A method for preparing carbon nanotube-doped electrolytic copper foil

Through the purification, sensitization, activation and electroless plating of carbon nanotubes, the problems of uneven thickness and insufficient mechanical properties of electrolytic copper foil are solved, the mechanical and electrical properties of electrolytic copper foil are improved, and the safety of lithium batteries is ensured. and performance.

CN115295750BActive Publication Date: 2024-10-11NANCHANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211036785.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-10-11
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

The existing electrolytic copper foil has uneven thickness and insufficient mechanical properties during the thinning process, which makes lithium batteries prone to corrosion, breakdown and explosion during electrochemical reactions. Moreover, the purity of carbon nanotubes in the electrolyte is not high and the deposition efficiency is low. , limiting its application in the field of electrolytic copper foil.

Method used

Through the purification, sensitization, activation and electroless plating of carbon nanotubes, impurities are removed and their electromigration rate and deposition efficiency are improved, preventing excessive deposition of copper ions on their surface, and controlling the current density during the electrodeposition process to prepare uniform nanotubes. of carbon nanotubes doped copper foil.

Benefits of technology

It improves the precipitation efficiency of carbon nanotubes in the electrolyte and the mechanical and electrical properties of the copper foil, ensures the thickness uniformity and quality of the copper foil, reduces the resistance, and enhances the capacity and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115295750B_ABST
    Figure CN115295750B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing carbon nanotube-doped electrolytic copper foil, comprising the following steps: (1) carbon nanotube purification treatment; (2) carbon nanotube sensitization treatment; (3) carbon nanotube activation treatment; (4) chemical deposition of copper on the surface of carbon nanotubes; (5) preparation of carbon nanotube-doped copper foil by electrodeposition. The present invention can keep the original structure of carbon nanotubes intact and efficiently remove impurities in carbon nanotubes; reduce the agglomeration of carbon nanotubes in electrolyte and copper foil; improve the migration rate of carbon nanotubes in electrolyte and the precipitation efficiency on cathode; the prepared copper foil has good mechanical properties and electrical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytic copper foil preparation, and in particular to a method for preparing electrolytic copper foil for carbon nanotube-doped lithium batteries. Background Art

[0002] Electrolytic copper foil is an important material for manufacturing negative electrode current collectors, copper-clad laminates and printed circuit boards for lithium-ion batteries. In today's "dual carbon" era, new energy vehicles are booming, and the market demand for lithium batteries is increasing. As lithium batteries develop towards "high power, high energy storage, and light weight", the current market generally produces and uses 4-12 micron double-sided photoelectrolytic copper foil as a negative electrode current collector material for lithium batteries, and the thickness of electrolytic copper foil is getting thinner and thinner. Thinning will bring about problems such as uneven thickness of electrolytic copper foil and weakened mechanical properties: uneven thickness of copper foil affects the coating quality of negative electrode active materials, and local corrosion is prone to occur during the electrochemical reaction process, and the battery is easily punctured and exploded; copper foil has low tensile properties and elongation, and is prone to splitting during the rolling process or high-power rapid charging and discharging, affecting battery capacity, and even causing battery breakdown, combustion and explosion. It is of great significance to improve or seek new ultra-thin, high-performance, and high-capacitance electrolytic copper foil preparation processes.

[0003] The invention patent with application number CN201780026112.6 discloses an electrolytic copper foil for graphene synthesis and a method for preparing the graphene-doped electrolytic copper foil. By adding nickel to promote graphene synthesis, graphene can be evenly distributed on the surface of the copper foil. The thickness of the copper foil is 4-70 microns; the room temperature tensile strength is 45-70Kgf / mm 2 ; High temperature tensile strength reaches 20-35Kgf / mm 2 .

[0004] The electrical properties of graphene are more than 100 times that of copper; the speed of electrons in graphene is more than 100 times faster than that of single-crystal silicon; the strength of graphene is 200 times greater than that of steel; the thermal conductivity of graphene is 2 times higher than that of diamond, which has the highest thermal conductivity; and the excellent elasticity of graphene means that it will not lose its electrical properties when stretched or bent. Carbon nanotubes are superior to graphene in terms of electrical conductivity, thermal conductivity, strength, toughness and stability. Carbon nanotubes can be regarded as a cylinder made of a hexagonal periodic arrangement of graphite sheets, with a tube diameter of about 100nm and an axial dimension of the micrometer order. It is a typical one-dimensional quantum material and is considered to be the most promising reinforcement material at present.

