphite sheet to a certain extent. If the concentration of the organic salt solution is too high, the intercalation voltage is too large or the time is too long, the graphite sheet will be blocked by the organic component, which is not conducive to the subsequent coordination of the inorganic metal component and the organic precursor, and will also damage the morphology of the graphite sheet. Preferably, the intercalation voltage of step 2 is 3-8V, and the intercalation time is 30min-180min.

[0025] The transition metal salt in step 3 includes any one or more of iron salt, nickel salt, cobalt salt and copper salt.

[0026] Preferably, the transition metal salt is a soluble salt, including one or more of sulfates, chlorates, chlorides and acetates of transition metals.

[0027] In some embodiments, the iron salt includes one of ferric acetate, ferric sulfate, ferric nitrate, ferric chloride, and hydrates thereof, etc. Preferably, the iron salt is ferric nitrate nonahydrate.

[0028] In some embodiments, the nickel salt includes one of nickel acetate, nickel sulfate, nickel nitrate, nickel chloride, and hydrates thereof, etc. Preferably, the nickel salt is nickel chloride hexahydrate.

[0029] In some embodiments, the cobalt salt includes one of cobalt acetate, cobalt sulfate, cobalt nitrate, cobalt chloride, and hydrates thereof. Preferably, the cobalt salt is anhydrous cobalt acetate.

[0030] In some embodiments, the copper salt includes one of copper acetate, copper sulfate, copper nitrate, copper chloride and hydrates thereof, etc. Preferably, the copper salt is copper acetate hydrate.

[0031] Further preferably, the transition metal salt is a mixture of nickel salt and iron salt.

[0032] The molar concentration of transition metal in the transition metal salt solution in step 3 is 0.01-2 mol L -1 If the concentration of the transition metal salt solution is too high, the number of coordinated carboxylate groups will be less, which is not conducive to proton transfer; if the concentration is too low, the number of coordinated carboxylate groups with nickel and iron will be less, the number of active centers will be small, and the catalytic performance of the catalyst will be poor. The preferred transition metal molar concentration is 0.01-0.05 mol L -1 .

[0033] The soaking reaction time in step 3 is 2-48 hours. The soaking process is to allow the transition metal to be immersed in the graphite sheets and to combine with the organic ligands between the graphite sheets to form MOFs materials. If the soaking time is too long, the metal active centers may aggregate, and if the soaking time is too short, it will be difficult for the organic salt and the inorganic salt to fully react to form transition metal-based MOFs. The temperature of the soaking process is 15-60°C. The preferred soaking time is 12-48 hours.

[0034] The molar ratio of the carboxylic acid group in the organic ligand salt to the transition metal salt should be 1:0.8-1.5, preferably 1:1.

[0035] On the other hand, the present invention provides a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure prepared according to the method, wherein the transition metal organic-inorganic metal framework structure in the catalyst is confined between layers of graphite sheets. It can effectively block the direct contact between the catalyst and the harsh reaction environment, effectively delay or prevent the deactivation of the catalyst, and at the same time, the confinement effect greatly shortens the mass transfer distance in the catalytic process, thereby further improving the electrocatalytic oxygen evolution performance, which is of great significance for replacing traditional commercial precious metal catalysts.

[0036] The present invention also provides the use of the two-dimensional confined catalyst of the transition metal-based organic-inorganic metal framework structure in oxygen evolution reaction.

[0037] Specifically, the two-dimensional confined catalyst is used as the working electrode, and a three-electrode system is used, specifically using an Ag / AgCl electrode as a reference electrode, a carbon rod as a counter electrode, and a potassium hydroxide solution as an electrolyte to perform an electrolytic water oxygen evolution reaction. The catalyst exhibits excellent electrochemical performance and stability at 10 mA cm -2 The overpotential is only 106mV at a current density of 1.38kV, and it can operate stably for more than 150h.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The present invention utilizes electrochemical intercalation and impregnation methods to obtain a two-dimensional confined catalyst of a nickel-iron-based organic-inorganic metal framework structure, wherein NiFe-MOFs is confined between graphite layers.

