A three-dimensional porous carbon-supported Fe single-atom catalyst and its preparation method and application
By using Fe single-atom catalyst based on three-dimensional porous carbon load in zinc air batteries, the problem of slow kinetics of cathode oxygen reduction reaction in zinc air batteries is solved, and high activity, low cost and stable catalytic effects are achieved, suitable for large-scale industries. application.
Patent Information
- Application Number
- CN202210996109.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-19
AI Technical Summary
The cathode oxygen reduction reaction kinetics of zinc air batteries limit their energy conversion efficiency. The existing platinum-based catalysts are costly and have poor stability, making them difficult to apply on a large scale.
Fe single atom catalyst based on three-dimensional porous carbon load is used to form a Fe-N4 coordination structure through the combination of amorphous nitrogen-doped carbon layer skeleton and iron single atoms. The preparation is made using salt template assisted in the in-situ pyrolysis method to improve the mass transfer of the catalyst Capacity and active sites are exposed.
It significantly improves the catalytic activity and iron atom utilization rate of the catalyst, reduces costs, and improves activity, selectivity and stability by regulating the electronic environment, making it suitable for large-scale industrial production and application.
Smart Images

Figure CN115332548B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of zinc-air batteries, and in particular to a three-dimensional porous carbon-supported Fe single-atom catalyst, a preparation method and an application thereof. Background Art
[0002] Zinc-air batteries have a high theoretical energy density (1086Wh kg -1 ), low cost and environmental protection, it is considered to be one of the most promising energy storage and conversion devices. However, the oxygen reduction reaction kinetics at its cathode are slow, which seriously limits the energy conversion efficiency of zinc-air batteries. Platinum (Pt)-based catalysts are known as commercial oxygen reduction reaction (ORR) electrocatalysts with high activity. However, the small reserves of platinum metal and the high cost and poor stability of platinum-based catalysts limit their large-scale industrial application. Therefore, it is urgent to develop highly active, stable and low-cost ORR catalysts.
[0003] MN supported on a carbon support x Transition metal single-atom catalysts (MNC, M=Fe, Mn, Co, etc.) with a large number of groups have great development prospects due to their advantages such as high reserves, low cost, high atomic utilization rate and adjustable electronic environment. Among them, Fe-NC single-atom catalysts have the most potential. In the past few years, Fe-NC single-atom catalysts supported on different carbon substrates, such as MOF-derived carbon blocks, carbon nanotubes and graphene sheets, have been widely studied. However, most Fe-NC single-atom catalysts are not as efficient as Fe-NC single-atom catalysts. x The groups are anchored on bulk carbon that is easy to agglomerate or two-dimensional graphene that is easy to stack, resulting in only a few Fe-N x The groups act as real active sites, while the internal sites do not participate in the oxygen reduction reaction because they are not in contact with the electrolyte and dissolved oxygen, thus limiting the ORR performance. In addition, since single iron atoms are prone to agglomeration, it is difficult to improve the electrocatalytic activity of the catalyst simply by increasing the metal loading. Therefore, improving the porous geometry and nanostructure of the catalyst to expose more active sites and enhance mass transfer capacity has become an effective strategy. Summary of the invention
[0004] The object of the present invention is to provide a three-dimensional porous carbon-supported Fe single-atom catalyst and a preparation method and application thereof, wherein the Fe single-atom catalyst has excellent mass transfer capability and high catalytic activity.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an iron single atom catalyst based on three-dimensional porous carbon support, comprising an amorphous nitrogen-doped carbon layer skeleton and iron single atoms supported on the amorphous nitrogen-doped carbon layer skeleton, presenting a Fe-N4 coordination structure, and the iron single atom catalyst presents a three-dimensional porous morphology.
[0007] Preferably, the content of single iron atoms is 4 to 8 wt.%.
[0008] The present invention provides a method for preparing an iron single-atom catalyst based on three-dimensional porous carbon support according to the above technical solution, comprising the following steps:
[0009] A carbon source, a nitrogen source, an iron source, a salt template and water are mixed and self-assembled to obtain a three-dimensional precursor;
[0010] Under an argon atmosphere, the three-dimensional precursor is sequentially calcined and annealed to obtain an iron single atom catalyst based on three-dimensional porous carbon support.
[0011] Preferably, the carbon source is glucose; the nitrogen source is dicyandiamide or ammonia; and the iron source is ammonium ferric citrate.
[0012] Preferably, the salt template is sodium chloride or ammonium chloride.
[0013] Preferably, the mass ratio of the carbon source, nitrogen source, iron source and salt template is 0.62:(1-1.5):(0.028-0.056):(8-12).
[0014] Preferably, the self-assembly temperature is -35°C to -50°C, and the time is 10 to 15 hours.
[0015] Preferably, the calcination temperature is 760-780° C. and the calcination time is 2-3 hours.
[0016] Preferably, the annealing temperature is 850-1050° C. and the time is 0.5-2 h.
[0017] The present invention provides the use of the iron single-atom catalyst based on three-dimensional porous carbon support described in the above technical scheme or the iron single-atom catalyst based on three-dimensional porous carbon support prepared by the preparation method described in the above technical scheme in electrocatalytic oxygen reduction reaction.
[0018] The present invention provides an iron single-atom catalyst based on three-dimensional porous carbon support, comprising an amorphous nitrogen-doped carbon layer skeleton and an iron single atom supported on the amorphous nitrogen-doped carbon layer skeleton, presenting a Fe-N4 coordination structure, and the iron single-atom catalyst presents a three-dimensional porous morphology. The catalyst of the present invention has an internally connected three-dimensional porous structure, and the three-dimensional structure not only increases the mass transfer rate but also exposes more active sites, promotes the mass transfer process, and thus enables the catalyst material to obtain extremely high catalytic activity. The Fe-N4 coordination structure serves as an active site for the oxygen reduction reaction, and oxygen adsorption reduction and product desorption occur.
