Electrochemical devices and electrical devices

By using a design in which the tensile strength of the second conductive layer is greater than that of the first conductive layer in the tab of the electrochemical device, the problem of shortened service life of the tab after a collision is solved and the long-lasting effect of the electrochemical device is achieved. Charge and discharge function.

CN115332738BActive Publication Date: 2024-10-18NINGDE AMPEREX TECHNOLOGY LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210962684.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-09
Publication Date
2024-10-18
Estimated Expiration
2042-05-09

AI Technical Summary

Technical Problem

The service life of the tabs of the electrochemical device is greatly shortened after being impacted, resulting in a reduction in the overall life of the electrochemical device.

Method used

An electrochemical device is designed, the tab of which is composed of a stacked first conductive layer and a second conductive layer. The tensile strength of the second conductive layer is greater than that of the first conductive layer, which enhances the overall strength of the tab and ensures that the electrode is Even when the ear is broken or cracked, it can still conduct, extending the service life of the electrochemical device.

Benefits of technology

By improving the tensile resistance and bending resistance of the tabs, it ensures that the electrochemical device can still charge and discharge after a collision, significantly extending the service life of the electrochemical device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115332738B_ABST
    Figure CN115332738B_ABST
Patent Text Reader

Abstract

The present application discloses an electrochemical device and an electrical device. The electrochemical device comprises an electrode assembly and a tab, the tab extending from the electrode assembly, the tab comprising a first conductive layer and a second conductive layer stacked, the first conductive layer being electrically connected to the electrode assembly, the first conductive layer and the second conductive layer being electrically conductive; wherein the tensile strength of the second conductive layer is greater than the tensile strength of the first conductive layer. The tab of the electrochemical device provided by the present application has good conductivity and tensile strength, thereby increasing the service life of the product.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application based on the invention with application number 202210495814.1, application date May 9, 2022, applicant Ningde New Energy Technology Co., Ltd., and invention name “Electrochemical device and electrical device”. Technical Field

[0002] The present application relates to the technical field of electric energy storage, and in particular to an electrochemical device and an electric device. Background Art

[0003] An electrochemical device is a device that converts external energy into electrical energy and stores it inside to power external electrical devices (such as portable electronic devices, etc.) when needed. In the development of electrochemical device technology, in addition to improving energy density, service life is also an issue that cannot be ignored. In particular, after an electrochemical device is hit, whether the tab can work normally greatly affects the service life of the electrochemical device.

[0004] In summary, it is necessary to design an electrochemical device and an electrical device to solve the above-mentioned technical problems. Summary of the invention

[0005] The embodiments of the present application provide an electrochemical device and an electrical device, wherein the electrode tabs of the electrochemical device have good electrical conductivity and tensile strength, thereby increasing the service life of the product.

[0006] In a first aspect, an embodiment of the present application provides an electrochemical device, comprising:

[0007] Electrode assembly;

[0008] A tab extending from the electrode assembly, the tab comprising a first conductive layer and a second conductive layer stacked together, the first conductive layer being electrically connected to the electrode assembly, and the first conductive layer and the second conductive layer being electrically conductive;

[0009] Wherein, the tensile strength of the second conductive layer is greater than the tensile strength of the first conductive layer.

[0010] In some embodiments, the electrode assembly includes a first end and a second end, the first end and the second end are arranged opposite to each other along a first direction, the electrode ear is bent and extended from the first end toward the direction close to the central axis of the electrode assembly, the second conductive layer is arranged on at least one side of the first conductive layer close to the electrode assembly, and the extension direction of the central axis is perpendicular to the first direction.

[0011] In some embodiments, the electrode tab is at least partially bent into an arc shape that bulges toward the central axis of the electrode assembly.

[0012] In some embodiments, the second conductive layer is coated on the outside of the first conductive layer, or the first conductive layer is coated on the outside of the second conductive layer.

[0013] In some embodiments, the number of the first conductive layers is two, and along the thickness direction of the first conductive layer, the two first conductive layers are disposed on opposite sides of the second conductive layer.

[0014] In some embodiments, the tab further includes a conductive composite layer disposed between the first conductive layer and the second conductive layer, and the first conductive layer and the second conductive layer are hot-rolled to form the conductive composite layer.

[0015] In some embodiments, the tab further includes a conductive adhesive layer disposed between the first conductive layer and the second conductive layer, and the conductive adhesive layer adheres and electrically connects the first conductive layer and the second conductive layer.