[0040] (2) The catalyst prepared by the present invention can effectively block the direct contact between the catalyst and the harsh reaction environment, effectively delaying or preventing the deactivation of the catalyst. At the same time, the confinement effect greatly shortens the mass transfer distance in the catalytic process, making up for the disadvantage of poor conductivity of MOFs materials, thereby greatly improving the electrocatalytic oxygen evolution performance and stability of the catalyst.

[0041] (3) The catalyst preparation method of the present invention has the advantages of being simple, efficient, low cost, highly controllable and reproducible, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a scanning electron microscope image of the cross section of the catalyst prepared in Example 1.

[0043] Figure 2 This is a transmission electron micrograph of the cross section of the catalyst prepared in Example 1.

[0044] Figure 3 High-resolution transmission electron microscopy image and selected area electron diffraction spectrum of the catalyst prepared in Example 1.

[0045] Figure 4 This is a scanning electron microscope image and electron energy spectrum analysis diagram of the inner layer of the catalyst graphite sheet prepared in Example 1.

[0046] Figure 5 Polarization curves of the oxygen evolution reaction in water electrolysis of the catalysts prepared in Example 1 and Comparative Examples 1 to 4 in the application examples.

[0047] Figure 6 This is a curve diagram of the voltage variation over time under constant current for the electrocatalytic water splitting and oxygen release reaction of the catalyst prepared in Example 1.

[0048] Figure 7 Polarization curves of the oxygen evolution reaction in water electrolysis of the catalysts prepared in Example 2 and Comparative Examples 1-5 in the application examples. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0050] The raw materials used in the following specific embodiments are all purchased from the market.

[0051] Example 1

[0052] (1) Prepare 0.5 mol L -1 Commercially available graphite sheets (1 cm × 3 cm) were electrochemically intercalated with dilute sulfuric acid using a DC power supply. The solvent was 50 mL 0.5 mol L -1 The intercalation voltage was 3 V and the intercalation time was 30 min. After the intercalation, the graphite sheet was soaked and washed with deionized water.

[0053] (2) 420 mg of 1,3,5-benzenetricarboxylic acid and 240 mg of sodium hydroxide were added to 75 mL of deionized water and stirred until the powder was completely dissolved. The prepared solution, a DC power supply and the graphite sheet of step (1) were used for electrochemical intercalation. The intercalation voltage was 5 V and the intercalation time was 2 h. After the intercalation, the graphite sheet was soaked and washed with deionized water;

[0054] (3) 1.21 g of ferric nitrate nonahydrate and 0.713 g of nickel chloride hexahydrate are placed in a mixed solvent of 50 mL of deionized water and 50 mL of ethanol, and stirred until the powder is completely dissolved to obtain a clear and transparent inorganic salt solution. The graphite sheet obtained in step (2) is immersed in the inorganic salt solution for 24 hours, and then the graphite sheet is taken out, and is immersed and washed with distilled water and ethanol for 3 times respectively, and dried at 60° C. overnight to obtain a two-dimensional confined catalyst with a nickel-iron based organic-inorganic metal framework structure, which can be represented by NiFe-BTC / G.

[0055] The prepared NiFe-BTC / G was observed by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). Figure 1 As shown in the TEM image Figure 2 As shown. Figure 1-2 It can be seen that the graphite sheets are open and the catalyst can be uniformly inserted between the layers of graphite. The high-magnification transmission electron microscopy and selected area electron diffraction patterns of NiFe-BTC / G prepared in this example are shown in FIG. Figure 3 As shown, no diffraction fringes or diffraction rings are observed in the figure, indicating that the catalyst is an amorphous material.