[0019] In addition, the iron single-atom catalyst provided by the present invention has a single-atom dispersed catalytic active site, which maximizes the utilization rate of the iron atom of the catalyst, improves the activity of the catalyst and reduces the cost of the material. On the other hand, the active site of the catalyst is a homogeneous active site with an adjustable electronic environment, which makes the activity, selectivity and stability of the catalyst easily controllable by regulating the electronic structure of the catalyst material, which helps to obtain high catalytic activity.
[0020] The present invention adopts a salt template-assisted in-situ pyrolysis method to prepare an iron single-atom catalyst, and the obtained material has a three-dimensional porous structure. The salt template sodium chloride has a high melting point, is stable at high temperatures and is not easy to decompose and deform, and can be used as a template for carbon skeleton attachment during heat treatment. The salt template is cheap, easy to obtain, safe and environmentally friendly, and can be used for large-scale material preparation.
[0021] With the help of salt templates, the present invention produces iron single-atom catalysts with high specific surface area and open-pore structure on a large scale, increases the number of effective active sites and promotes the mass transfer process, and obtains catalyst materials with high catalytic activity and high practical application performance. The present invention rationally designs precursors and template materials to regulate the porous geometry and nanostructure of the catalyst, adopts a preparation method of salt template-assisted in-situ pyrolysis, has a simple process, is safe and environmentally friendly, and has low cost. The catalyst material has high activity, selectivity, and stability, and can achieve large-scale industrial production and application, solving the current problems that the removal of hard templates (such as SiO2) requires the use of highly corrosive or strong acid and alkali reagents such as hydrofluoric acid (HF), and that soft templates usually require specific precursor polymers, and the precursors are prone to aggregation and deformation during pyrolysis, which affects the synthesis process of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 (a) SEM of 3D SAFe prepared in Example 1; (b) TEM; (c) HR-TEM; (d) EDS image;
[0023] Figure 2 N2 adsorption and desorption isotherms of 3D SAFe prepared in Example 1;
[0024] Figure 3 This is a pore size distribution curve of the 3D SAFe prepared in Example 1;
[0025] Figure 4 HAADF-STEM image of the 3D SAFe prepared in Example 1;
[0026] Figure 5 (a) High-resolution XPS N 1s spectrum of 3D SAFe prepared in Example 1; (b) High-resolution XPS Fe 2p spectrum; (c) XPS full spectrum;
[0027] Figure 6 (a) is the Fe K-edge XANES spectra of 3D SAFe prepared in Example 1 and iron foil (Fe-foil), FeO, ferrocyanide (FePc) and Fe2O3, and the inset shows the enlarged marked area; (b) is the k-edge XANES spectra of 3D SAFe, Fe-foil, FePc and Fe2O3 3 Weighted FT-EXAFS spectra; (c) k of 3D SAFe 3 Weighted FT-EXAFS curve and fitting results (the inset shows the structure of the Fe site in 3D SAFe; the gray, blue, and yellow balls represent C, N, and Fe atoms, respectively; (d) is the R-space fitting result of the FT-EXAFS curve of 3DSAFe;
[0028] Figure 7 WT-EXAFS graphs of 3D SAFe, FePc and Fe-foil prepared in Example 1; (a) WT-EXAFS graph of 3D SAFe; (b) WT-EXAFS graph of FePc; (c) WT-EXAFS graph of Fe-foil;
[0029] Figure 8 (a) LSV curves of 3D SAFe with different Fe contents prepared in Examples 1 to 3; (b) Tafel slope diagram;
[0030] Fig. 9 The electron transfer number and H2O2 yield of 3D SAFe and Pt / C prepared in Example 1 are curves showing changes with electrode potential;
[0031] Fig.10 (a) is the ORR polarization curve of the 3D SAFe prepared in Example 1 before and after 10,000 cycles; (b) TEM image of 3D SAFe after the cycle test; (c) chronoamperometric curve of methanol crossover test using 3D SAFe and Pt / C at 0.7 V;
[0032] Fig.11The electrocatalytic performance test results of the catalyst prepared in Example 1 in a zinc-air battery: (a) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled from 3DSAFe and Pt / C electrocatalyst; (b) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled from 3DSAFe and Pt / C electrocatalyst; (c) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled from 3DSAFe and Pt / C electrocatalyst; (d) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled from 3DSAFe and Pt / C electrocatalyst; (e) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled from 3DSAFe and Pt / C electrocatalyst; (f) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled from 3DSAFe and Pt / C electrocatalyst; (g) the discharge polarization curve and corresponding power density diagram of the zinc- -2 The specific capacity of the zinc-air battery was evaluated by constant current discharge, and the measured specific capacity was normalized by the mass of the consumed zinc anode; (c) Rate performance test of zinc-air battery; (d) 3D SAFe was used in zinc-air battery at 10 mA cm -2 Long-term galvanostatic discharge curve under the condition of (e) 3D SAFe, where charging is achieved by replacing the electrolyte solution and the zinc sheet anode; (e) E 1 / 2 and comparison of peak power density with other publicly reported catalysts;
[0033] Fig.12 A diagram of a zinc-air battery device;
[0034] Fig.13 Morphological characterization results of Fe-BC prepared in Comparative Example 1: (a) SEM; (b) TEM; (c) HR-TEM; (d) EDS image;
[0035] Fig.14 Morphological characterization results of Fe-rGO prepared in Comparative Example 2: (a) SEM; (b) TEM; (c) HR-TEM; (d) EDS image;