[0016] In some embodiments, the conductive adhesive layer includes a substrate and conductive particles mixed in the substrate.

[0017] In some embodiments, the material of the substrate is one or more of ethyl cyanoacrylate, epoxy resin, acrylate resin, and polyurethane.

[0018] In some embodiments, the melting temperature of the conductive adhesive layer is greater than or equal to 200°C.

[0019] In some embodiments, a surface of the second conductive layer is at least partially a passivated surface.

[0020] In some embodiments, the thickness of the first conductive layer is 10-100 μm, and the thickness of the second conductive layer is 5-30 μm.

[0021] In some embodiments, the first conductive layer is an aluminum layer and the second conductive layer is a steel layer.

[0022] In some embodiments, the electrochemical device further includes an insulating member connected to the tab, and the peel strength between the tab and the insulating member is greater than 1.5 N / mm.

[0023] In a second aspect, an embodiment of the present application further provides a battery, comprising:

[0024] A shell having a receiving space;

[0025] According to the electrochemical device provided in the first aspect, the electrochemical device is accommodated in the accommodation space.

[0026] In a third aspect, an embodiment of the present application further provides an electrical device, comprising the electrochemical device provided according to the first aspect, the electrochemical device being used to provide electrical energy.

[0027] Compared with the prior art, in the electrochemical device and electrical device provided in the embodiments of the present application, since the second conductive layer has a large tensile strength, the second conductive layer can enhance the overall strength of the pole ear, and the pole ear has better tensile and bending resistance; by setting the tensile strength of the second conductive layer to be greater than the tensile strength of the first conductive layer, when the first conductive layer in the pole ear is damaged by breakage, cracks, etc., the second conductive layer can still conduct electricity to the electrode assembly and external parts, so that the pole ear still has a conductive function, the electrochemical device can still participate in charging and discharging, and the service life of the electrochemical device is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0029] Figure 1 is a schematic diagram of the three-dimensional structure of an electrochemical device provided in one embodiment of the present application;

[0030] Figure 2 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0031] Figure 3 is a schematic structural diagram of an electrochemical device provided in another embodiment of the present application;

[0032] Figure 4 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0033] Figure 5 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0034] Figure 6 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0035] Figure 7 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0036] Figure 8 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0037] Fig. 9 is a schematic diagram of the cross-sectional structure of a tab provided in one embodiment of the present application;

[0038] Fig.10 It is a schematic diagram of the three-dimensional structure of a battery provided in one embodiment of the present application.

[0039] In the attached figure:

[0040] Battery 100; electrochemical device 10; housing 20; receiving space 201;

[0041] Electrode assembly 1; first end 11; second end 12; electrode tab 2; first conductive layer 21; second conductive layer 22; conductive composite layer 23; conductive adhesive layer 24; insulating member 3. DETAILED DESCRIPTION

[0042] The features and exemplary embodiments of various aspects of the application will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the application. However, it is obvious to those skilled in the art that the application can be implemented when some details in these specific details are not needed. The following description of the embodiments is only to provide a better understanding of the application by illustrating the example of the application.

[0043] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The embodiments will be described in detail below in conjunction with the accompanying drawings.

[0044] In one aspect, the present application provides an electrochemical device. In order to better understand the technical solution and technical effects of the present application, specific embodiments will be described in detail below in conjunction with the accompanying drawings.

[0045] See also Figure 1 and Figure 2 An electrochemical device 10 includes an electrode assembly 1 and a tab 2, the tab 2 extending from the electrode assembly 1, the tab 2 including a stacked first conductive layer 21 and a second conductive layer 22, the first conductive layer 21 being electrically connected to the electrode assembly 1, and the first conductive layer 21 and the second conductive layer 22 being electrically conductive; wherein the tensile strength of the second conductive layer 22 is greater than the tensile strength of the first conductive layer 21.

[0046] The electrochemical device 10 provided in the present application can be applied to lithium-ion batteries, lithium-sulfur batteries, sodium-lithium-ion batteries, sodium-ion batteries or magnesium-ion batteries, etc., and the embodiments of the present application are not limited to this. When the electrochemical device 10 is applied to a battery, the electrochemical device 10 is immersed in an electrolyte, and at least two electrochemical devices 10 can be used as a positive electrode sheet and a negative electrode sheet, respectively. The parts of the positive electrode sheet and the negative electrode sheet with active substances constitute the electrode assembly 1 of the electrochemical device 10, and the parts of the positive electrode sheet and the negative electrode sheet without active substances each constitute a pole ear 2. During the charge and discharge process of the battery, the positive electrode active substance and the negative electrode active substance react with the electrolyte. The pole ear 2 is used to connect the electrode terminals to form a current loop.