[0056] The scanning electron microscope image and electron energy spectrum analysis diagram of the inner layer of the prepared catalyst graphite sheet are shown in the figure. Figure 4 As shown, it can be proved that the nickel-iron based organic-inorganic metal framework material is successfully intercalated into the graphene sheet.

[0057] Comparative Example 1

[0058] According to the process of Example 1, no ferric nitrate nonahydrate is added in step (3), to obtain a two-dimensional confined catalyst with a nickel-based organic-inorganic metal framework structure, denoted as Ni-BTC / G.

[0059] Comparative Example 2

[0060] According to the process of Example 1, without adding nickel chloride hexahydrate in step (3), a two-dimensional confined catalyst with an iron-based organic-inorganic metal framework structure is obtained, which is denoted as Fe-BTC / G.

[0061] Comparative Example 3

[0062] According to the process of Example 1, only step (1) is performed to obtain an intercalated graphite foil, which is recorded as Graphite foil.

[0063] Comparative Example 4

[0064] According to the process of Example 1, no graphite sheet is used, no electrochemical intercalation step is performed, only the inorganic salt solution and the organic salt solution are mixed and stirred and left to stand for 24 hours, and then the mixture is soaked and washed with distilled water and ethanol for 3 times respectively, and dried at 60° C. overnight to obtain a nickel-iron-based organic-inorganic metal framework material, which is recorded as Bulk NiFe-BTC.

[0065] Application Examples

[0066] (1) Using a three-electrode system, the catalyst prepared in Example 1 or Comparative Examples 1-4 was used as the working electrode, the counter electrode was a carbon rod, the reference electrode was a saturated Ag / AgCl electrode, and the electrolyte was 1.0 M KOH;

[0067] (2) CV activation: Shanghai Chenhua CHI 760E electrochemical workstation was used. Nitrogen was introduced into the electrolyte for 30 min before testing. The CV program was used, with the test interval at 0-0.8 V vs. Ag / AgCl and a scan rate of 50 mV s -1 After 50 cycles, the electrode reaches a stable state.

[0068] The catalysts prepared in Example 1 and Comparative Examples 1-4 were subjected to linear sweep voltammetry (LSV) test. After activation, the program was switched to the LSV program, the test interval was 0-0.8 V vs. Ag / AgCl, the sweep rate was 1 mV / s, and the overpotential was 1.23 V relative to the reversible hydrogen electrode and 10 mA cm -2 The potential difference is measured. Figure 5 The polarization curves of the NiFe-BTC / G catalyst provided in the embodiment and Ni-BTC / G, Fe-BTC / G, Graphite foil and Bulk NiFe-BTC in the electrolysis of water and oxygen evolution in 1.0M KOH solution are shown. It can be seen that NiFe-BTC / G has a high conductivity at 10 mA cm -2 The overpotential at the current density is only 106mV, while the overpotentials of Ni-BTC / G, Fe-BTC / G, Graphite foil and Bulk NiFe-BTC are 212mV, 226mV, 380mV and 339mV respectively, and the catalytic effect is significantly better than other comparative examples. The organic salt ligand 1,3,5-benzenetricarboxylate contains three carboxyl salt groups, which can randomly combine with two or more of the active metal ions such as iron, nickel and cobalt to form irregular metal active sites, which is conducive to the catalytic reaction.

[0069] The catalyst prepared in Example 1 was tested for stability

[0070] After CV activation, switch the program to ISTEP, set the current to 0.010A, and the time to 540000s. Figure 6 As shown, the potential of NiFe-BTC / G does not change much over time, proving its excellent catalytic stability.

[0071] Example 2

[0072] (1) Prepare 0.5 mol L -1 Commercially available graphite sheets (1 cm × 3 cm) were electrochemically intercalated with dilute sulfuric acid using a DC power supply. The solvent was 50 mL 0.5 mol L -1 The intercalation voltage was 3 V and the intercalation time was 30 min. After the intercalation, the graphite sheet was soaked and washed with deionized water.