[0036] Fig.15 (a) N2 adsorption and desorption isotherms of the three samples; (b) pore size distribution curves;
[0037] Fig.16 (a) High-resolution XPS N 1s spectrum of Fe-BC prepared in Comparative Example 1; (b) High-resolution XPS Fe 2p spectrum; (c) XPS full spectrum;
[0038] Fig.17 (a) High-resolution XPS N 1s spectrum of Fe-rGO prepared in Comparative Example 2; (b) High-resolution XPS Fe 2p spectrum; (c) XPS full spectrum;
[0039] Fig.18 The ORR electrocatalytic performance of the three samples and commercial Pt / C materials was tested in 0.1 M KOH: (a) ORR polarization curves of 3D SAFe, Pt / C and control samples (Fe-BC and Fe-rGO) prepared in Example 1; (b) E 1 / 2 and j at 0.8V k; (c) Tafel curves of 3D SAFe, Fe-rGO and Pt / C; (d) Unique three-dimensional open pore structure of 3D SAFe;
[0040] Fig.19 The curves showing the relationship between the electron transfer number (n) and H2O2 yield of 3D SAFe prepared in Example 1 and Pt / C, Fe-rGO and Fe-BC as a function of electrode potential;
[0041] Fig. 20 Discharge polarization curves and corresponding power density diagrams of zinc-air batteries assembled with 3D SAFe prepared in Example 1 and Pt / C, Fe-rGO and Fe-BC. DETAILED DESCRIPTION
[0042] The present invention provides an iron single-atom catalyst based on three-dimensional porous carbon support, comprising an amorphous nitrogen-doped carbon layer skeleton and iron single atoms supported on the amorphous nitrogen-doped carbon layer skeleton, presenting a Fe-N4 coordination structure, and the iron single-atom catalyst presents a three-dimensional porous morphology.
[0043] In the present invention, the content of single iron atoms in the iron single atom catalyst is preferably 4 to 8 wt.%, more preferably 4 to 6 wt.%; iron is dispersed in the form of single atoms on the amorphous nitrogen-doped carbon layer skeleton, presenting a Fe-N4 coordination structure, and is a Fe-NC single atom catalyst with Fe-N4 as the active site.
[0044] In the iron single atom catalyst provided by the present invention, the electronic environment of the single atom active site can be regulated by adjusting the coordination structure of the single atom center and the electron density of the carbon substrate. Regulating the electronic environment can adjust the adsorption and desorption ability of the single atom catalyst to the reaction intermediate, thereby improving the activity of the oxygen reduction reaction. In addition, by adjusting the electronic structure of the catalyst, the catalyst can be easily released oxygen-containing intermediates, so it is easier to generate 2e hydrogen peroxide by-products. In addition, by adjusting the coordination environment and electronic structure of the single atom, the transformation of the catalytic site can be achieved, thereby improving stability.
[0045] The present invention provides a method for preparing an iron single-atom catalyst based on three-dimensional porous carbon support according to the above technical solution, comprising the following steps:
[0046] A carbon source, a nitrogen source, an iron source, a salt template and water are mixed and self-assembled to obtain a three-dimensional precursor;
[0047] Under an argon atmosphere, the three-dimensional precursor is sequentially calcined and annealed to obtain an iron single atom catalyst based on three-dimensional porous carbon support.
[0048] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.
[0049] The present invention mixes a carbon source, a nitrogen source, an iron source, a salt template and water to perform self-assembly to obtain a three-dimensional precursor.
[0050] In the present invention, the carbon source is preferably glucose; the nitrogen source is preferably dicyandiamide or ammonia; and the iron source is preferably ammonium ferric citrate.
[0051] In the present invention, the salt template is preferably sodium chloride or ammonium chloride.
[0052] In the present invention, the mass ratio of the carbon source, nitrogen source, iron source and salt template is preferably 0.62:(1-1.5):(0.028-0.056):(8-12), and more preferably 0.62:1.2:(0.028-0.042):8.5. The present invention has no particular limitation on the amount of water, as long as it can fully dissolve the materials.
[0053] In the present invention, the mixing time of the carbon source, nitrogen source, iron source, salt template and water is preferably 4 hours, and the mixing is preferably carried out under stirring conditions. The present invention has no special limitation on the stirring rate, as long as the materials can be completely dissolved and evenly dispersed in water.
[0054] In the present invention, the self-assembly temperature is preferably -35°C to -50°C, and the time is preferably 10 to 15 hours; the present invention freezes the solution under low temperature conditions to completely solidify, and the salt template self-assembles to form a three-dimensional template, and the carbon source, unit and iron source are evenly loaded on the grain boundaries of the salt template material.
[0055] After completing the self-assembly, the present invention preferably dries the obtained product under vacuum for 48 hours to obtain a three-dimensional precursor.
[0056] After obtaining the three-dimensional precursor, the present invention sequentially calcines and anneals the three-dimensional precursor under an argon atmosphere to obtain an iron single-atom catalyst based on three-dimensional porous carbon support.
[0057] In the present invention, the calcination temperature is preferably 760-780°C, the time is preferably 2-3h; the heating rate to the calcination temperature is preferably 4-6°C min -1 ; During the calcination process, the precursor completes carbonization, the nitrogen source decomposes to achieve nitrogen doping, and a single atomic site is formed.
