A three-dimensional flexible structure tactile sensor and its preparation method
By using a three-dimensional three-dimensional flexible structure of the imitation fingerprint structure and a chitosan/CNT piezoresistive layer in the tactile sensor, combined with laser processing and printing electronics technology, the problems of low detection accuracy and insufficient flexibility in the existing technology are solved, and the problem of low detection accuracy and insufficient flexibility is achieved. High sensitivity detection and real-time perception of deformation and vibration.
Patent Information
- Application Number
- CN202210871580.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-07-22
AI Technical Summary
The existing haptic sensors have insufficient detection accuracy, which is difficult to bend or fold freely, and cannot effectively perceive weak tactile stimuli such as deformation and vibration in special environments.
A three-dimensional flexible structure tactile sensor using imitation fingerprint structure and chitosan/CNT piezoresistive layer is formed by tightly laminating the imitation fingerprint layer, piezoresistive sensing layer, stretchable electrode layer and flexible substrate layer. Flexible structural arrays, combined with laser processing and printed electronics, create sensors that can sense deformation and vibration.
High sensitivity detection of deformation and vibration is realized, and the sensor can be freely bent or folded on various curved surfaces, enhancing the real-time detection ability of tactile information and overcoming the problem of insufficient fine tactile perception ability in the prior art.
Smart Images

Figure CN115200615B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sensor technology, and in particular to a three-dimensional flexible structure tactile sensor and a preparation method thereof. Background Art
[0002] Sensors can be used to sense various external information and convert external information into electrical signals. Faced with special signals and special environments, sensors are required to be flexible, ductile, freely bendable or even foldable, easy to carry, and wearable. With the development of flexible matrix materials, flexible sensors came into being on this basis. Flexible sensors have good ductility and bendability, and their structural forms are flexible and diverse, and can be arranged arbitrarily according to the monitoring environment. The rapid development of flexible sensors has promoted the extensive research of intelligent robots, human-computer interaction, and wearable devices.
[0003] Flexible sensors are widely used in medical electronics, environmental monitoring and wearable fields. As robots enter people's daily lives, they will be engaged in many fine processing and manufacturing tasks. It is particularly important to study the fine perception ability of tactile sensors. However, the detection accuracy of existing tactile sensors is not high enough, it is not easy to bend or even fold freely, and it cannot be used in special environments, which limits the development of flexible sensors. The multilayer bionic tactile sensor based on the skin tactile perception architecture and preparation method with application patent number 202210035590.6 includes a four-layer structure, which is a human epidermal membrane layer, a PDMS-filled fabric layer, a conductive sensitive material layer and an electrode substrate, but it can only detect contact sensing including pressing, and cannot sense non-contact weak tactile stimuli such as vibration. The bionic tactile system and multifunctional robot with application patent number 201810133317.0 include a first sensor with a skin structure and a second sensor with a cilia structure, but its structure is complex and requires a two-layer structure to achieve perception. Moreover, the cilia are not easy to return to their original state after deformation, which affects the continuous working ability and stability of the sensor. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a three-dimensional flexible structure tactile sensor and a preparation method thereof, so as to solve the problem that the existing tactile sensors are difficult to meet the requirements of fine tactile perception. The present invention provides a three-dimensional flexible structure tactile sensor and a preparation method thereof. The sensor has an arch bridge-shaped three-dimensional flexible structure by adding a fingerprint-like structure and a chitosan / CNT piezoresistive layer to form a sensor array. The present invention can sense weak tactile stimuli including deformation and vibration.
[0005] The present invention adopts the following technical solutions to achieve the above-mentioned purpose:
[0006] A three-dimensional flexible structure tactile sensor, which is formed by closely stacking a fingerprint imitation layer, a piezoresistive sensing layer, a stretchable electrode layer and a flexible substrate layer from top to bottom;
[0007] The material of the flexible substrate layer is PDMS or PEN; the thickness is 50-500 μm;
[0008] The material of the stretchable electrode layer is a mixture of multi-walled carbon nanotubes and PDMS, or a mixture of silicone rubber and silver nanoparticles; the thickness is 10 to 200 μm;
[0009] The mass ratio is 1:3:10 for multi-walled carbon nanotubes and PDMS, and 1:2:4 for silicone rubber and silver nanoparticles.