[0005] By utilizing the excellent electrical and mechanical properties of carbon nanotubes, as a reinforcing phase doping into electrolytic copper foil, the capacitance of electrolytic copper foil can be increased, the resistance of copper foil can be reduced, and the mechanical properties of copper foil can be increased. However, due to the low purity of carbon nanotubes themselves, they are easy to agglomerate and stratify in the electrolyte, have a low migration rate, and have low deposition and precipitation efficiency; and during the electrodeposition process, copper ions will preferentially nucleate and deposit on the surface of carbon nanotubes, which can easily cause problems such as uneven thickness of copper foil, which seriously restricts the application of carbon nanotubes in the field of electrolytic copper foil. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing carbon nanotube-doped electrolytic copper foil around the solution of the above bottleneck problem. On the one hand, impurities in carbon nanotubes are removed through a "purification" process. On the other hand, a "sensitization-activation-chemical plating" process is used to coat some nucleation points on the surface of carbon nanotubes to prevent the transitional deposition of copper ions on their surface; at the same time, metal ion complexes will be adsorbed on the surface of carbon nanotubes to improve the electrical migration rate and electrodeposition efficiency of carbon nanotubes.

[0007] To achieve the above object, the present invention is implemented by the following technical steps:

[0008] (1) Purification of carbon nanotubes: First, prepare a mixed acid solution of concentrated nitric acid and concentrated sulfuric acid at a volume ratio of 1:3; then add 5-15 g / L of carbon nanotubes to the mixed acid solution; stir magnetically or oscillate ultrasonically at 50-80°C for 5-8 hours; filter, rinse with deionized water until neutral, and then vacuum dry or freeze-dry.

[0009] (2) Sensitization of carbon nanotubes. First, dilute concentrated hydrochloric acid with deionized water at a volume ratio of 1:15-20; then add 15-25 g / L of SnCl2 to the diluted hydrochloric acid solution and stir evenly; then add 5-10 g / L of purified carbon nanotubes to the above prepared solution; stir magnetically or ultrasonically oscillate at 50-60°C for 0.5-1h; filter, rinse with deionized water until neutral, and then vacuum dry or freeze-dry.

[0010] (3) Activation of carbon nanotubes. First, dilute concentrated hydrochloric acid with deionized water at a volume ratio of 1:20-25; then add PdCl2 at 5-20 g / L to the diluted hydrochloric acid solution and stir evenly; then add sensitized carbon nanotubes at 5-10 g / L to the above prepared solution; stir magnetically or ultrasonically oscillate at 50-60°C for 0.5-1h; filter, rinse with deionized water until neutral, and then vacuum dry or freeze-dry.

[0011] (4) Chemical deposition of copper on the surface of carbon nanotubes. Dissolve EDTA-CuNa2 in deionized water at 13-50 g / L; then add NaOH at 15-20 g / L to control the pH value at 9-13; then add 0.5-3 g / L of activated carbon nanotubes to the above prepared solution; then add formaldehyde at 15-30 mL / L; first stir magnetically or ultrasonically oscillate for 2 minutes at 50-60°C, then let stand for 3-5 minutes and then stir for 1-2 minutes, the reaction time is 10-30 minutes; filter, rinse with deionized water until neutral, and then vacuum dry or freeze dry.

[0012] (5) Preparation of carbon nanotube-doped copper foil by electrodeposition. First, prepare the electrolyte: Cu 2+ The concentration is 30-60g / L; a mixture of SPS (sodium polydisulfide propane sulfonate) and MPS (sodium 3-mercapto-1-propane sulfonate) is 1-15mg / L; chloride ions are 10-35mg / L; concentrated sulfuric acid is 70-100g / L. Then, 25-200mg / L of carbon nanotubes surface-modified in steps (1) to (4) are added to the above electrolyte, and after continuous stirring at 60°C for 0.5-1h, the current density is controlled to be 5-40A / dm 2 Electrodeposition begins, and carbon nanotube-doped copper foil is prepared on the cathode surface. The copper foil is peeled off from the cathode, and the surface is treated with anti-oxidation, cleaned, and dried.

[0013] Furthermore, in step (1), the carbon nanotubes are 10-12 g / L; the temperature is 60-70° C.; and the time is 5-6 h.

[0014] Furthermore, in step (2), SnCl2 is 18-23 g / L; carbon nanotubes are 5-7 g / L; and the time is 30-40 min.

[0015] Furthermore, in step (3), PdCl2 is 16-20 g / L; carbon nanotubes are 5-7 g / L; and the time is 30-40 min.