[0058] After the calcination is completed, the present invention preferably washes the obtained product with excess deionized water, vacuum filters, dissolves and removes the salt template, and anneals the obtained solid product. The present invention has no particular limitation on the specific process of the washing and vacuum filtration, and can be carried out according to the process well known in the art.
[0059] In the present invention, the annealing is preferably performed in an argon atmosphere; the annealing temperature is preferably 850-1050° C., more preferably 900° C., and the annealing time is preferably 0.5-2 h, more preferably 1 h.
[0060] The present invention reduces defects in the material through annealing, increases the graphitization degree of the material, and improves the electrical conductivity of the material.
[0061] After the annealing is completed, the temperature is preferably lowered to room temperature to obtain a three-dimensional porous carbon-supported iron single atom catalyst, which is referred to as 3D SAFe. The present invention has no particular limitation on the process of lowering the temperature to room temperature, and the process may be performed according to a process well known in the art.
[0062] The present invention provides the use of the three-dimensional porous carbon-supported iron single-atom catalyst described in the above technical solution or the three-dimensional porous carbon-supported iron single-atom catalyst prepared by the preparation method described in the above technical solution in an electrocatalytic oxygen reduction reaction. The present invention has no special limitation on the method of application, and the application can be carried out according to methods well known in the art.
[0063] In the present invention, the electrocatalytic oxygen reduction reaction is preferably derived from a zinc-air battery.
[0064] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] Example 1
[0066] 8.5 g of sodium chloride, 0.62 g of glucose, 1.2 g of dicyandiamide and 28 mg of ammonium ferric citrate were dissolved in 75 mL of deionized water, stirred for 4 h, and the resulting mixture was frozen at -35 ° C for 15 h until completely solidified, and then dried under vacuum for 48 h to obtain a three-dimensional precursor with an iron content of 4 wt.%;
[0067] Under the protection of argon atmosphere, the three-dimensional precursor was calcined at 760°C for 3 h with a heating rate of 4°C min -1 The obtained product was washed with a large amount of deionized water and then vacuum filtered. The obtained solid was annealed at 900°C for 1h under the protection of argon atmosphere. After cooling to room temperature, a three-dimensional porous carbon-supported iron single atom catalyst was obtained.
[0068] Example 2
[0069] 8.5 g of sodium chloride, 0.62 g of glucose, 1.2 g of dicyandiamide and 42 mg of ammonium ferric citrate were dissolved in 75 mL of deionized water, stirred for 4 h, and the resulting mixture was frozen at -35 ° C for 15 h until completely solidified, and then dried under vacuum for 48 h to obtain a three-dimensional precursor with an iron content of 6 wt.%;
[0070] Under the protection of argon atmosphere, the three-dimensional precursor was calcined at 760°C for 3 h with a heating rate of 4°C·min -1 The obtained product was washed with a large amount of deionized water and then vacuum filtered. The obtained solid was annealed at 900°C for 1h under the protection of argon atmosphere. After cooling to room temperature, a three-dimensional porous carbon-supported iron single atom catalyst was obtained.
[0071] Example 3
[0072] 8.5 g of sodium chloride, 0.62 g of glucose, 1.2 g of dicyandiamide and 56 mg of ammonium ferric citrate were dissolved in 75 mL of deionized water, stirred for 4 h, and the resulting mixture was frozen at -35 ° C for 15 h until completely solidified, and then dried under vacuum for 48 h to obtain a three-dimensional precursor with an iron content of 8 wt.%;
[0073] Under the protection of argon atmosphere, the three-dimensional precursor was calcined at 760°C for 3 h with a heating rate of 4°C·min -1 The obtained product was washed with a large amount of deionized water and then vacuum filtered. The obtained product was annealed at 900°C for 1h under the protection of argon atmosphere. After cooling to room temperature, a three-dimensional porous carbon-supported iron single atom catalyst was obtained.
[0074] Comparative Example 1
[0075] Catalyst material with 4 wt.% iron content supported on a zero-dimensional substrate (Fe-BC):
[0076] 0.62 g of glucose, 1.2 g of dicyandiamide and 28 mg of ammonium ferric citrate were dissolved in 75 mL of deionized water, stirred for 4 hours and freeze-dried to obtain a zero-dimensional precursor; the zero-dimensional precursor was calcined and annealed according to the conditions of Example 1 to obtain a Fe-BC catalyst material.
[0077] Comparative Example 2
[0078] Catalyst material with 4 wt.% iron content supported on a two-dimensional substrate (Fe-rGO):
[0079] 1g of dicyandiamide powder was added to 50mL of 2mg mL -1 After ultrasonic treatment for 2 h, 10 mL of 2 mg mL -1The solution of ammonium ferric citrate was stirred for 2 h and then freeze-dried to obtain a two-dimensional precursor;
[0080] Under the protection of argon atmosphere, the two-dimensional precursor was calcined at 320°C for 2 h, and then heated to 520°C for 2 h, with a heating rate of 5°C·min -1 , then cooled to room temperature and ground to obtain a black powder precursor; the obtained black powder precursor was annealed at 800°C for 1h, and then cooled to room temperature to obtain a Fe-rGO two-dimensional material.
[0081] Characterization and performance testing
[0082] Morphological characterization:
[0083] The morphology of the samples was observed using a scanning electron microscope (SEM, Hitachi SU8020). The surface contrast information of the samples was reflected by the secondary electron signals excited by the high-energy electron beam bombarding the sample surface.
[0084] The morphology of the samples was observed using a transmission electron microscope (TEM, JEOL JEM-2100F). The thickness information of the samples was reflected by the angle change caused by the collision between the high-energy electron beam and the sample atoms.