[0010] The material of the piezoresistive sensor is a mixed material of chitosan and CNT; the thickness is 100-500 μm; the mass ratio is chitosan: CNT=8-30:1;
[0011] The material of the imitation fingerprint layer is silicone rubber; the surface is arrayed with imitation fingerprint-shaped protrusions, the height of the protrusions is 10 to 500 μm, the width of the protrusions is 10 to 500 μm, and the spacing between adjacent micro-protrusions is 10 to 500 μm.
[0012] The three-dimensional flexible structure tactile sensor forms an arch bridge-shaped three-dimensional flexible structure array, and the curvature thereof is 1-10.
[0013] The method for preparing the three-dimensional flexible structure tactile sensor comprises the following steps:
[0014] Laser processing technology is used to cut the flexible substrate and form an arch-bridge-shaped three-dimensional flexible structure through directional bending. Printed electronics technology or template method is used to manufacture a stretchable electrode layer on the surface of the flexible substrate. A composite material formed by chitosan and multi-walled carbon nanotubes (mw-CNT) is used to manufacture a piezoresistive sensing layer. The template method is used to manufacture the surface fingerprint-like microstructure of the sensor, thereby enhancing the sensing ability of friction and vibration. The sensor is encapsulated using flexible bonding technology to obtain a three-dimensional flexible structure tactile sensor that can work continuously and stably.
[0015] The specific steps include:
[0016] 1) Cutting and manufacturing of flexible substrate layer:
[0017] Use a laser cutter or engraving machine to cut the flexible substrate, then clean and dry it;
[0018] The flexible substrate is made of methyl siloxane (PDMS) or polyethylene naphthalate (PEN);
[0019] (2) Fabrication of the stretchable electrode layer, which can be done by one of the following two methods:
[0020] Method 1:
[0021] The multi-walled carbon nanotubes and PDMS are added to a mixed organic solvent, stirred for 30 to 60 minutes, and then the solvent is volatilized at 80 to 100 degrees Celsius for 4 to 6 hours to obtain a printing ink; then, a microelectronic printer is used to print it on a flexible substrate to form interdigital electrodes, and then annealed at 100 to 120 degrees Celsius for 20 to 40 minutes to obtain a stretchable electrode layer;
[0022] The mass ratio is: multi-walled carbon nanotubes: PDMS = 1-3:10; multi-walled carbon nanotubes: mixed organic solvent = 1:15-30;
[0023] The mixed organic solvent consists of ethanol and ethyl acetate, and the volume ratio is ethanol:ethyl acetate=1:0.5-2.
[0024] Or, method 2:
[0025] The interdigitated electrode mask is attached to a flexible substrate, the mixed material is coated on the mask, an electrode pattern is formed at the hollowed-out portion of the mask, the mask is removed, and the mixture is heated and cured at 80 to 100 degrees Celsius for 1 to 2 hours, and a stretchable electrode layer is obtained after cooling;
[0026] The mixed material is composed of silicone rubber, curing agent and silver nanoparticles, and the mass ratio of silicone rubber, curing agent and silver nanoparticles is 1:0.1:2-4.