[0016] Furthermore, in step (4), EDTA-CuNa2 is 22-32 g / L, Cu 2+ The concentration is 3-4.6 g / L; carbon nanotubes are 1-1.5 g / L; the pH value is 10-11; and the time is 15-20 min.

[0017] Furthermore, in step (5), Cu 2+ Concentration is 30-45g / L; SPS+MPS mixture is 5-10mg / L; chloride ion is 20-25mg / L; concentrated sulfuric acid is 70-80g / L; modified carbon nanotubes is 50-100mg / L; current density is 5-25A / dm 2 .

[0018] The beneficial effects of the present invention are:

[0019] The present invention can keep the original structure of carbon nanotubes intact and efficiently remove impurities in carbon nanotubes; reduce the agglomeration of carbon nanotubes in electrolyte and copper foil; improve the migration rate of carbon nanotubes in electrolyte and the precipitation efficiency on the cathode; the prepared copper foil has good mechanical properties and electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The SEM images of the copper foil obtained in Comparative Example 1 are as follows; (a) agglomeration of carbon nanotubes; (b) abnormal and coarse growth of copper particles on the surface of carbon nanotubes;

[0021] Figure 2 The scanning electron microscope images of the copper foil obtained in Example 1; (a) and (b) are different regions;

[0022] Figure 3 The following are scanning electron microscope images of the copper foil obtained in Example 2; (a) and (b) are different regions. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with specific examples, which are only preferred embodiments of the present invention and are not intended to limit the present invention. Other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.

[0024] The reagents described in the present invention are all commercially available products, wherein the carbon nanotubes are multi-walled carbon nanotubes with a purity greater than 95.0%; the purity of copper sulfate pentahydrate is not less than 99.9%; the purity of sodium hydroxide is not less than 96.0%; the purity of sodium copper ethylenediaminetetraacetate is not less than 99.0%, and the copper content is ≥14.5%; the purity of stannous chloride is not less than 98.0%; the purity of concentrated hydrochloric acid is 36.0-38.0%; the purity of palladium chloride is 99.0%; the purity of concentrated sulfuric acid is not less than 99.0%; the purity of concentrated nitric acid is not less than 65.0%. A pure titanium plate is used as a cathode, and a copper plate with a purity of 99.9% is used as an anode.

[0025] The ICP4562 method was used to measure the thickness of the copper foil, the ICP-TM-650 method was used to test the tensile strength and elongation of the copper foil, and the double-arm bridge method was used to measure the resistance of the copper foil.

[0026] Comparative Example 1:

[0027] The carbon nanotubes were not purified or surface treated. The electrolyte was prepared by adding 120g CuSO4·5H2O, 200mg polyacrylic acid (3000), 55mg concentrated hydrochloric acid, and 70g concentrated sulfuric acid into deionized water and heating to dissolve, and finally calibrated to 1000mL; 200mg of the original carbon nanotubes were added into the above electrolyte, and after continuous stirring at 60℃ for 1h, the current density was controlled to be 5A / dm 2 Electrodeposition was started to prepare a 12 μm thick copper foil. The copper foil was peeled off from the cathode, and the surface was treated for oxidation resistance, cleaned, and dried. The SEM image of the copper foil obtained is shown below: Figure 1 shown.

[0028] Embodiment 1:

[0029] (1) Purification of carbon nanotubes: prepare 250 mL of a mixed acid solution of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3; add 2.5 g of original carbon nanotubes to the mixed acid solution; stir magnetically at 60° C. for 6 h; filter, rinse with deionized water until neutral, and then vacuum dry.

[0030] (2) Sensitization of carbon nanotubes: dilute concentrated hydrochloric acid to 400 mL at a volume ratio of 1:20; add 8 g of SnCl2 to the diluted hydrochloric acid solution and stir evenly; then add 2 g of purified carbon nanotubes to the above prepared solution; stir magnetically at 60°C for 0.5 h; filter, rinse with deionized water until neutral, and then vacuum dry.

[0031] (3) Activation of carbon nanotubes: dilute concentrated hydrochloric acid to 300 mL at a volume ratio of 1:20; add 6 g of PdCl2 to the diluted hydrochloric acid solution and stir evenly; then add 1.5 g of sensitized carbon nanotubes to the above prepared solution; stir magnetically at 60°C for 0.5 h; filter, rinse with deionized water until neutral, and then vacuum dry.