[0085] High Angle Annular Dark Field-Scanning Transmission Electron Microscopy (HAADF-STEM, JEOL JEMARM200F) was used to observe the atomic structure information of the samples.
[0086] Structural characterization:
[0087] Raman spectrometer (LabRAM HR Evolution) is used to characterize the defect structure of the material. The Raman scattering spectrum generated by the material at different incident light frequencies reflects the degree of material defects.
[0088] X-ray diffraction (XRD, D / max 2200HB / PC) is used to characterize the phase composition of the material. The Bragg scattering of X-rays in the sample is used to determine the material phase.
[0089] The specific surface area and pore size distribution of the material were characterized by a specific surface area analyzer (Brunauer-Emmett-Teller, BET, ASAP 2020 HD88 PLUS). The specific surface area and pore size distribution of the material were calculated by nitrogen adsorption and desorption.
[0090] Composition and chemical environment characterization:
[0091] Energy Dispersive Spectroscopy (EDS) is used to observe the elemental composition and element distribution of the sample. The characteristic X-rays released by the electron transition in the material are used to distinguish different elements and their distribution positions.
[0092] X-ray Photoelectron Spectroscopy (XPS, ThermoFisher Scientific) is used to determine the elemental composition and the existence state of each element on the surface of the material. The number and energy of photoelectrons generated by the material are used to reflect the elemental composition and element binding energy information of the material.
[0093] Inductively Coupled Plasma-Mass Spectrometry (ICP-MS, PerkinElmer NexION 300X ICP-MS) was used to determine the element content of the material. High-energy plasma is used to excite atoms into ions and mass spectrometry is used to separate different particles to determine the content of each element.
[0094] X-ray absorption fine structure spectroscopy (XAFS, Beijing Synchrotron Radiation Facility (BSRF)), including X-ray absorption near edge structure (XANES), extended X-ray absorption fine structure (EXAFS) and Fourier transform (FT-EXAFS) and wavelet transform (WT-EXAFS) are used to characterize the elemental composition and microscopic chemical environment of the material. The absorption of X-rays by characteristic elements and the scattering of X-rays by surrounding atoms are used to characterize the valence state of specific elements and the surrounding chemical environment.
[0095] Oxygen reduction reaction (ORR) electrochemical test: It was carried out in 0.1 M KOH saturated with O2 on a CHI 760E electrochemical workstation (Shanghai Chenhua Company) at room temperature and ambient pressure. In a standard three-electrode system, a rotating disk electrode (RDE) or a rotating ring disk electrode (RRDE) was used as the working electrode, and a graphite rod and Ag / AgCl were used as the counter electrode and reference electrode, respectively.
[0096] Preparation of working electrode: 8 mg of catalyst material was dispersed in a mixed solution of deionized water (0.25 mL), isopropanol (0.7 mL) and Nafion (5 wt.%, 50 uL) to form a uniform catalyst ink suspension. The resulting suspension was heated to 408 μg cm -2 The loading amount is dropped on the RDE / RRDE electrode. All potentials of the reference electrode are calibrated relative to the reversible hydrogen electrode (RHE) according to formula 1, and all potentials mentioned are relative to the RHE potential:
[0097] E (RHE) =E Ag / AgCl +0.204+0.0591×pH(1).
[0098] Linear Sweep Voltammetry (LSV) was used at a speed of 400-1600 rpm and 95% iR compensation at 5 mV·s -1 The cathodic polarization curve of the material is tested at a scan rate to obtain the half-wave potential (E 1 / 2 ), limiting diffusion current density (j L ), kinetic current density (j k ), Tafel slope and other parameters to characterize the catalytic activity of the material.
[0099] The disk current (I D ), ring current (I R ), calculate the byproduct hydrogen peroxide yield (H2O2%) and the electron transfer number (n) (Equation 2, 3) during the reaction, and characterize the catalytic selectivity of the material, (N is the collection coefficient 0.37)
[0100]
[0101]
[0102] Cyclic voltammetry (CV, 0.57 V-1.17 V, 200 mV s -1 ) and linear sweep voltammetry (LSV) to test the half-wave potential decay (ΔE 1 / 2 ) and the limiting diffusion current density change, characterizing the catalytic stability of the material.
[0103] Zinc-air battery testing:
[0104] Using a stacked zinc-air battery device (such as Fig.12 The actual application performance of the material in zinc-air batteries was tested using zinc sheets as anodes and 6M KOH as electrolytes. The catalyst ink suspension was droplet-coated on 28-BC carbon paper to make a simple gas diffusion electrode with a catalyst loading of 0.48 mg cm -2 .
[0105] The open circuit voltage of the zinc-air battery was tested using a CHI 760E electrochemical workstation to characterize the output voltage of the catalyst as a cathode catalytic material in practical applications. The discharge curve and power density (W) of the material in practical applications were tested using a Coster electrochemical workstation to characterize the material's practical application activity. The chromopotentiometric (CP) method was used at 10 mA cm -2 The specific capacity of the material was tested under constant current conditions to characterize the practical application activity of the material. The multi-current step method (ISTEP) was used to measure the specific capacity of the material under constant current conditions of 2-50 mA cm -2 The rate performance of the material is tested to characterize the performance of the material in practical applications at different current densities. The material is tested using the constant current discharge method (CP) at 10 mA cm -2 The stability of long-term discharge under constant current conditions. The chronoamperometric curve was used to test the methanol crossover resistance of the material at 0.7V.