[0047] The first conductive layer 21 can be electrically connected to the electrode assembly 1 by welding, and the second conductive layer 22 electrically connected to the first conductive layer 21 may not have a direct connection relationship with the electrode assembly 1, and the second conductive layer 22 is electrically connected to the electrode assembly 1 through the first conductive layer 21. The first conductive layer 21 and the second conductive layer 22 may also have a direct connection relationship with the electrode assembly 1, so that the second conductive layer 22 may not be electrically connected to the electrode assembly 1 through the first conductive layer 21. It can be understood by those skilled in the art that the material of the first conductive layer 21 and the material of the second conductive layer 22 can be a single element or a mixture. When the first conductive layer 21 and the second conductive layer 22 are both mixtures, the components of the first conductive layer 21 and the second conductive layer 22 may be different or the same. In the case where the components of the first conductive layer 21 and the second conductive layer 22 are the same, those skilled in the art can adjust the proportion of each component so that the second conductive layer 22 exhibits better tensile strength than the first conductive layer 21.

[0048] When the structure of the electrochemical device 10 is intact and undamaged, the electrode assembly 1 can form a current loop with external parts through the first conductive layer 21 and the second conductive layer 22 in the pole ear 2, and specifically, can form a current loop with the electrode terminal through the first conductive layer 21 and the second conductive layer 22. When the electrochemical device 10 is collided or bent by external force, since the tensile strength of the first conductive layer 21 is less than the tensile strength of the second conductive layer 22, the second conductive layer 22 has better tensile and bending resistance than the first conductive layer 21, and the tensile and bending resistance of the first conductive layer 21 is improved under the support of the second conductive layer 22; when the first conductive layer 21 in the pole ear 2 is broken, cracked or damaged, the second conductive layer 22 can still conduct the electrode assembly 1 and external parts, so that the pole ear 2 still has a conductive function, and the electrochemical device 10 can still participate in charging and discharging.

[0049] In the electrochemical device 10 provided in the present application, since the second conductive layer 22 has a large tensile strength, the second conductive layer 22 can enhance the overall strength of the pole lug 2, and the pole lug 2 has better tensile and bending resistance; by setting the tensile strength of the second conductive layer 22 to be greater than the tensile strength of the first conductive layer 21, the first conductive layer 21 in the pole lug 2 has damage such as breakage and cracks, and the second conductive layer 22 can still conduct electricity between the electrode assembly 1 and external parts, so that the pole lug 2 still has a conductive function, and the electrochemical device 10 can still participate in charging and discharging operations, thereby improving the service life of the electrochemical device 10.

[0050] See also Figure 3, the electrode assembly 1 can be formed by winding the positive electrode sheet and the negative electrode sheet along the central axis L, and the pole ear 2 is connected to the first end 11 of the electrode assembly 1 and extends outward to facilitate the connection of the pole ear 2 to other components. The pole ear 2 connected to the positive electrode sheet and the pole ear 2 connected to the negative electrode sheet are bent and extended in the direction close to the central axis L to facilitate the connection of the pole ear 2 connected to the positive electrode sheet and the pole ear 2 connected to the negative electrode sheet to the same insulating structure. The second conductive layer 22 is at least arranged on one side of the first conductive layer 21 close to the electrode assembly 1, so that the second conductive layer 22 can support the first conductive layer 21, and at the same time disperse the stress of the first conductive layer 21 when it is impacted or squeezed, which is conducive to preventing the first conductive layer 21 from breaking and extending the service life of the pole ear 2. The pole ear 2 is at least partially bent into an arc that bulges toward the central axis L of the electrode assembly 1.

[0051] In some embodiments, the electrochemical device 10 further includes an insulating member 3 connected to the pole tab 2, and the peel strength between the pole tab 2 and the insulating member 3 is greater than 1.5 N / mm at 85°C and 4h. It can be understood by those skilled in the art that the peel strength between the first conductive layer 21 and the insulating member 3, and the peel strength between the second conductive layer 22 and the insulating member 3 may be different. The insulating member 3 is used to insulate the pole tab 2, and the pole tab 2 connected to the positive electrode sheet and the pole tab 2 connected to the negative electrode sheet can be connected to the same insulating member 3, and the insulating member 3 is used to insulate the two. The outer surface of the pole tab 2 can be roughened to increase the peel strength between the pole tab 2 and the insulating member 3.

