A packaging method for a packaging structure of a planar power device

By using metal bumps and three-dimensional metal frames for welding and plastic packaging material filling in planar power devices, the problem of high on-resistance in traditional packages is solved, a packaging structure with low on-resistance and excellent heat dissipation performance is achieved, and the product is improved. current carrying capacity and stability.

CN115274461BActive Publication Date: 2024-10-11ZHE JIANG HE XIN SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210604881.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-31
Publication Date
2024-10-11
Estimated Expiration
2042-05-31

AI Technical Summary

Technical Problem

The traditional wire-bonded package has a large on-resistance, which affects the current carrying capacity and heat dissipation performance of the product, making it difficult to meet the low loss and high thermal stability requirements of high-power consumption equipment such as 5G base stations.

Method used

Using the packaging structure of planar power devices, through welding of metal bumps and three-dimensional metal frames and filling with plastic packaging materials, a packaging structure with low on-resistance and excellent heat dissipation performance is formed, simplifying the process and reducing inductance and capacitance, and realizing the integration of chips and PCBs direct interconnection and efficient cooling.

Benefits of technology

The on-resistance of the package is reduced, the current carrying capacity and heat dissipation performance are improved, the stability and quality of the product are improved, the production process is simplified and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115274461B_ABST
    Figure CN115274461B_ABST
Patent Text Reader

Abstract

The present invention discloses a packaging method for a packaging structure applied to a planar power device, and belongs to the field of semiconductor packaging technology. It adopts the metal bump under the chip on the front of the chip to be flipped onto the etched surface of the three-dimensional metal frame, and realizes direct interconnection between the chip and the PCB through the folding of the metal bump under the chip and the three-dimensional metal frame, which simplifies the packaging structure, avoids the traditional wire bonding process, reduces the packaging resistance, and increases the current carrying capacity; at the same time, it shortens the interconnection distance between the chip and the outside world, and enhances the conductive effect of the chip. It provides a single-sided precise plastic sealing and low-temperature bonding protective film process, simplifies the packaging process, and compared with the traditional wire bonding method, the FC process transmission performance is improved, the interconnection structure size is short, the inductance, resistance and capacitance are reduced, the signal integrity, the radio frequency performance is better, the production efficiency is improved and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a packaging method for a packaging structure applied to a planar power device, belonging to the technical field of semiconductor packaging. Background Art

[0002] With the development of the 5G industry, consumer electronics and new energy vehicle industries, for example, the power consumption of 5G base stations has increased. The power consumption of 5G base stations is twice that of 4G. In order to reduce power consumption requirements, it is necessary to increase the requirements for low loss and high thermal stability of chips. At the same time, this also places higher requirements on the package type's low on-resistance, low heat generation and fast heat dissipation.

[0003] Traditional wire bonding packages all use wire bonding packaging, and the wire resistance R w Large, which will increase the on-resistance of the entire package and ultimately affect the current carrying capacity of the product. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a packaging method for a packaging structure applied to a planar power device, so that the chip using this packaging method can achieve low on-resistance, carry large current, have excellent heat dissipation performance, and have a simple packaging structure.

[0005] The technical solution of the present invention:

[0006] The present invention provides a packaging method for a packaging structure of a planar power device, and the process method thereof is as follows:

[0007] Step 1: prepare the incoming wafer, on which there are neatly arranged horizontal and vertical cross-cutting lanes I, which pre-divide the wafer into a plurality of chips. Each chip is provided with a plurality of under-chip metal bumps on the front side and a heat dissipation layer on the back side. One end of the under-chip metal bump corresponds to the electrode of the chip, and the other end is provided with a welding layer I;

[0008] Step 2: Using a dicing process to cut the wafer along dicing lanes I to form a plurality of independent chips;

[0009] Step 3, prepare a metal original plate, the material of which is preferably copper with excellent electrical conductivity, which includes a metal surface I on the upper surface and a metal surface II on the lower surface, and the metal surface II is electroplated to form a welding layer II;

[0010] Step 4: The back side of the chip is fixedly connected to the metal surface Ⅰ of the metal original plate through silver paste in sequence, and the chips are arranged in an array with spaces between them, leaving a cutting path Ⅱ on the metal original plate;

[0011] Step 5: Cut the metal original plate along cutting path II to form a new chip monomer, and the metal original plate forms a metal heat sink on the back of the chip;