[0027] (3) Fabrication of piezoresistive sensing layer:
[0028] The chitosan powder is dissolved in a 2-4wt% glacial acetic acid solution, and then stirred at 60-70°C for 40-60 minutes, and then glycerol is added and stirred again for 10-30 minutes, and then a 10%-12.5% multi-walled carbon nanotube solution is added and stirred for 30-50 minutes; the mixed solution is ultrasonically defoamed for 20-40 minutes, taken out and allowed to stand at room temperature for 1-2 hours; then the solution is poured into a mold, dried in a drying oven at 80-100°C for 20-40 minutes, and cooled to obtain a piezoresistive sensing layer;
[0029] Wherein, 4 to 6 g of chitosan, 100 to 200 μL of glycerol, and 2 to 4 ml of multi-walled carbon nanotube solution are added to every 20 to 40 ml of glacial acetic acid solution; the stirring speed is 350 to 850 rmp;
[0030] (4) Manufacture of fingerprint-like layer:
[0031] The silicone rubber and the curing agent are mixed in a mass ratio of 1:0.1-0.2, and after degassing in a vacuum drying oven, poured into a fingerprint-like mold, cured at 85-100° C. for 1-2 hours, and then cooled to obtain a fingerprint-like layer;
[0032] The silicone rubber and curing agent are specifically Sylgard TM product.
[0033] (5) Assembly and directional bending of three-dimensional flexible structure tactile sensors:
[0034] The fingerprint-imitation layer and the piezoresistive sensing layer are sequentially bonded to a flexible substrate with a stretchable electrode layer using a silicone adhesive, and the cut part of the flexible substrate is directionally bent to form an arch-shaped three-dimensional flexible structure with a curvature of 1 to 10, which is fixed to the surface of the flexible substrate with a silicone adhesive to finally obtain a three-dimensional flexible structure tactile sensor.
[0035] The essential features of the present invention are:
[0036] When the sensor is pressed slightly, it is easy to deform due to its arch bridge structure. The deformation is transmitted to the piezoresistive sensing layer, and the piezoresistive sensing layer converts it into a resistivity change. The imitation fingerprint layer is composed of imitation fingerprint-shaped protrusions. When an object contacts the imitation fingerprint layer of the sensor, the imitation fingerprint micro-protrusions have a greater surface roughness than the smooth surface, and the friction is also greater. The large friction makes the sensor deform larger, thereby improving the detection sensitivity of the sensor.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The present invention obtains a three-dimensional flexible structure tactile sensor with an arch bridge shape by tightly stacking a fingerprint imitation layer, a piezoresistive sensing layer, a stretchable electrode layer and a flexible substrate layer, and directionally bending the flexible substrate layer to form an array.
[0039] (2) Each layer of the three-dimensional flexible structure tactile sensor is made of flexible materials and uses a flexible substrate, so that the sensor can be freely bent or even folded and can be applied to various curved surfaces.
[0040] (3) The fingerprint-like micro-protrusions of the three-dimensional flexible structure tactile sensor can increase the friction force, and the piezoresistive sensing layer can convert stimuli such as deformation and vibration into resistivity changes, and conduct them through the stretchable electrode layer. This structure can improve the sensor's detection sensitivity to deformation and vibration ( Figure 5 The relationship between the relative resistance change and pressure of the sensor obtained in Example 1 is shown in FIG. The sensitivity of the tactile sensor is mainly divided into two stages. The first stage is from 0Pa to 2kPa, with a sensitivity of 0.023Pa-1; the second stage is from 2kPa to 6kPa, with a sensitivity of 0.0047Pa -1; The experimental results prove the feasibility of the sensor structure, and the sensor has extremely high sensitivity compared with traditional sensors. ) and enhance the sensor's real-time detection capability for the spatial distribution of tactile information, so that the sensor can sense weak tactile stimuli including deformation and vibration, overcoming the deficiency of sensors in the prior art that are difficult to meet the requirements of fine tactile perception.
[0041] (4) The three-dimensional flexible structure tactile sensor of the present invention is combined with laser processing and printed electronic technology, etc., and can be prepared on a large area, reducing manufacturing costs and increasing the flexibility of sensor design and development. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic diagram of the structural decomposition of a three-dimensional flexible structure tactile sensor of the present invention.
[0043] Figure 2 for Figure 1 A three-dimensional schematic diagram of .
[0044] Figure 3 for Figure 1 Schematic diagram of the fingerprint-like layer structure. The left picture is a top view, and the right picture is a cross-sectional view of the dotted part of the left picture.