[0052] See also Figure 4 In some embodiments, the second conductive layer 22 is coated on the outside of the first conductive layer 21. Figure 5 In other embodiments, the first conductive layer 21 is coated on the outside of the second conductive layer 22. That is, one of the first conductive layer 21 and the second conductive layer 22 is coated around the other, so that one of them is completely protected and isolated from external gas, liquid, etc. to a certain extent, thereby reducing or preventing the conductive layer located in the center from being corroded or oxidized.

[0053] When the second conductive layer 22 is coated on the outside of the first conductive layer 21, the second conductive layer 22 can support the first conductive layer 21 from all sides, so that the first conductive layer 21 is not easily damaged by breakage, cracks, etc. When the first conductive layer 21 is coated on the outside of the second conductive layer 22, the first conductive layer 21 in the electrode has more exposed outer surface, which facilitates the connection of the electrode tab 2 to the electrode assembly 1 and external components through the first conductive layer 21.

[0054] See also Figure 6In some other embodiments, the number of the first conductive layer 21 is two, and along the thickness direction of the first conductive layer 21, the two first conductive layers 21 are disposed on opposite sides of the second conductive layer 22.

[0055] It can be understood by those skilled in the art that in order to coat more active materials on the electrode assembly 1 for chemical reaction and improve the overall energy density of the prepared battery, the electrode assembly 1 is usually a sheet structure, so the tab 2 is usually also a sheet structure. Correspondingly, the thickness direction of the first conductive layer 21 and the second conductive layer 22 is the thickness direction of the tab 2. The two layers of the first conductive layer 21 are arranged on opposite sides of the second conductive layer 22, that is, a three-layer stacked structure of the first conductive layer 21-the second conductive layer 22-the first conductive layer 21 is formed. The first conductive layer 21 and the second conductive layer 22 can be stacked together by pressing, laminating, etc. Similarly, the first conductive layer 21 in the tab 2 has a more exposed outer surface, which facilitates the tab 2 to connect the electrode assembly 1 and external components through the first conductive layer 21.

[0056] Those skilled in the art may also set different thicknesses of the two first conductive layers 21 as needed. For example, when the tab 2 is assembled into the battery in a state of being bent in a certain direction, the thickness of the first conductive layer 21 located on the outside may be set to be greater than that of the first conductive layer 21 located on the inside, so that the first conductive layer 21 located on the outside can withstand greater bending stress.

[0057] See also Figure 7 The tab 2 further includes a conductive composite layer 23 disposed between the first conductive layer 21 and the second conductive layer 22 . The conductive composite layer 23 is formed by hot rolling of the first conductive layer 21 and the second conductive layer 22 .

[0058] Hot rolling is a rolling process performed above the recrystallization temperature of the material. The first material of the first conductive layer 21 and the second material of the second conductive layer 22 can be prepared as sheet rolled materials respectively, and then the two rolled materials are stacked together and passed through a hot rolling mill. The pressure applied by the hot rolling mill causes the two to be compressed and deformed into a whole. Under the action of pressure, the surfaces of the first material and the second material are pressed against each other to form a material mixing area, in which the first material and the second material are mixed, and the area is the conductive composite layer 23. It can be understood by those skilled in the art that the conductive composite layer 23 has no obvious boundary with the first conductive layer 21 and the second conductive layer 22 respectively. The conductive composite layer 23 formed by hot rolling is conducive to ensuring that the first conductive layer 21 and the second conductive layer 22 are closely connected, and to a certain extent, it is avoided that there is a gap between the first conductive layer 21 and the second conductive layer 22 due to the action of external force, temperature, etc., which affects the supporting effect of the second conductive layer 22 on the first conductive layer 21, and affects the electrical path effect between the first conductive layer 21 and the second conductive layer 22.

[0059] See also Figure 8 and Fig. 9 The tab 2 further includes a conductive adhesive layer 24 disposed between the first conductive layer 21 and the second conductive layer 22 , and the conductive adhesive layer 24 adheres and electrically connects the first conductive layer 21 and the second conductive layer 22 .