[0032] (4) Chemical deposition of copper on the surface of carbon nanotubes: 25 g of EDTA-CuNa2 and 15 g of NaOH were added to 1000 mL of deionized water to dissolve, and the pH value was controlled at 10; 1-1.3 g of activated carbon nanotubes were added to the above prepared solution; 20 mL of formaldehyde was added; the mixture was allowed to stand for 3 min at 60°C and then magnetically stirred for 2 min, with a reaction time of 15 min; the mixture was filtered, rinsed with deionized water until neutral, and then dried in a vacuum.

[0033] (5) Preparation of carbon nanotube-doped copper foil by electrodeposition. 120 g of CuSO4·5H2O, 5 mg of SPS+MPS mixture, 55 mg of concentrated hydrochloric acid, and 70 g of concentrated sulfuric acid were added to deionized water and heated to dissolve, and finally calibrated to 1000 mL; 50 mg of carbon nanotubes surface-modified in steps (1)-(4) were added to the above electrolyte, stirred continuously at 60°C for 1 h, and the current density was controlled to 5 A / dm 2 Electrodeposition was started to prepare a 12 μm thick copper foil. The copper foil was peeled off from the cathode, and the surface was treated for oxidation resistance, cleaned, and dried. The SEM image of the copper foil obtained is shown below: Figure 2 shown.

[0034] Embodiment 2:

[0035] (1) Purification of carbon nanotubes: prepare 200 mL of a mixed acid solution of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3; add 3 g of original carbon nanotubes into the mixed acid solution; stir magnetically at 60°C for 8 h; filter, rinse with deionized water until neutral, and then vacuum dry.

[0036] (2) Sensitization of carbon nanotubes: dilute concentrated hydrochloric acid to 350 mL at a volume ratio of 1:20; add 8 g of SnCl2 to the diluted hydrochloric acid solution and stir evenly; then add 2.5 g of purified carbon nanotubes to the above prepared solution; stir magnetically at 60°C for 40 min; filter, rinse with deionized water until neutral, and then dry in vacuum.

[0037] (3) Activation of carbon nanotubes: dilute concentrated hydrochloric acid to 300 mL at a volume ratio of 1:20; add 6 g of PdCl2 to the diluted hydrochloric acid solution and stir evenly; then add 2 g of sensitized carbon nanotubes to the above prepared solution; stir magnetically at 60°C for 40 min; filter, rinse with deionized water until neutral, and then vacuum dry.

[0038] (4) Chemical deposition of copper on the surface of carbon nanotubes: 30 g of EDTA-CuNa2 and 20 g of NaOH were added to 1000 mL of deionized water to dissolve, and the pH value was controlled at 11; 1.5 g of activated carbon nanotubes were added to the above prepared solution; 20 mL of formaldehyde was added; the mixture was allowed to stand for 3 min at 60°C and then magnetically stirred for 2 min, with a reaction time of 20 min; the mixture was filtered, rinsed with deionized water until neutral, and then dried in a vacuum.

[0039] (5) Preparation of carbon nanotube-doped copper foil by electrodeposition. 175 g of CuSO4·5H2O, 10 mg of SPS+MPS mixture, 70 mg of concentrated hydrochloric acid, and 80 g of concentrated sulfuric acid were added to deionized water and heated to dissolve, and finally calibrated to 1000 mL; 100 mg of carbon nanotubes surface-modified in steps (1)-(4) were added to the above electrolyte, stirred continuously at 60°C for 1 h, and the current density was controlled to 15 A / dm 2 Electrodeposition was started to prepare a 9 μm thick copper foil. The copper foil was peeled off from the cathode, and the surface was treated for oxidation resistance, cleaned, and dried. The SEM image of the copper foil obtained is shown below: Figure 3 shown.

[0040] From the attached Figure 1-3 According to the data in Table 1, the carbon nanotubes without surface modification are prone to agglomeration, and the copper particles on the local surface are coarse, resulting in uneven thickness distribution and increased roughness of the copper foil. The carbon nanotubes after surface modification are evenly dispersed in the copper foil, the copper particles on the surface of the carbon nanotubes are evenly deposited, the thickness of the copper foil is also uniform, the roughness also meets the product quality requirements, and the electrical and mechanical properties are improved to a certain extent.