[0045] Figure 4 for Figure 1 Schematic diagram of the mask for the stretchable electrode layer.
[0046] Figure 5 Schematic diagram of the relationship between the relative resistance change and pressure of the sensor obtained in Example 1.
[0047] In the figure, 1. Flexible substrate layer, 2. Stretchable electrode layer, 3. Piezoresistive sensing layer, 4. Imitation fingerprint layer. Specific implementation plan
[0048] The invention will be further described below in conjunction with the drawings and embodiments. The described embodiments are only part of the embodiments of the present invention. Other embodiments obtained without any innovative work are within the protection scope of the present invention.
[0049] like Figure 1 , Figure 2As shown, the three-dimensional flexible structure tactile sensor is mainly composed of a flexible substrate layer 1, a stretchable electrode layer 2, a piezoresistive sensing layer 3 and an imitation fingerprint layer 4 tightly stacked. The piezoresistive sensing layer 3 is located on the stretchable electrode layer 2, and the imitation fingerprint layer 4 is located on the piezoresistive sensing layer 3. The flexible substrate layer 1 can be bent in a directional manner to form a three-dimensional flexible structure and constitute a three-dimensional flexible structure array. The stretchable electrode layer 2 can transmit the generated electrical signal, can be bent and deformed, and has stable conductive properties. The piezoresistive sensing layer 3 can convert stimuli such as deformation, vibration, and touch into resistivity changes. The imitation fingerprint layer 4 is composed of imitation fingerprint-shaped protrusions, which can increase friction.
[0050] like Figure 3 As shown, the left picture is a top view of the imitation fingerprint layer 4 structure, and the right picture is a cross-sectional view of the dotted part of the left picture. There are five imitation fingerprint basic units in total, and each unit is distributed with circles of Chinese characters. The black rectangular part is a micro-protrusion, and the height of the micro-protrusion is 50μm. The spacing between adjacent micro-protrusions is 25μm, and the width of the micro-protrusion is 25μm. The micro-protrusion structure of the imitation fingerprint can increase the roughness of the sensor surface, thereby increasing the detection sensitivity of the sensor.
[0051] like Figure 4 As shown, the stretchable electrode layer 2 adopts interdigital electrodes, the mask size is 4x4cm, and four interdigital electrodes are distributed.
[0052] Example 1
[0053] (1) Cutting and manufacturing of the flexible substrate layer 1:
[0054] The flexible substrate was cut into 2.9x0.5 cm pieces using a laser cutter, and the thickness of the flexible substrate was 50 μm. The flexible substrate was a polydimethylsiloxane (PDMS) film. After the flexible substrate was cut, its surface was cleaned with ethanol and deionized water, respectively, and dried with nitrogen.
[0055] (2) Fabrication of the stretchable electrode layer 2:
[0056] The multi-walled carbon nanotubes and PDMS materials were added to a mixed solvent of ethanol and ethyl acetate (mass ratio of 1:1) at a mass ratio of 1:10, and the mass ratio of multi-walled carbon nanotubes to the solvent was 1:20, and stirred for 30 minutes, and then the solvent was evaporated at 90 degrees Celsius for 6 hours to prepare the printing ink. The interdigitated electrodes were inkjet printed on the surface of the cut part of the flexible substrate layer 1, and then annealed at 120 degrees Celsius for 20 minutes, with a thickness of 50μm.
[0057] (3) Manufacturing of the piezoresistive sensing layer 3:
[0058] 6g of chitosan powder was dissolved in 20ml of 2wt% glacial acetic acid solution, then stirred at 70°C at 600rmp for 40 minutes, then 100μL of glycerol was added and stirred again for 10 minutes, and then 2ml of 12.5% multi-walled carbon nanotube solution was added and stirred for 30 minutes. The mixed solution was ultrasonically debubbled for 20 minutes, taken out and allowed to stand at room temperature for 2 hours. The solution was then poured into a rectangular mold, dried in a drying oven at 80°C for 20 minutes, and cooled to obtain a piezoresistive sensing layer 3 of about 100μm.