[0012] Step 6, prepare a three-dimensional metal frame bar, and use the etching surface on the back side as the working surface. The three-dimensional metal frame bar etches the back side of the three-dimensional metal frame bar through a half-etching process to remove excess metal material. A plurality of hollow patterns I and hollow patterns II and alignment points are arranged in an array on the back side of the three-dimensional metal frame bar to form an etching surface, and a horizontal cutting path III and a longitudinal cutting path III are designed. The alignment points are arranged on the four sides of the three-dimensional metal frame bar, the hollow pattern I and the hollow pattern II are parallel and staggered in the center of the three-dimensional metal frame bar, and are both rectangles of equal length, and the width of the hollow pattern I is greater than the width of the hollow pattern II; the hollow pattern I divides the three-dimensional metal frame bar into a plurality of block-shaped metal frame bodies, and the hollow pattern II is parallel to the hollow pattern I to further divide the metal frame body into a plurality of strip-shaped metal frame support bars, and the hollow pattern II divides the metal frame body into a number of metal frame support bars;

[0013] Metal pins are formed on both ends of the etched surface of the metal frame support bar, and the metal pins are located inside the long sides of the hollow pattern I and the hollow pattern II;

[0014] The longitudinal cutting path III is parallel to the length direction of the hollow pattern I and cuts the hollow pattern I. The transverse cutting path III is set on the upper and lower sides of the three-dimensional metal frame bar and passes through the upper and lower ends of the hollow pattern I and the hollow pattern II to pre-cut the metal frame support bars from the three-dimensional metal frame bar one by one.

[0015] The etched surface of the metal frame support bar and the metal pins thereon together form a cavity;

[0016] Step 7: Place the front side of the new chip monomer inverted into the cavity of the three-dimensional metal frame bar in sequence, and align the points so that the metal bumps under the chip are fixedly connected to the metal frame support bar through the welding layer I to achieve circuit conduction of the chip;

[0017] Step 8: After the plastic encapsulation material is melted by a film-assisted plastic encapsulation single-sided molding process, the gap between the three-dimensional metal frame strip and the new chip monomer is filled by pressure, and the hollow pattern I and the hollow pattern II are filled, and at the same time, the welding layer II on the back of the new chip monomer and the upper surface of the metal pin are accurately exposed; the hollow pattern I and the hollow pattern II play a role in guiding the plastic encapsulation material to form a guide channel;

[0018] Step 9: Laminating a protective film with adhesive backing on the flat front surface of the three-dimensional metal frame strip through a lamination process;

[0019] Step 10: forming a conductive metal layer on the upper surface of the metal pin by sputtering, chemical deposition, printing or spraying;

[0020] Step 11: Divide the package into a plurality of chip package structure monomers along the horizontal cutting line III and the vertical cutting line III, and fold the chip upward through the metal bumps under the chip and the three-dimensional metal frame to directly connect and dissipate heat with the back of the chip and the PCB.

[0021] Furthermore, in step three, the forming process of the metal pin is as follows:

[0022] Symmetrical metal columns are formed on both ends of the etched surface of the metal frame support bar by sputtering, corrosion, chemical deposition, printing or spraying as metal pins.

[0023] Furthermore, in step three, the forming process of the metal pin is as follows:

[0024] A plurality of metal pillars of the same height are formed by photoresist patterning and metal deposition method, and the bottoms of the metal pillars are connected to the etched surfaces of the above-mentioned metal frame support bars by welding process to form metal pins.

[0025] Furthermore, in step three, the forming process of the metal pin is as follows:

[0026] Prepare a metal sheet, use a high-reflection laser to form a number of metal columns with the same height through a laser cutting process, and connect the bottom of the metal column to the etched surface of the above-mentioned metal frame support bar through a welding process to form a metal pin.

[0027] Furthermore, in step three, the forming process of the metal pin is as follows:

[0028] When the three-dimensional metal frame bar is formed, the back side of the three-dimensional metal frame bar is etched through a semi-etching process to remove excess metal material, and a plurality of hollow patterns I, hollow patterns II, alignment points and metal pins are arranged in an array on the back side of the three-dimensional metal frame bar, and a horizontal cutting path III and a longitudinal cutting path III are designed. Due to the different etching speeds, the cylindrical surface of the metal pin is a concave arc column, and its curvature R is controlled by the actual process. The metal pin and the metal frame support bar are an integrated structure.