[0106] 1) Figure 1 (a) SEM of 3D SAFe prepared in Example 1; (b) TEM; (c) HR-TEM; (d) EDS image, C (red), N (blue), Fe (green); Figure 1 It can be seen that the sample has a three-dimensional open-pore morphology, no iron particles are generated, and the elements are evenly distributed.
[0107] 2) Figure 2 N2 adsorption and desorption isotherms of 3D SAFe prepared in Example 1; Figure 2 It can be calculated that the specific surface area of 3D SAFe measured by the specific surface area analyzer is 282.82m 2 ·g -1, the typical type IV curve characteristics prove the simultaneous existence of mesopores and micropores.
[0108] 3) Figure 3 This is a pore size distribution curve of the 3D SAFe prepared in Example 1 measured by a specific surface area analyzer. Figure 3 It is proved that mesopores and micropores exist simultaneously.
[0109] 4) Figure 4 HAADF-STEM image of 3D SAFe prepared in Example 1; Figure 4 It can be seen that single iron atoms with larger atomic numbers appear as bright spots on the carbon substrate, proving the single atomic distribution of iron.
[0110] 5) Figure 5 (a) High-resolution XPS N 1s spectrum of 3D SAFe prepared in Example 1; (b) high-resolution XPS Fe 2p spectrum; (c) full XPS spectrum. Figure 5 It proves that no iron particles are generated in the sample. In addition, ICP-MS inductively coupled plasma mass spectrometry was used to detect the iron content in the 3D SAFe prepared in Example 1. The ICP results prove that the iron content in the 3D SAFe prepared in Example 1 is 3.68 wt.%.
[0111] 6) Figure 6 In the figure, (a) is the Fe K-edge XANES spectra of 3D SAFe prepared in Example 1 and commercially available iron foil (Fe-foil), FeO, ferrocyanide (FePc), and Fe2O3, and the inset shows the enlarged marked area; (b) is the k-edge XANES spectra of 3D SAFe, Fe-foil, FePc, and Fe2O3 3 Weighted FT-EXAFS spectra; (c) k of 3D SAFe 3 Weighted FT-EXAFS curve and fitting results (the inset shows the structure of the Fe site in 3D SAFe; the gray, blue, and yellow balls represent C, N, and Fe atoms, respectively; (d) is the R space fitting result of the FT-EXAFS curve of 3D SAFe, Figure 6 The fitting results of the amplitude and imaginary part after Fourier transformation are shown in Figure 1. The fitting parameters are shown in Table 1. 3 Weighted and not phase corrected. The single-atom distribution of Fe and the coordination structure of Fe-N4 are demonstrated.
[0112] Table 1 Fitting parameters of Fe K-edge EXAFS spectrum of 3D SAFe a
[0113]
[0114]
[0115] Note a: The coordination number N is fixed to 4. S0 2 and ΔE0 are used as global fitting parameters, and their values are adjusted according to the fitting results. The results are fed back as (1.0±0.3) and (-1±3) eV respectively. The data range selected is There are 6 variable parameters set in the fitting, and the total number of independent variable parameter points that can exist determined by the data range is 8.3. The R factor of this fitting is 1.9%.
[0116] Note b: The distances between Fe-N and Fe-C are determined from the 3DSAFe crystal structure obtained from DFT calculations.
[0117] Note c: Based on the calculated crystal structure, the coordination numbers are fixed as N(Fe-N)=4, N(Fe-C)=4.
[0118] 7) Figure 7 WT-EXAFS graphs of 3D SAFe, FePc and Fe-foil: (a) WT-EXAFS graph of 3D SAFe; (b) WT-EXAFS graph of FePc; (c) WT-EXAFS graph of Fe-foil, which proves the coordination structure of Fe-N.
[0119] 8) Figure 8 (a) 3D SAFe LSV curves of different Fe contents prepared in Examples 1 to 3; (b) Tafel slope diagram. Figure 8 It can be seen that the half-wave potentials of catalysts with different iron single atom loadings are close to and all higher than 0.9 V vs. RHE, among which the sample with an Fe content of 4 wt.% has the lowest Tafel slope, proving that the different catalyst materials obtained have high catalytic activity, among which the sample with an Fe content of 4 wt.% has the highest catalytic activity.
[0120] 9) Fig. 9 The electron transfer number and H2O2 yield curves calculated from the disk and ring currents of 3D SAFe and Pt / C prepared in Example 1 as a function of electrode potential indicate that the prepared catalyst material has high selectivity.
[0121] 10) Fig.10 (a) is the LSV polarization curve of the 3D SAFe prepared in Example 1 before and after 10,000 CV cycles; (b) is the TEM image of the 3D SAFe after the cycle test; (c) is the chronoamperometric curve of the methanol crossover test using 3D SAFe and Pt / C at 0.7 V. Fig.10 The catalyst was demonstrated to have high stability.
[0122] 11) Fig.11 The electrocatalytic performance test results of the catalyst prepared in Example 1 in a zinc-air battery: (a) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled by 3D SAFe and Pt / C electrocatalyst; (b) the discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled by 10 mA cm -2 The specific capacity of the zinc-air battery was evaluated by constant current discharge, and the measured specific capacity was normalized by the mass of the consumed zinc anode; (c) Rate performance test of zinc-air battery; (d) 3D SAFe was used in zinc-air battery at 10 mA cm -2 Long-term constant-current discharge curve under the condition of (e) E of 3DSAFe, where charging is achieved by replacing the electrolyte solution and the zinc sheet anode; 1 / 2 Comparison of peak power density with other publicly reported catalysts [1-16] , see Table 1 for details. The peak power density of the zinc-air battery assembled by 3D SAFe is as high as 156 mW cm -2 , much higher than commercial Pt / C materials, with a specific capacity of up to 815 mAh g -1 Zn , close to the theoretical value, high rate performance, the discharge voltage remains unchanged before and after 80h constant current discharge, and the stability is high, which proves that the sample has the potential for practical application. Table 1 E of 3D SAFe prepared in Example 1 and the published catalyst 1 / 2 Comparison with peak power density
[0123]
[0124]
[0125] References in Table 1:
[0126] (1) Shi, Q.; Liu, Q.; Ma, Y.; Fang, Z.; Liang, Z.; Shao, G.; Tang, B.; Yang, W.; Qin, L.; Fang, Mater.2020,10(10),1903854.