[0060] The conductive adhesive layer 24 is made of a material that is both sticky and conductive, and specifically can be conductive glue. When bonding the first conductive layer 21 and the second conductive layer 22, the conductive adhesive layer 24 can have a certain fluidity so as to change along with the structural state of the tab 2. By bonding the first conductive layer 21 and the second conductive layer 22 through the conductive adhesive layer 24, the stability of the connection between the first conductive layer 21 and the second conductive layer 22 can be improved.

[0061] The conductive adhesive layer 24 includes a substrate and conductive particles mixed in the substrate. The substrate is made of a viscous material, and the first conductive layer 21 and the second conductive layer 22 are conductive through one or more conductive particles in the substrate. Optionally, the material of the substrate is one or more of ethyl cyanoacrylate, epoxy resin, acrylate resin and polyurethane. Optionally, the material of the conductive particles can be aluminum powder, silver powder, copper powder, iron powder, nickel powder, zinc powder, etc. Those skilled in the art can select a suitable substrate and conductive particles, and adjust the mixing ratio of the substrate and the conductive particles so that the prepared conductive adhesive layer 24 has better conductivity and adhesion. Optionally, the adhesion of the conductive adhesive layer 24 is greater than 15N / 8mm, and the peel strength of the first conductive layer 21 and the second conductive layer 22 is greater than 6N / 15mm, so as to ensure that the first conductive layer 21 and the second conductive layer 22 can support each other and be electrically conductive. Optionally, the peel strength of the conductive adhesive layer 24 and the first conductive layer 21 is greater than the peel strength of the first conductive layer 21 and the second conductive layer 22.

[0062] It is understood by those skilled in the art that since the tab 2 needs to be electrically connected to other external parts and needs to participate in other processing steps in the preparation of the battery, for example, in the process of setting a seal at the tab 2 by ultrasonic welding, and in the process of connecting the tab 2 to the current collector by ultrasonic welding, in these processing steps, the temperature of the tab 2 will be much higher than the room temperature, so the conductive adhesive layer 24 also needs to have better heat resistance. In some embodiments, the melting temperature of the conductive adhesive layer 24 is greater than or equal to 200°C to ensure that the conductive adhesive layer 24 will not be denatured during the subsequent processing of the electrochemical device 10, and to avoid the delamination phenomenon in the tab 2 to a certain extent.

[0063] Since the tab 2 will inevitably contact the electrolyte, the materials of the first conductive layer 21, the second conductive layer 22 and the conductive adhesive layer 24 also need to be resistant to electrolyte corrosion. In some embodiments, the outer surfaces of the first conductive layer 21 and the second conductive layer 22 are passivated to improve the corrosion resistance of the tab 2 in the electrolyte. In other embodiments, only the outer surface of the tab 2 is passivated. For example, in one embodiment, the tab 2 includes only one first conductive layer 21 and one second conductive layer 22, and only the surfaces of the first conductive layer 21 and the second conductive layer 22 that are separated from each other are passivated. For another example, in another embodiment, the tab 2 includes two first conductive layers 21 and one second conductive layer 22, and the first conductive layer 21 is disposed on both sides of the second conductive layer 22, and only the side of the first conductive layer 21 away from the second conductive layer 22 is passivated. Only part of the surface of the first conductive layer 21 and the second conductive layer 22 is passivated, thereby reducing the preparation cost.

[0064] In another embodiment, at least part of the surface of the second conductive layer 22 is a passivated surface. Those skilled in the art will appreciate that the second conductive layer 22 may also be passivated to improve the corrosion resistance of the second conductive layer 22 in the electrolyte.

[0065] In some embodiments, the first conductive layer 21 is an aluminum layer, and the second conductive layer 22 is a steel layer. The tensile strength of the steel layer with a thickness of 50 μm is ≥ 300 N / m, which is higher than the tensile strength of the aluminum layer with the same thickness. Compared with the pole lug 2 made of only aluminum, the pole lug 2 with the same thickness and the steel layer has better tensile strength. Among the pole lugs 2 with the same tensile strength, the pole lug 2 with the steel layer is thinner than the pole lug 2 made of only aluminum. When ultrasonically welding the sealant, it can avoid the generation of leakage channels to a certain extent, thereby improving product quality.

[0066] Optionally, the surface of the steel layer may be subjected to a chromium solution passivation treatment to improve the electrochemical corrosion resistance of the steel layer.