[0029] Furthermore, the surface of the metal pin or the surface of the metal pin and the etched surface of the three-dimensional metal frame strip are roughened by a plasma etching process, and the roughness Ra is controlled in the range of Ra 0.2-0.4.

[0030] Furthermore, the welding layer I is a metal selected from titanium, copper, silver, nickel, gold, tin, and tin-silver, or a combination of several metals.

[0031] Furthermore, the cross-sectional dimension of the metal heat sink is not less than the cross-sectional dimension of the chip.

[0032] Furthermore, the cross section of the metal pin is circular, rectangular or hexagonal.

[0033] Furthermore, in step ten, the welding layer II and the conductive metal layer are formed simultaneously.

[0034] Beneficial Effects

[0035] The present invention discloses a packaging method for a packaging structure of a planar power device, provides a single-sided precise plastic sealing and low-temperature bonding protective film process, simplifies the packaging process, and compared with the traditional wire bonding method, the FC process transmission performance is improved, the interconnection structure size is short, the inductance, resistance and capacitance are reduced, the signal integrity, the radio frequency performance is better, the production efficiency is improved and the production cost is reduced; the traditional wire bonding method is avoided, and the resistance R between the chip and the lead frame is reduced. D , reducing the bond wire resistance R W , thereby achieving the purpose of reducing the on-resistance RDS (on) of the packaged product; the package structure formed by the chip is applied to the planar power device, and the metal bump under the chip on the front side of the chip is flipped onto the etched surface of the three-dimensional metal frame, and the chip and the PCB are directly connected through the metal bump under the chip and the folding of the three-dimensional metal frame, which simplifies the package structure, avoids the traditional wire bonding process, reduces the package resistance, and increases the current carrying capacity; at the same time, the interconnection distance between the chip and the outside world is shortened, and the conductive effect of the chip is enhanced; the back side of the chip is exposed, and the heat is dissipated through the close contact of the metal heat sink PCB, which improves the heat dissipation capacity of the package, improves the stability of the chip when running at high speed, and improves the quality of the product; in addition, the metal pins of the three-dimensional metal frame are concave arc columns, which enhances the bonding force between the metal pins and the plastic packaging material, and achieves the purpose of increasing product reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A flow chart of a packaging method for a packaging structure applied to a planar power device according to the present invention;

[0037] Figure 2 A schematic diagram of an embodiment of a cross-sectional structure of a packaging structure applied to a planar power device of the present invention;

[0038] Figure 3 A schematic diagram of an embodiment of a cross-sectional structure of a packaging structure applied to a planar power device of the present invention;

[0039] Figure 4 for Figure 2 A schematic diagram of the relative positions of the chip and the three-dimensional metal frame;

[0040] Figure 5A schematic diagram of a cross-sectional structure of an embodiment of a packaging structure applied to a planar power device of the present invention;

[0041] FIG. 6A to FIG. 6Q A flowchart of a process of a packaging method for a packaging structure of a planar power device according to the present invention;

[0042] Among them: Chip 10

[0043] Welding layer Ⅰ12

[0044] Welding layer Ⅱ55

[0045] Conductive circuit layer 30

[0046] Three-dimensional metal frame 20

[0047] Metal frame support strip 21

[0048] Cavity 26

[0049] Metal heat sink 50

[0050] Cutting Road Ⅱ57

[0051] Conductive metal layer 61

[0052] Plastic packaging material 90;

[0053] Wafer 100

[0054] Cutting channel Ⅰ110

[0055] Three-dimensional metal frame bar 200

[0056] Horizontal cutting channel Ⅲ210

[0057] Longitudinal cutting channel Ⅲ230

[0058] Counterpoint 250

[0059] Metal conductive heat dissipation original plate 400. DETAILED DESCRIPTION

[0060] The present application will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should also be noted that, for ease of description, only the parts related to the relevant invention are shown in the accompanying drawings.