[0127] (2)Ge,H.;Li,G.;Shen,J.;Ma,W.;Meng,X.;Xu,L.Co4N nanoparticlesencapsulated in N-doped carbon box as tri-functional catalyst for Zn-airbattery and overall water splitting.Appl.Catal.B Environ.2020,275,119104.
[0128] (3)Zhou,Q.;Cai,J.;Zhang,Z.;Gao,R.;Chen,B.;Wen,G.;Zhao,L.;Deng,Y.;Dou,H.;Gong,X.;Zhang,Y.;Hu,Y.;Yu,A.;Sui,X.;Wang,Z.;Chen,Z.A Gas-Phase MigrationStrategy to Synthesize Atomically Dispersed Mn-N-C Catalysts for Zn-AirBatteries.Small Methods 2021,5(6),e2100024.
[0129] (4)Zeng,Z.;Fu,G.;Yang,H.B.;Yan,Y.;Chen,J.;Yu,Z.;Gao,J.;Gan,L.Y.;Liu,B.;Chen,P.Bifunctional N-CoSe 2 / 3 D-MXene as Highly Efficient and DurableCathode for Rechargeable Zn–Air Battery.ACS Materials Lett.2019,1(4),432–439.
[0130] (5)Li,H.;Li,Q.;Wen,P.;Williams,T.B.;Adhikari,S.;Dun,C.;Lu,C.;Itanze,D.;Jiang,L.;Carroll,D.L.;Donati,G.L.;Lundin,P.M.;Qiu,Y.;Geyer,S.M.ColloidalCobalt Phosphide Nanocrystals as Trifunctional Electrocatalysts for OverallWater Splitting Powered by aZinc-Air Battery.Adv.Mater.2018,30(9),1705796.
[0131] (6)Wang,H.-F.;Tang,C.;Wang,B.;Li,B.-Q.;Zhang,Q.BifunctionalTransition Metal Hydroxysulfides:Room-Temperature Sulfurization andTheirApplications in Zn-Air Batteries.Adv.Mater.2017,29(35),1702327.
[0132] (7)Xiao,M.;Xing,Z.;Jin,Z.;Liu,C.;Ge,J.;Zhu,J.;Wang,Y.;Zhao,X.;Chen,Z.Preferentially Engineering FeN4 Edge Sites onto Graphitic Nanosheets forHighly Active and Durable Oxygen Electrocatalysis in Rechargeable Zn-AirBatteries.Adv.Mater.2020,32(49),e2004900.
[0133] (8)Qiao,Y.;Yuan,P.;Hu,Y.;Zhang,J.;Mu,S.;Zhou,J.;Li,H.;Xia,H.;He,J.;Xu,Q.Sulfuration of an Fe-N-C Catalyst Containing Fex C / Fe Species to Enhancethe Catalysis of Oxygen Reduction in Acidic Media and for Use in Flexible Zn-Air Batteries.Adv.Mater.2018,30(46),e1804504.
[0134] (9)Han,X.;Ling,X.;Yu,D.;Xie,D.;Li,L.;Peng,S.;Zhong,C.;Zhao,N.;Deng,Y.;Hu,W.Atomically Dispersed Binary Co-Ni Sites in Nitrogen-Doped HollowCarbon Nanocubes for Reversible Oxygen Reduction andEvolution.Adv.Mater.2019,31(49),e1905622.
[0135] (10)Han,X.;Ling,X.;Wang,Y.;Ma,T.;Zhong,C.;Hu,W.;Deng,Y.Generation ofNanoparticle,Atomic-Cluster,and Single-Atom Cobalt Catalysts from ZeoliticImidazole Frameworks by Spatial Isolation and Their Use in Zinc-Air Batteries.Angew.Chem.Int.Ed.2019,58(16),5359–5364.
[0136] (11)Jose,V.;Hu,H.;Edison,E.;Manalastas,W.;Ren,H.;Kidkhunthod,P.;Sreejith,S.;Jayakumar,A.;Nsanzimana,J.M.V.;Srinivasan,M.;Choi,J.;Lee,J.-M.Modulation of Single Atomic Co and Fe Sites on Hollow Carbon Nanospheres asOxygen Electrodes for Rechargeable Zn-Air Batteries.Small Methods 2021,5(2),e2000751.
[0137] (12)Ban,J.;Wen,X.;Xu,H.;Wang,Z.;Liu,X.;Cao,G.;Shao,G.;Hu,J.DualEvolution in Defect and Morphology of Single-Atom Dispersed Carbon BasedOxygen Electrocatalyst.Adv.Funct.Mater.2021,31(19),2010472.
[0138] (13)Feng,Y.;Tian,G.;Peng,Q.;Wu,Y.;Li,Y.;Luo,X.;Han,Y.;Li,Q.Fe-N DopedPeanut Shell Activated Carbon as a Superior Electrocatalyst for OxygenReduction and Cathode Catalyst for Zinc-Air Battery.ChemElectroChem 2021,8(24),4797-4803.