[0059] (4) Manufacturing of imitation fingerprint layer 4:
[0060] Silicone rubber (Sylgard TM Silicone rubber basic components) and curing agent (specifically Sylgard TM Organic silicon elastomer curing agent, item number 01673921. ) are uniformly mixed in a mass ratio of 1:0.1, degassed in a vacuum drying oven, poured into a fingerprint-like mold, the height of the fingerprint-like protrusion is 50 μm, the spacing between adjacent micro-protrusions is 25 μm, the width of the micro-protrusion is 25 μm, and cured at 90 degrees Celsius for 1 hour and cooled to obtain a fingerprint-like layer 4 with a thickness of 75 μm.
[0061] (5) Assembly and directional bending of three-dimensional flexible structure tactile sensors:
[0062] The fingerprint imitation layer and the piezoresistive sensing layer are sequentially bonded to the flexible substrate with the stretchable electrode layer using a silicone adhesive, and the cut portion of the flexible substrate is directional bent to form an arch bridge-shaped three-dimensional flexible structure with a curvature of 1 to 10. The structure is fixed to the surface of the flexible substrate using a silicone adhesive.
[0063] Figure 5 Example 1 is the sensor data obtained using the Mark-10 dynamometer and the Keithley 2400 source meter, showing the relationship between the relative resistance change and the pressure. The sensitivity of the tactile sensor is mainly divided into two stages. The first stage is from 0Pa to 2kPa, and the sensitivity is 0.023Pa -1 ; The second stage is from 2kPa to 6kPa, with a sensitivity of 0.0047Pa -1 ; The experimental results prove the feasibility of the sensor structure, and the sensor has extremely high sensitivity compared to traditional sensors.
[0064] Example 2
[0065] The other steps are the same as those in Example 1, except that the flexible substrate material in step (1) is replaced by a polyethylene naphthalate (PEN) film instead of a polydimethylsiloxane (PDMS) film.
[0066] Example 3
[0067] The other steps are the same as those in Example 1, except that the electrode preparation method in step (2) is replaced by:
[0068] The polydimethylsiloxane liquid, silicone elastomer curing agent and silver nanoparticles are uniformly mixed in a mass ratio of 1:0.1:3, and the interdigital electrode mask is attached to the flexible substrate layer 1. Under an optical microscope, the electrode hollowing part of the interdigital electrode mask is aligned with the cut part of the flexible substrate layer 1. The above-mentioned mixed material is coated on the flexible substrate layer 1 with a coating thickness of 100 μm. After removing the mask, heat and cure at 90 degrees Celsius for 1 hour, and obtain the stretchable electrode layer 2 after cooling.
[0069] Matters not covered by the present invention are known technologies.