[0061] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0062] The present invention is a flow chart of a packaging method for a packaging structure of a planar power device, as shown in FIG. Figure 1 As shown:

[0063] Step S1: preparing incoming wafers;

[0064] Step S2: using a dicing process to cut the wafer into a plurality of independent chips;

[0065] Step S3: preparing a metal original plate;

[0066] Step S4: The back side of the chip is fixedly connected to the metal original plate through silver paste in sequence;

[0067] Step S5: cutting the original metal plate to form a new chip unit;

[0068] Step S6: preparing a three-dimensional metal frame bar, forming a metal frame support bar by a half-etching process, and forming metal pins at both ends of the etched surface of the metal frame support bar to form a cavity;

[0069] Step S7: sequentially flip the front side of the new chip monomer into the cavity of the three-dimensional metal frame strip;

[0070] Step S8: plastic-sealing the three-dimensional metal frame strip and the new chip unit by a film-assisted plastic-sealing single-sided molding process;

[0071] Step S9: laminating a protective film on the front surface of the three-dimensional metal frame strip through a lamination process;

[0072] Step S10: forming a conductive metal layer on the upper surface of the metal pin by sputtering, chemical deposition, printing or spraying;

[0073] Step S11: dividing the package body into a plurality of package structure units.

[0074] The examples are as follows:

[0075] The present invention provides a packaging structure for a planar power device, such as Figures 2 to 5 As shown, the front side of the chip 10 is provided with a plurality of metal bumps 11 under the chip, one end of the metal bump 11 under the chip is connected to the electrode of the chip 10 (the electrode is not shown in the figure), and the electrode of the chip 10 is buried in the silicon base 13 under the passivation layer on the surface of the chip; the other end of the metal bump 11 under the chip is provided with a welding layer I12, which becomes the I / O end of the chip 10.

[0076] The metal heat sink 50 has a metal surface I51 on one side and a metal surface II52 on the other side. The back side of the chip 10 is fixedly connected to the metal surface I51 of the metal heat sink 50 through silver paste 53 to form a new chip monomer 30. The metal surface II52 forms a welding layer II55 through an electroplating process.

[0077] The cross-sectional dimension of the metal heat sink 50 is not less than the cross-sectional dimension of the chip 10, and its material is preferably copper with excellent conductive properties. The metal heat sink 50 is arranged on the back of the chip 10, and the chip 10 is closely connected to the PCB for heat dissipation, thereby improving the heat dissipation capacity of the package, improving the quality of the product, and achieving excellent heat dissipation performance of the packaged product.

[0078] The three-dimensional metal frame 20 includes a plurality of metal frame support bars 21 and a plurality of metal pins 22. The back of the metal frame support bars 21 is an etched surface, and the metal pins 22 are arranged at both ends of the etched surface of each metal frame support bar 21. The cross section of the metal pins 22 is circular, rectangular, hexagonal, etc. Figure 3 The cross section of the metal pin 22 is shown as a rectangle. The etched surface of the metal frame support bar 21 and the inner side of the metal pin 22 form a cavity 26.

[0079] The front side of the new chip unit 30 is flipped into the cavity 26 through the solder layer I12 of the chip 10, and the metal bump 11 under the chip is fixedly connected to the etched surface of the metal frame support bar 21 through the solder layer I12, and is electrically connected to the three-dimensional metal frame 20. The etched surface of the metal frame support bar 21 is a rough surface, and its roughness contributes to the connection strength between it and the chip 10.

[0080] In an optional embodiment, the metal pin 22 and the metal frame support bar 21 are an integrated structure, such as Figure 2 shown.

[0081] The chip 10 is directly connected to the PCB by the metal bump 11 under the chip and the folding of the three-dimensional metal frame 20, and the chip 10 is efficiently cooled by the metal heat sink 50 and the PCB, which shortens the distance between the chip 10 and the outside world, enhances the conductive effect of the chip, avoids the use of traditional wire bonding, and reduces the resistance R between the chip drain and the lead frame. D , reducing the bond wire resistance R W , thereby achieving the purpose of reducing the on-resistance RDS (on) of the packaged product.

[0082] The front of the three-dimensional metal frame 20 is a flat exposed surface, and a protective film 40 with adhesive backing is provided, such as Adwill LC tape. The protective film 40 has a uniform thickness and is attached to the front of the three-dimensional metal frame 20 through a lamination process. It can be carried out at a relatively low temperature, and is easy to install, thereby reducing the risk of damage to the circuit due to heat. It can protect the chip from external solvents, moisture, impact, etc., and at the same time, electrically insulate the chip from the external environment. It can also block light to minimize the impact of light on the circuit surface.

[0083] The plastic encapsulation material 90 fills and encapsulates the three-dimensional metal frame 20 and the chip 10 as a whole, leaving only the etched surface 221 of the metal heat sink 50 and the metal pin exposed. The plastic encapsulation material 90 arranged between the chip 10 and its metal heat sink 50 and the metal pin 22 can effectively prevent short circuits caused by voltage breakdown, thereby improving product reliability.