[0067] In some embodiments, the thickness of the first conductive layer 21 is 10 to 100 μm, and the thickness of the second conductive layer 22 is 5 to 30 μm. The thickness of the second conductive layer 22 is less than at least half of the thickness of the first conductive layer 21. It can be understood by those skilled in the art that when there are multiple first conductive layers 21, the thickness of each first conductive layer 21 can be reduced accordingly so that the thickness of the entire pole ear 2 is within a preset range. Optionally, the number of first conductive layers 21 is two layers, and the thickness of the first conductive layer 21 is 10 to 50 μm. Too thick first conductive layers 21 and second conductive layers 22 will increase the overall thickness of the pole ear 2, increase the probability of leakage channels during ultrasonic welding of sealants to a certain extent, and reduce product quality; too thin first conductive layers 21 and second conductive layers 22 will cause the overall tensile strength of the pole ear 2 to be insufficient, and it is easy to be damaged under the action of external forces.

[0068] To verify the beneficial effects of the above-mentioned embodiments of the tab 2, please refer to the following embodiments.

[0069] Example 1

[0070] An aluminum foil with a thickness of 80 um and a steel foil with a thickness of 20 um are fixed together by hot rolling to prepare a metal strip.

[0071] Example 2

[0072] Take an aluminum foil with a thickness of 75um and a steel foil with a thickness of 15um, and fix the aluminum foil and the steel foil together with a conductive glue with a thickness of 10um to prepare a metal strip. The conductive glue is epoxy resin and aluminum powder.

[0073] Example 3

[0074] Take an aluminum foil with a thickness of 40um and a steel foil with a thickness of 20um, fix the steel foil between two layers of aluminum foil by hot rolling, and prepare a metal strip.

[0075] Example 4

[0076] Take an aluminum foil with a thickness of 30um and a steel foil with a thickness of 20um, and fix the steel foil between the two layers of aluminum foils with a conductive glue with a thickness of 10um to prepare a metal strip. The conductive glue is epoxy resin and aluminum powder.

[0077] Example 5

[0078] Aluminum foil with a thickness of 90 um and steel foil with a thickness of 10 um were fixed together by hot rolling to prepare a metal strip.

[0079] Example 6

[0080] Take an aluminum foil with a thickness of 80um and a steel foil with a thickness of 10um, and bond and fix the aluminum foil and the steel foil together with a conductive glue with a thickness of 10um to prepare a metal strip. The conductive glue is epoxy resin and aluminum powder.

[0081] Comparative Example 1

[0082] Take an aluminum foil with a thickness of 100 um and prepare it into a metal strip.

[0083] The metal strips prepared in Examples 1 to 6 and Comparative Example 1 were cut into strips with a width of 15 mm and a length of 150 mm for tensile testing and current capacity testing. In the tensile test, the clamp spacing of the tensile strips in the tensile machine was 100 mm, and the tensile speed was 30 mm / min. In the current capacity test, the current capacity of the tab = Tab 宽度 *Tab 厚度 *Tab 载流系数 ; Metal strip current carrying capacity = the sum of the current carrying capacity of different metal layers. Tab represents the tab, and the current carrying coefficient of Al material is 5A / mm 2 , the current carrying coefficient of Cu material is 8A / mm 2 , Ni material current carrying coefficient is 2A / mm 2 , the current carrying coefficient of steel is 3.2A / mm 2 , the current carrying coefficient of conductive glue is 0.08-0.1A / mm 2 Please refer to Table 1 for specific test results.

[0084] Table 1 Tensile test results of metal strips

[0085] Group Preparation process thickness Tensile strength(MPa) Current capacity(A) Example 1 Hot Rolling 100um 213 6.96 Example 2 Bonding 100um 190 6.36 Example 3 Hot Rolling 100um 220 6.96 Example 4 Bonding 100um 202 5.49 Example 5 Hot Rolling 100um 135 7.23 Example 6 Bonding 100um 130 6.49 Comparative Example 1 none 100um 74.7 7.5

[0086] Comparing Examples 1 to 6 with Comparative Example 1, it can be seen that compared with the metal strip prepared only from aluminum foil, the metal strip with steel foil has better tensile strength and less effect on the flow capacity. Comparing Example 1 and Example 2, it can be seen that the prepared metal strip has good flow capacity and tensile strength regardless of whether the aluminum foil and the steel foil are fixed by hot rolling or by a conductive adhesive layer. Comparing Example 1 and Example 3, and Comparing Example 2 and Example 4, it can be seen that the metal strip with a single-layer aluminum foil structure and the metal strip with a double-layer aluminum foil structure have good flow capacity and tensile strength. Comparing Example 1 and Example 5, and Comparing Example 2 and Example 6, it can be seen that when the steel foil is thicker, the tensile strength of the metal strip is greatly improved, and the effect on the flow capacity is not significant.