[0139] (14)Wang,C.;Li,Z.;Wang,L.;Lu,X.;Wang,S.;Niu,X.Vertical-Space-LimitSynthesis ofBifunctional Fe,N-Codoped 2D Multilayer Graphene Electrocatalystsfor Zn-Air Battery.Energy Technol.2019,7(6),1900123.
[0140] (15) Zhang,XT; Hu, SZ; Sun, SG; Zhang,
[0141] (16) Yang, Y.; Wu, Y.; Chen,
[0142] 12) Fig.13 The morphology characterization results of Fe-BC prepared in Comparative Example 1: (a) SEM; (b) TEM; (c) HR-TEM; (d) EDS image, C (red), N (purple), Fe (blue), proving that the sample has a zero-dimensional block morphology.
[0143] 13) Fig.14 The morphology characterization results of Fe-rGO prepared in Comparative Example 2: (a) SEM; (b) TEM; (c) HR-TEM; (d) EDS image, C (red), N (green), Fe (purple), proving that the sample has a two-dimensional stacked morphology.
[0144] 14) Fig.15 (a) N2 adsorption and desorption isotherms of the three samples obtained by surface area analyzer; (b) pore size distribution curve; Fig.15 It can be seen that the three-dimensional open-pore structure sample prepared in Example 1 has the highest specific surface area and has mesopores and micropores, which helps to expose more active sites and promote the mass transfer process.
[0145] 15) Fig.16(a) High-resolution XPS N 1s spectrum of Fe-BC prepared in Comparative Example 1; (b) High-resolution XPS Fe 2p spectrum; (c) XPS full spectrum. Fig.16 It can be seen that the coordination mode, iron valence state and chemical environment composition of Fe-BC are similar to those of 3DSAFe, so the difference in oxygen reduction reaction activity should be attributed only to their different micromorphologies.
[0146] 16) Fig.17 (a) High-resolution XPS N 1s spectrum of Fe-rGO prepared in Comparative Example 2; (b) High-resolution XPS Fe2p spectrum; (c) XPS full spectrum. Fig.17 It can be seen that the coordination mode, iron valence state and chemical environment composition of Fe-rGO are similar to those of 3DSAFe, so the difference in their oxygen reduction reaction activities should be attributed only to their different micromorphologies.
[0147] 17) Fig.18 The ORR electrocatalytic performance of the three samples and commercial Pt / C materials was tested in 0.1 M KOH: (a) LSV polarization curves of 3D SAFe, Pt / C and control samples (Fe-BC and Fe-rGO) prepared in Example 1; (b) E 1 / 2 and j at 0.8V k ; (c) Tafel curves of 3D SAFe, Fe-rGO and Pt / C; (d) The unique three-dimensional open pore structure of 3D SAFe is conducive to the diffusion and mass transfer of reactants, thus providing abundant catalytic sites for ORR. 3D SAFe has the highest half-wave potential and kinetic current density at 0.8V, the lowest Tafel slope and the highest catalytic activity. In addition, 3D SAFe has the highest limiting diffusion current density, proving that the three-dimensional open pore structure increases the number of effective active sites and promotes the mass transfer process, thereby improving the oxygen reduction reaction activity.
[0148] 18) Fig.19 The relationship curves of the electron transfer number (n) and H2O2 yield calculated from disk and ring currents of 3D SAFe prepared in Example 1 and Pt / C, Fe-rGO and Fe-BC as a function of electrode potential demonstrate that the selectivity of the three samples is similar.
[0149] 19) Fig. 20 The discharge polarization curve and corresponding power density diagram of the zinc-air battery assembled with 3D SAFe prepared in Example 1 and Pt / C, Fe-rGO and Fe-BC. Fig. 20 It can be seen that the 3D SAFe prepared by the present invention has the best practical application performance.
[0150] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an iron single-atom catalyst based on three-dimensional porous carbon support, characterized in that: The following steps are involved: A carbon source, a nitrogen source, an iron source, a salt template and water are mixed and self-assembled to obtain a three-dimensional precursor; In an argon atmosphere, the three-dimensional precursor is sequentially calcined and annealed to obtain an iron single atom catalyst supported on three-dimensional porous carbon; The mass ratio of the carbon source, nitrogen source, iron source and salt template is 0.62:(1-1.5):(0.028-0.056):(8-12); The iron single atom catalyst based on three-dimensional porous carbon support includes an amorphous nitrogen-doped carbon layer skeleton and iron single atoms supported on the amorphous nitrogen-doped carbon layer skeleton, presenting a Fe-N4 coordination structure, and the iron single atom catalyst presents a three-dimensional porous morphology.
2. The preparation method according to claim 1, characterized in that: The content of single iron atoms is 4~8wt.%.
3. The preparation method according to claim 1, characterized in that: The carbon source is glucose; the nitrogen source is dicyandiamide or ammonia; and the iron source is ammonium ferric citrate.
4. The preparation method according to claim 1, characterized in that: The salt template is sodium chloride or ammonium chloride.
5. The preparation method according to claim 1, characterized in that: The self-assembly temperature is -35 to -50°C and the time is 10 to 15 hours.
6. The preparation method according to claim 1, characterized in that: The calcination temperature is 760-780° C. and the calcination time is 2-3 hours.
7. The preparation method according to claim 1, characterized in that: The annealing temperature is 850-1050° C. and the annealing time is 0.5-2 h.
8. Use of the iron single-atom catalyst based on three-dimensional porous carbon support prepared by the preparation method according to any one of claims 1 to 7 in zinc-air batteries.