[0084] In an optional embodiment, the metal pin 22 is in a concave arc column shape, and its curvature R is generated during the half-etching process of the three-dimensional metal frame 20 due to the difference in etching rate, such as Figure 4 As shown, by controlling the half-etching process to obtain the actually required arc R, the bonding force between the metal pin 22 and the plastic packaging material 90 can also be increased, thereby achieving the purpose of increasing product reliability.

[0085] In an optional embodiment, the cylindrical surface of the metal pin 22 may also be a rough surface with a roughness Ra ranging from Ra 0.2 to 0.4, which may also increase the bonding force between the metal pin 22 and the plastic packaging material 90 to achieve the purpose of increasing product reliability.

[0086] In an optional embodiment, the plastic packaging material 90 may also be exposed on both sides of the metal frame support bar 21, such as Figure 5 shown.

[0087] In an optional embodiment, a new packaging structure for planar power devices of the present invention further includes a conductive metal layer 26, which is disposed on an etched surface 221 of the metal pin to facilitate electrical connection with other external devices and heat dissipation.

[0088] The present invention provides a packaging method for a packaging structure of a planar power device, such as Figures 6A to 6Q As shown, the process is as follows:

[0089] Step 1: Fig. 6A and Figure 6B As shown, the incoming wafer 100 is prepared, and qualified wafers are selected through the incoming material inspection process, and a cleaning process is performed to remove dust, oil, etc. There are neatly arranged horizontal and vertical cutting lanes Ⅰ110 on the wafer 100. The cutting lanes Ⅰ110 pre-divide the wafer 100 into a plurality of chips 10. The front of each chip 10 is provided with a plurality of under-chip metal bumps 11. The under-chip metal bumps 11 correspond to the electrodes of the chip 10 (the electrodes are not shown in the figure). The electrodes of the chip 10 are buried in the silicon base 13 under the passivation layer on the surface of the chip. One end of each under-chip metal bump 11 corresponds to the electrode of the chip 10, and the other end is provided with a welding layer Ⅰ12.

[0090] Step 2: Figure 6C and Fig.6DAs shown, a dicing process is used to dicing the wafer 100 along dicing lanes I 110 to form a plurality of independent chips 10. Fig.6D It is a front view of the chip, showing the metal bumps 11 under the chip in a 3*5 array.

[0091] Step 3: Fig. 6E and 6F As shown, a metal original plate 500 is prepared, and its material is preferably copper with excellent conductive properties. It includes a metal surface Ⅰ51 on the upper surface and a metal surface Ⅱ52 on the lower surface. The metal surface Ⅱ52 is formed into a welding layer Ⅱ55 through an electroplating process. The solder used for the welding layer Ⅱ55 can be one metal or a combination of several metals selected from titanium, copper, silver, nickel, gold, tin, and tin-silver. The welding layer Ⅱ55 covers the metal surface Ⅱ52 to prevent metal oxidation.

[0092] Step 4: Figure 6G As shown, the back side of the chip 10 is fixedly connected to the metal surface I51 of the metal original plate 500 through the silver paste 53 in sequence, and the chips 10 are arranged in an array with spaces between them, leaving a cutting path II57 on the metal original plate 500;

[0093] Step 5: Figure 6H As shown, the metal original plate 500 is cut along the cutting line II 57 to form a new chip monomer 30 , and the metal original plate 500 forms the metal heat sink 50 on the back side of the chip 10 ;