[0041] Table 1 Performance indicators of three groups of samples

[0042]

[0043]

Claims

1. A method for preparing carbon nanotube-doped electrolytic copper foil, characterized in that: The following steps are involved: Step 1, purification of carbon nanotubes; first, prepare a mixed acid solution of concentrated nitric acid and concentrated sulfuric acid at a volume ratio of 1:3; then add 5-15 g / L of carbon nanotubes into the mixed acid solution; magnetically stir or ultrasonically oscillate at 50-80° C. for 5-8 hours; filter, rinse with deionized water until neutral, and then vacuum dry or freeze-dry; Step 2, sensitization treatment of carbon nanotubes; first dilute concentrated hydrochloric acid with deionized water at a volume ratio of 1:15-20; then add SnCl2 at 15-25g / L to the diluted hydrochloric acid solution and stir evenly; then add the purified carbon nanotubes at 5-10g / L to the prepared solution; Magnetic stirring or ultrasonic oscillation at 50-60°C for 0.5-1h; filtering, washing with deionized water until neutral, and then vacuum drying or freeze drying; Step 3, activation treatment of carbon nanotubes; first dilute concentrated hydrochloric acid with deionized water at a volume ratio of 1:20-25; then add 5-20g / L of PdCl2 to the diluted hydrochloric acid solution and stir evenly; then add 5-10g / L of sensitized carbon nanotubes to the above prepared solution; magnetically stir or ultrasonically oscillate at 50-60°C for 0.5-1h; Filter, rinse with deionized water until neutral, and then vacuum dry or freeze dry; Step 4, chemically deposit copper on the surface of carbon nanotubes; add EDTA-CuNa2 at 13-50g / L into deionized water to dissolve; then add NaOH at 15-20g / L to control the pH value at 9-13; then add 0.5-3g / L of the activated carbon nanotubes into the above-mentioned prepared solution; then add formaldehyde at 15-30mL / L; first magnetically stir or ultrasonically oscillate for 2min at 50-60°C, then let it stand for 3-5min and then stir for 1-2min, and the reaction time is 10-30min; filter, rinse with deionized water until neutral, and then vacuum dry or freeze-dry; Step 5, preparing carbon nanotube-doped copper foil by electrodeposition; first prepare the electrolyte: Cu 2+ The concentration is 30-60g / L; a mixture of sodium polydisulfide propane sulfonate and sodium 3-mercapto-1-propane sulfonate 1-15mg / L; chloride ions 10-35mg / L; concentrated sulfuric acid 70-100g / L; then the carbon nanotubes surface-modified in steps 1-4 are added to the above electrolyte at 25-200mg / L, and stirred continuously at 60°C for 0.5-1h, and the current density is controlled to be 5-40A / dm 2 Electrodeposition begins to prepare carbon nanotube-doped copper foil on the cathode surface; the copper foil is peeled off from the cathode, and surface anti-oxidation treatment, cleaning, and drying are performed.

2. The method for preparing carbon nanotube-doped electrolytic copper foil according to claim 1, characterized in that: In step 1, the carbon nanotubes are 10-12 g / L; the temperature is 60-70° C.; and the time is 5-6 h.

3. The method for preparing carbon nanotube-doped electrolytic copper foil according to claim 1, characterized in that: In step 2, SnCl2 is 18-23 g / L; carbon nanotubes are 5-7 g / L; and the time is 30-40 min.

4. The method for preparing carbon nanotube-doped electrolytic copper foil according to claim 1, characterized in that: In step 3, PdCl2 is 16-20 g / L; carbon nanotubes are 5-7 g / L; and the time is 30-40 min.

5. The method for preparing carbon nanotube-doped electrolytic copper foil according to claim 1, characterized in that: In step 4, EDTA-CuNa2 is 22-32 g / L, Cu 2+ The concentration is 3-4.6 g / L; carbon nanotubes are 1-1.5 g / L; the pH value is 10-11; and the time is 15-20 min.

6. The method for preparing carbon nanotube-doped electrolytic copper foil according to claim 1, characterized in that: Step 5 Cu 2+ The concentration is 30-45 g / L; the mixture of sodium polydisulfide propane sulfonate and sodium 3-mercapto-1-propane sulfonate is 5-10 mg / L; chloride ions are 20-25 mg / L; concentrated sulfuric acid is 70-80 g / L; modified carbon nanotubes are 50-100 mg / L; the current density is 5-25 A / dm 2 .

Citation Information

Patent Citations

  • Electrolytic copper foil for graphene and method for producing former

    CN109072466A

  • Preparation method of lithium ion battery based on porous copper current collector

    CN109817988A

  • Method for preparing an electrode comprising a substrate, aligned carbon nanotubes and a metal oxide deposited by oxidative deposition, the electrode and uses thereof

    US20200286690A1