[0073] (2) dissolving 250 mg of dimethyl naphthalene dicarboxylate in 75 mL of deionized water, stirring until the powder is completely dissolved, and using the prepared solution, a DC power supply and the graphite sheet of step (1) for electrochemical intercalation, the intercalation voltage is 5 V, the intercalation time is 1 h, and after intercalation, the graphite sheet is soaked and washed with deionized water;

[0074] (3) 0.39 g of ferric nitrate nonahydrate and 0.23 g of nickel nitrate hexahydrate are placed in a mixed solvent of 50 mL of deionized water and 50 mL of ethanol, and stirred until the powder is completely dissolved to obtain a clear and transparent inorganic salt solution. The graphite sheet obtained in step (2) is immersed in the inorganic salt solution for 24 hours, and then the graphite sheet is taken out, and is immersed and washed with distilled water and ethanol for 3 times respectively, and dried at 60° C. overnight to obtain a nickel-iron based organic-inorganic metal framework structure two-dimensional confined catalyst, which can be represented by FeNi-MOF / G.

[0075] Example 3

[0076] According to the process of Example 2, no ferric nitrate nonahydrate is added in step (3), thereby obtaining a two-dimensional confined catalyst with a nickel-based organic-inorganic metal framework structure, which is denoted as Ni-MOF / G.

[0077] Example 4

[0078] According to the process of Example 2, nickel nitrate hexahydrate is not added in step (3), to obtain a two-dimensional confined catalyst with an iron-based organic-inorganic metal framework structure, which is denoted as Fe-MOF / G.

[0079] Example 5

[0080] According to the process of Example 2, in step (3), nickel nitrate hexahydrate and ferric nitrate nonahydrate are not added, and 0.188 g of cobalt chloride hexahydrate is added to obtain a two-dimensional confined catalyst with a cobalt-based organic-inorganic metal framework structure, which is recorded as Co-MOF / G.

[0081] Example 6

[0082] According to the process of Example 2, in step (3), nickel nitrate hexahydrate and ferric nitrate nonahydrate are not added, and 0.163 g of hydrated copper nitrate is added to obtain a two-dimensional confined catalyst with a copper-based organic-inorganic metal framework structure, which is recorded as Cu-MOF / G.

[0083] Example 7

[0084] According to the process of Example 2, in step (3), instead of adding nickel nitrate hexahydrate, 0.39 g of ferric nitrate nonahydrate and 0.188 g of cobalt chloride hexahydrate were added to obtain a two-dimensional confined catalyst with an iron-cobalt-based organic-inorganic metal framework structure, which was recorded as FeCo-MOF / G.

[0085] Application Examples

[0086] (1) Using a three-electrode system, the catalyst prepared in Example 2-7 was used as the working electrode, the counter electrode was a carbon rod, the reference electrode was a saturated Ag / AgCl electrode, and the electrolyte was 1.0 M KOH;

[0087] (2) CV activation: Shanghai Chenhua CHI 760E electrochemical workstation was used. Nitrogen was introduced into the electrolyte for 30 min before testing. The CV program was used, with the test interval at 0-0.8 V vs. Ag / AgCl and a scan rate of 50 mV s -1 After 50 cycles, the electrode reaches a stable state.

[0088] The catalyst prepared in Example 2-7 was subjected to linear sweep voltammetry (LSV) test. After activation, the program was switched to the LSV program, the test interval was 0-0.8 V vs. Ag / AgCl, the sweep rate was 1 mV / s, and the overpotential was 1.23 V relative to the reversible hydrogen electrode and 10 mA cm -2 The potential difference is measured. Figure 7 The polarization curves of the electrolytic water evolution reaction of various materials in 1.0 M KOH solution are shown. It can be seen that FeNi-MOF / G, Ni-MOF / G, Fe-MOF / G, Co-MOF / G, Cu-MOF / G and FeCo-MOF / / G are -2 The overpotentials at current densities of 1.1, 1.2, 1.5, 2.0, 2.5, 3.5, 4.5, 5.5, 6.5, 7.5, 8.5, 9.5, 10.5, 11.5, 12.5, 13.5, 14.5, 15.5, 16.5, 17.0, 18.5, 19.5, 20.5, 21.0, 22.5, 23.5, 24.5, 26.5, 27.5, 28.5, 29.5, 30.5, 31.5, 32.5, 33.5, 34.5, 36.5, 37.5, 38.5, 39.5, 40.5, 41.5, 42.