[0094] Step 6: Fig.6I , Figure 6J and Figure 6K As shown, a three-dimensional metal frame bar 200 is prepared. The material of the three-dimensional metal frame bar 200 is selected with reference to the lead frame of the chip carrier used for integrated circuits, and the etching surface on the back side is used as the working surface. Fig.6I is a top view of the back side of the three-dimensional metal frame bar 200, Figure 6J and Figure 6K for Fig.6IIn the BB cross-sectional view, the three-dimensional metal frame bar 200 is etched on the back of the three-dimensional metal frame bar 200 by a half-etching process to remove the excess metal material, and a plurality of hollow patterns I221 and hollow patterns II222 and alignment points 250 are arranged in an array on the back of the three-dimensional metal frame bar 200 to form an etching surface, and a horizontal cutting path III210 and a vertical cutting path III230 are designed. The alignment points 250 are arranged on the four sides of the three-dimensional metal frame bar 200, the hollow patterns I221 and the hollow patterns II222 are parallel and staggered in the center of the three-dimensional metal frame bar 200, and are both equal-length rectangles, and the width of the hollow pattern I221 is greater than the width of the hollow pattern II222. The hollow pattern I 221 divides the three-dimensional metal frame bar 200 into a plurality of block-shaped metal frame bodies, and the hollow pattern II 222 is parallel to the hollow pattern I 221 and further divides the metal frame body into a plurality of strip-shaped metal frame support bars 21. Fig.6I In the figure, four hollow patterns II 222 are arranged between adjacent hollow patterns I 221, and the hollow patterns II 222 divide the metal frame body into five metal frame support bars 21. Symmetrical metal columns are formed on both ends of the etched surface of the metal frame support bar 21 by sputtering, corrosion, chemical deposition, printing or spraying in sequence as metal pins 22, and the metal pins 22 are located inside the long sides of the hollow patterns I 221 and the hollow patterns II 222 to avoid the transverse cutting path III 210 so that the metal pins 22 are not damaged.

[0095] The longitudinal cutting road III230 cuts the hollow pattern I221 in parallel with the length direction of the hollow pattern I221. Generally, the longitudinal cutting road III230 coincides with the center line of the hollow pattern I221. For the outermost hollow pattern I221, the longitudinal cutting road III230 only cuts off a part of the hollow pattern I221 along the length direction of the hollow pattern I221.

[0096] The transverse cutting path III 210 is set on the upper and lower sides of the three-dimensional metal frame bar 200 and passes through the upper and lower ends of the hollow pattern I 221 and the hollow pattern II 222 to pre-cut the metal frame support bars 21 from the three-dimensional metal frame bar 200 one by one.

[0097] The etched surfaces of the five metal frame support bars 21 and the metal pins 22 thereon together form a cavity 26, such as Figure 6J As shown;

[0098] Alternatively, when the three-dimensional metal frame bar 200 is formed, the raw material of the three-dimensional metal frame bar 200 is removed from the excess metal material through a semi-etching process, and the above-mentioned array-arranged multiple hollow patterns I221 and hollow patterns II222, alignment points 250 and metal pins 22 are formed on the etched surface, and a horizontal cutting path III210 and a longitudinal cutting path III230 are designed. Due to the different etching speeds, the cylindrical surface of the metal pin 22 is a concave arc column, and its curvature R is controlled by the actual process. The metal pin 22 and the metal frame support bar 21 are an integrated structure, and the five metal frame support bars 21 and the metal pins 22 thereon together constitute a cavity 26, such as Figure 6K shown.

[0099] Alternatively, a plurality of metal pillars of the same height are formed by photoresist patterning and metal deposition, and the bottoms of the metal pillars are connected to the etched surfaces of the metal frame support bars 21 by welding to form metal pins 22. The solder used for welding can be one of the metals selected from titanium, copper, silver, nickel, gold, tin, and tin-silver, or a combination of several metals.

[0100] Alternatively, prepare a metal sheet, use a high-reflection laser to form several metal columns of the same height through a laser cutting process, and connect the bottom of the metal column to the etched surface of the above-mentioned metal frame support bar 21 through a welding process to form a metal pin 22. The solder used for welding can be one of titanium, copper, silver, nickel, gold, tin, tin-silver, or a combination of several of them.

[0101] In this step, the surface of the metal pin 22 or the surface of the metal pin 22 and the etched surface of the three-dimensional metal frame bar 200 may be roughened by plasma etching process, and the roughness Ra is controlled in the range of Ra 0.2-0.4.

[0102] Step 7: Figure 6L and 6M As shown, the front side of the new chip monomer 30 is flipped and placed into the cavity 26 of the three-dimensional metal frame bar 200 in sequence, and the metal bump 11 under the chip is fixedly connected to the metal frame support bar 21 through the welding layer Ⅰ12 to achieve circuit conduction of the chip 10. The solder used in the welding layer Ⅰ12 can be one metal selected from titanium, copper, silver, nickel, gold, tin, tin-silver, or a combination of several metals. Figure 6L is a schematic diagram of the relative positions of the three-dimensional metal frame bar 200 and the chip 10, Figure 6M for Figure 6L CC cross-section diagram.