Claims
1. A method for preparing a three-dimensional flexible structure tactile sensor, characterized in that The tactile sensor is composed of a fingerprint-like layer, a piezoresistive sensing layer, a stretchable electrode layer and a flexible substrate layer tightly stacked from top to bottom; The material of the flexible substrate layer is PDMS or PEN; the thickness is 50-500 μm; The material of the stretchable electrode layer is a mixture of multi-walled carbon nanotubes and PDMS, or a mixture of silicone rubber and silver nanoparticles; the thickness is 10-200 μm; Among them, the mass ratio is, multi-walled carbon nanotubes and PDMS = 1~3:10, silicone rubber: silver nanoparticles = 1:2~4; The material of the piezoresistive sensor is a mixed material of chitosan and CNT; the thickness is 100-500 μm; the mass ratio is chitosan: CNT=8-30:1; The imitation fingerprint layer is made of silicone rubber with a thickness of 50-500 μm. The method for preparing the three-dimensional flexible structure tactile sensor comprises the following steps: (1) Cutting and manufacturing of flexible substrate layer: Use a laser cutter or engraving machine to cut the flexible substrate, then clean and dry it; The flexible substrate is made of methyl siloxane (PDMS) or polyethylene naphthalate (PEN); (2) Fabrication of the stretchable electrode layer, which can be done by one of the following two methods: Method 1: Add multi-walled carbon nanotubes and PDMS to a mixed organic solvent, stir for 30 to 60 minutes, and then volatilize the solvent at 80 to 100 degrees Celsius for 4 to 6 hours to obtain a printing ink; then use a microelectronic printer to print it on a flexible substrate to form interdigital electrodes, and then anneal at 100 to 120 degrees Celsius for 20 to 40 minutes to obtain a stretchable electrode layer; The mass ratio is MWCNTs: PDMS = 1-3:10; MWCNTs: mixed organic solvent = 1:15-30; Or, method 2: The interdigitated electrode mask is attached to a flexible substrate, the mixed material is coated on the mask, an electrode pattern is formed at the hollowed-out portion of the mask, the mask is removed, and the mixture is heated and cured at 80 to 100 degrees Celsius for 1 to 2 hours, and a stretchable electrode layer is obtained after cooling; The mixed material is composed of silicone rubber, curing agent and silver nanoparticles, and the mass ratio of silicone rubber, curing agent and silver nanoparticles is 1:0.1:2-4. (3) Fabrication of piezoresistive sensing layer: The chitosan powder is dissolved in a 2-4wt% glacial acetic acid solution, and then stirred at 60-70°C for 40-60 minutes, and then glycerol is added and stirred again for 10-30 minutes, and then a 10%-12.5% multi-walled carbon nanotube solution is added and stirred for 30-50 minutes; the mixed solution is ultrasonically defoamed for 20-40 minutes, taken out and allowed to stand at room temperature for 1-2 hours; then the solution is poured into a mold, dried at 80-100°C for 20-40 minutes, and cooled to obtain a piezoresistive sensing layer; Among them, 4-6 g of chitosan, 100-200 μL of glycerol, and 2-4 ml of multi-walled carbon nanotube solution were added to every 20-40 ml of glacial acetic acid solution; (4) Manufacture of fingerprint-like layer: The silicone rubber and the curing agent are mixed in a mass ratio of 1:0.1-0.2, and after degassing in a vacuum drying oven, poured into a fingerprint-like mold, cured at 85-100°C for 1-2 hours, and then cooled to obtain a fingerprint-like layer; (5) Assembly and directional bending of three-dimensional flexible structure tactile sensors: The fingerprint-imitation layer and the piezoresistive sensing layer are sequentially bonded to a flexible substrate with a stretchable electrode layer using a silicone adhesive, and the cut part of the flexible substrate is directionally bent to form an arch-shaped three-dimensional flexible structure with a curvature of 1 to 10, which is fixed to the surface of the flexible substrate with a silicone adhesive to finally obtain a three-dimensional flexible structure tactile sensor.
2. The method for preparing a three-dimensional flexible structure tactile sensor as described in claim 1 is characterized in that the surface of the imitation fingerprint layer is an array of imitation fingerprint-shaped protrusions, the height of the protrusions is 10~500μm, the width of the protrusions is 10~500μm, and the spacing between adjacent micro-protrusions is 10~500μm.
3. The method for preparing the three-dimensional flexible structure tactile sensor according to claim 1, characterized in that The three-dimensional flexible structure tactile sensor forms an arch bridge-shaped three-dimensional flexible structure array, and the curvature thereof is 1-10.
4. The method for preparing the three-dimensional flexible structure tactile sensor according to claim 1, characterized in that The mixed organic solvent described in step (1) is composed of ethanol and ethyl acetate, and the volume ratio is ethanol:ethyl acetate = 1:0.5~2.
5. The method for preparing the three-dimensional flexible structure tactile sensor according to claim 1, characterized in that The stirring speed in step (3) is 350~850rmp.
6. The method for preparing a three-dimensional flexible structure tactile sensor according to claim 1, wherein the silicone rubber and curing agent are specifically SylgardTM product.