Claims

1. A method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure, characterized in that: Includes steps: Step 1: electrochemically intercalate graphite sheets in an electrolyte to obtain graphite sheets with micro-separation between layers; the electrolyte concentration is 0.01-2 mol L -1 ; Step 1 electrochemical intercalation uses a DC power supply with a voltage of 0.5-8.0V and an intercalation time of 1-180min; Step 2, placing the graphite sheet obtained in step 1 in a solution of an organic ligand salt containing a carboxylic acid group for further electrochemical intercalation to obtain a graphite sheet intercalated with an organic ligand; in step 2, the electrochemical intercalation adopts a direct current power supply, the electrochemical intercalation voltage is 0.5-8V, and the time is 30-500min; Step 3, placing the graphite sheet obtained in step 2 in a transition metal salt solution for immersion reaction, taking out the graphite sheet, washing, and drying to obtain the transition metal-based organic-inorganic metal framework structure two-dimensional confined catalyst; in step 3, the transition metal molar concentration of the transition metal salt solution is 0.01-2 mol L -1 ; The soaking reaction time is 12-48h, and the temperature is 15-60℃.

2. The method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure according to claim 1, characterized in that: In step 1, the electrolyte includes any one of a dilute sulfuric acid solution, a perchloric acid solution, a sodium tungstate solution, a sodium sulfate solution, a potassium sulfate solution, an ammonium sulfate solution, and a dimethyl sulfoxide solution containing a lithium salt and triethylammonium hydrochloride.

3. The method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure according to claim 1, characterized in that: The organic ligand salt in step 2 includes any one of 1,3,5-benzenetricarboxylate, naphthalene dicarboxylate, terephthalate, and 1,2,3,4-cyclobutane tetracarboxylate; the molar concentration of the organic ligand salt in the organic ligand salt solution is 0.01-2 mol L -1 .

4. The method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure according to claim 1, characterized in that: The transition metal salt in step 3 includes any one or more of iron salt, nickel salt, cobalt salt and copper salt.

5. The method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure according to claim 1, characterized in that: The transition metal salt is a soluble salt, including one or more of sulfates, chlorates, chlorides and acetates of transition metals.

6. The method for preparing a two-dimensional confined catalyst of a transition metal-based organic-inorganic metal framework structure according to claim 1, characterized in that: The molar ratio of the carboxylic acid group in the organic ligand salt to the transition metal salt should be 1:0.8-1.

5.

7. A two-dimensional confined catalyst with a transition metal-based organic-inorganic metal framework structure obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The transition metal organic-inorganic metal framework structure in the two-dimensional confined catalyst is confined between layers of graphite sheets.

8. Use of the two-dimensional confined catalyst of the transition metal-based organic-inorganic metal framework structure according to claim 7 in oxygen evolution reaction.

Citation Information

Patent Citations

  • Preparation method of iron-based MOFs oxygen evolution electrocatalyst with high-activity crystal face proportion, and catalyst

    CN113073350A

  • Iron boride-based metal organic framework nano-catalyst as well as preparation method and application thereof

    CN113430562A

  • Graphene / functionalized metal-organic framework material composite intercalation as well as preparation method and application thereof

    CN112421133A

  • Preparation method of transition metal doped nickel-based metal organic framework three-dimensional electrode material, product and application thereof

    CN112430828A

  • Two-dimensional ultrathin metal organic framework nanosheet electrocatalyst as well as preparation method and application thereof