[0103] Step 8: Figure 6NAs shown, after the plastic encapsulation material 90 is melted by the film-assisted plastic encapsulation single-sided molding process (FAM), the gap between the three-dimensional metal frame bar 200 and the new chip monomer 30 is filled by pressure, and the hollow pattern I 221 and the hollow pattern II 222 are filled, and the welding layer II 55 on the back of the new chip monomer 30 and the upper surface 221 of the metal pin are accurately exposed. The hollow pattern I 221 and the hollow pattern II 222 play a role in guiding the plastic encapsulation material 90 to form a guiding channel.

[0104] Step 9: Fig.6O As shown, at a relatively low temperature, a protective film 70 with adhesive backing, such as Adwill LC tape, is attached to the flat front side of the three-dimensional metal frame strip 200 through a lamination process, which is easy to install, thereby reducing the risk of circuit damage due to heat and simplifying the traditional EMC process.

[0105] Step 10: Figure 6P As shown, a conductive metal layer 61 is formed on the upper surface 221 of the metal pin by sputtering, chemical deposition, printing or spraying, and the conductive metal layer 61 is used for subsequent mounting of the packaged chip. The welding layer II 55 can also be formed at the same time as the conductive metal layer 61 in this step. Generally, the welding layer II 55 is required to be flush with the conductive metal layer 61.

[0106] Step 11: Figure 6Q As shown, the above-mentioned package body is divided into a package structure monomer of a plurality of chips along the horizontal cutting road III210 and the vertical cutting road III230, and the chip 10 is folded upward through the metal bump 11 under the chip and the three-dimensional metal frame 20 to be directly interconnected with the back side of the chip 10 and the PCB, and the chip 10 is directly and efficiently cooled through the metal heat sink 50 and the PCB.

[0107] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the embodiments of the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A packaging method for a packaging structure of a planar power device, the process method of which is as follows: Step 1, preparing an incoming wafer (100), on which neatly arranged horizontal and vertical intersecting cutting paths I (110), the cutting paths I (110) pre-dividing the wafer (100) into a plurality of chips (10), each chip (10) being provided with a plurality of under-chip metal bumps (11) on the front side, one end of the under-chip metal bump (11) corresponding to the electrode of the chip (10), and the other end being provided with a welding layer I (12); Step 2: using a cutting process to cut the wafer (100) along the cutting path I (110) to form a plurality of independent chips (10); Step 3: prepare a metal original plate (500) made of copper, including a metal surface I (51) on the upper surface and a metal surface II (52) on the lower surface, wherein the metal surface II (52) is electroplated to form a welding layer II (55); Step 4: The back side of the chip (10) is fixedly connected to the metal surface I (51) of the metal original plate (500) through silver paste (53) in sequence, and the chips (10) are arranged in an array with spaces between them, leaving a cutting path II (57) on the metal original plate (500); Step 5: cutting the metal original plate (500) along the cutting path II (57) to form a new chip monomer (30); the metal original plate (500) forms a metal heat sink (50) on the back side of the chip (10); Step 6: Prepare a three-dimensional metal frame bar (200), with the etching surface on the back thereof serving as a working surface. The three-dimensional metal frame bar (200) is etched on the back of the three-dimensional metal frame bar (200) by a half-etching process to remove excess metal material. A plurality of hollow patterns I (221) and hollow patterns II (222) and alignment points (250) are arrayed on the back of the three-dimensional metal frame bar (200) to form an etching surface, and a horizontal cutting path III (210) and a vertical cutting path III (230) are designed. The alignment points (250) are arranged on four sides of the three-dimensional metal frame bar (200) at the top, bottom, left and right sides. The hollow pattern I (221) and the hollow pattern II (222) are parallel and staggeredly distributed in the center of the three-dimensional metal frame bar (200), both of which are rectangular with equal length, and the width of the hollow pattern I (221) is greater than the width of the hollow pattern II (222); the hollow pattern I (221) divides the three-dimensional metal frame bar (200) into a plurality of block-shaped metal frame bodies, and the hollow pattern II (222) is parallel to the hollow pattern I (221) and further divides the metal frame body into a plurality of strip-shaped metal frame support bars (21), and the hollow pattern II (222) divides the metal frame body into a plurality of metal frame support bars (21); Metal pins (22) are formed on both ends of the etched surface of the metal frame support bar (21), and the metal pins (22) are located inside the long sides of the hollow pattern I (221) and the hollow pattern II (222); The longitudinal cutting path III (230) cuts the hollow pattern I (221) in parallel with the length direction of the hollow pattern I (221); the transverse cutting path III (210) is arranged on the upper and lower sides of the three-dimensional metal frame strip (200) and passes through the upper and lower ends of the hollow pattern I (221) and the hollow pattern II (222), so as to pre-cut the metal frame support strips (21) from the three-dimensional metal frame strip (200) one by one; The etched surface of the metal frame support bar (21) and the metal pins (22) thereon together form a cavity (26); Step 7, sequentially placing the front side of the new chip monomer (30) invertedly into the cavity (26) of the three-dimensional metal frame bar (200), aligning the metal bumps (11) under the chip through the welding layer I (12) and correspondingly connecting the metal frame support bar (21), thereby achieving circuit conduction of the chip (10); Step 8: After the plastic encapsulation material (90) is melted by a film-assisted plastic encapsulation single-sided molding process, the gap between the three-dimensional metal frame strip (200) and the new chip monomer (30) is filled by pressure, and the hollow pattern I (221) and the hollow pattern II (222) are filled, and at the same time, the welding layer II (55) on the back of the new chip monomer (30) and the upper surface (221) of the metal pin are accurately exposed; the hollow pattern I (221) and the hollow pattern II (222) play a role in guiding the plastic encapsulation material (90) to form a guiding channel; Step nine: laminating a protective film (70) with adhesive backing onto the flat front surface of the three-dimensional metal frame strip (200) through a lamination process; Step 10: forming a conductive metal layer (61) on the upper surface (221) of the metal pin by sputtering, chemical deposition, printing or spraying; Step 11: Divide the package into a plurality of chip package structure monomers along the horizontal cutting line III (210) and the vertical cutting line III (230), and fold the chip (10) upward through the metal bump (11) under the chip and the three-dimensional metal frame (20) to directly connect and dissipate heat with the back side of the chip (10) and the PCB.

2. The packaging method according to claim 1, characterized in that: In step 3, the forming process of the metal pin (22) is as follows: Symmetrical metal columns are formed on both ends of the etched surface of the metal frame support bar (21) in sequence by sputtering, corrosion, chemical deposition, printing or spraying to serve as metal pins (22).

3. The packaging method according to claim 1, characterized in that: In step 3, the forming process of the metal pin (22) is as follows: A plurality of metal columns of the same height are formed by photoresist patterning and metal deposition, and the bottoms of the metal columns are connected to the etched surfaces of the metal frame support bars (21) by welding processes to form metal pins (22).

4. The packaging method according to claim 1, characterized in that: In step 3, the forming process of the metal pin (22) is as follows: A metal sheet is prepared, and a high-reflection laser is used to form a plurality of metal columns of the same height through a laser cutting process, and the bottom of the metal column is connected to the etched surface of the metal frame support bar (21) through a welding process to form a metal pin (22).

5. The packaging method according to claim 1, characterized in that: In step 3, the forming process of the metal pin (22) is as follows: When the three-dimensional metal frame bar (200) is formed, the three-dimensional metal frame bar (200) is etched on the back side of the three-dimensional metal frame bar (200) through a half-etching process to remove excess metal material, and a plurality of hollow patterns I (221), hollow patterns II (222), alignment points (250) and metal pins (22) are arranged in an array on the back side of the three-dimensional metal frame bar (200), and a transverse cutting path III (210) and a longitudinal cutting path III (230) are designed. Due to different etching speeds, the cylindrical surface of the metal pin (22) is in the shape of a concave arc column, and its curvature R is controlled by the actual process. The metal pin (22) and the metal frame support bar (21) are an integral structure.

6. The packaging method according to any one of claims 1 to 5, characterized in that: The surface of the metal pin (22) or the surface of the metal pin (22) and the etched surface of the three-dimensional metal frame bar (200) are roughened by a plasma etching process, and the roughness Ra is controlled in the range of Ra 0.2-0.

4.

7. The packaging method according to claim 1, characterized in that: The welding layer I (12) is a metal selected from the group consisting of titanium, copper, silver, nickel, gold, tin, and tin-silver, or a combination of several metals.

8. The packaging method according to claim 1, characterized in that: The cross-sectional dimension of the metal heat sink (50) is not less than the cross-sectional dimension of the chip (10).

9. The packaging method according to claim 1, characterized in that: The cross section of the metal pin (22) is circular, rectangular or hexagonal.

10. The packaging method according to claim 1, characterized in that: Step ten: the welding layer II (55) and the conductive metal layer (61) are formed simultaneously.