[0087] The metal strips prepared in Examples 1 to 6 and Comparative Example 1 were cut into strips with a width of 15 mm and a length of 150 mm for bending test. At room temperature, the metal strips were bent 180°, and the number of bending times at which the aluminum foil or steel foil in the metal strip broke was recorded. Please refer to Table 2 for specific results.

[0088] Table 2 Bending test results of metal strips

[0089] Group Preparation process thickness Fracture bending times Example 1 Hot Rolling 100um 198 Example 2 Bonding 100um 161 Example 3 Hot Rolling 100um 205 Example 4 Bonding 100um 203 Example 5 Hot Rolling 100um 110 Example 6 Bonding 100um 108 Comparative Example 1 none 100um 50

[0090] Comparing Examples 1 to 6 with Comparative Example 1, it can be seen that compared with the metal strip prepared only from aluminum foil, the number of fracture and bending of the metal strip with steel foil added is greatly increased, and it has better anti-bending ability, which can reduce or avoid the problem of fracture and failure of the pole ear 2 caused by external force collision. Comparing Example 1 and Example 2, it can be seen that the number of fracture and bending of the prepared metal strip can be greatly improved compared with Comparative Example 1. Comparing Example 1 and Example 3, and Comparing Example 2 and Example 4, it can be seen that the metal strip with a single-layer aluminum foil structure and the metal strip with a double-layer aluminum foil structure have good anti-bending ability. Comparing Example 1 and Example 5, and Comparing Example 2 and Example 6, it can be seen that when the steel foil is thicker, the number of fracture and bending is greatly improved. In some cases, the aluminum foil of the metal strip breaks while the steel foil does not break, which does not affect the state of the electrical path.

[0091] The metal strip prepared in Example 2 was cut into strips with a width of 15 mm and a length of 150 mm for high temperature resistance test. Different metal strips were welded with seals at different welding temperatures to test whether a leakage channel was generated between the seal and the metal strip, wherein the material of the seal was polyethylene. The welded metal strip was bent 90° and placed in an electrolyte to test whether the aluminum foil and the steel foil in the metal strip were separated and delaminated. Please refer to Table 3 for specific results.

[0092] Table 3 Heat resistance and corrosion resistance test results of metal strips

[0093]

[0094]

[0095] Through the above experiments, it can be known that when the seal is welded at 200°C, no leakage channel will be generated between the seal and the tab, and no delamination phenomenon will occur in the tab, proving that the tab provided by the present application can still effectively bond the first conductive layer and the second conductive layer under the processing of the welding temperature of 200°C and the corrosion of the electrolyte. When the welding temperature is above 220°C, the seal begins to be slightly burned, but there is still no delamination phenomenon in the tab, proving that the conductive adhesive layer can still effectively bond the first conductive layer and the second conductive layer.

[0096] In a second aspect, the present application also provides a battery. Fig.10The battery 100 includes a housing 20 having a receiving space 201 , and the electrochemical device 10 provided in the first aspect, and the electrochemical device 10 is received in the receiving space 201 .

[0097] At least two electrochemical devices 10 are used as positive electrode sheets and negative electrode sheets respectively, and the positive electrode sheets and negative electrode sheets can be arranged in a winding or stacked manner in the housing 20. Multiple batteries 100 can be connected in series, in parallel, or in hybrid connection to form a whole, and charge and discharge are performed externally through the whole, wherein hybrid connection means that multiple batteries 100 are connected in series and in parallel.

[0098] The relevant structure of the electrochemical device 10 in the battery 100 can be found in the electrochemical device 10 provided in the above embodiments, and will not be described in detail here.

[0099] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.

[0100] To verify the beneficial effects of the above-mentioned embodiments of the tab 2 and the battery 100 including the above-mentioned tab 2, please refer to the following embodiments.

[0101] Example 7

[0102] 1) Bonding an aluminum foil with a thickness of 60 μm and a steel foil with a thickness of 20 μm together with conductive glue to prepare a tab, wherein the thickness of the conductive glue is 10 μm, the aluminum foil is used as the first conductive layer, and the steel foil is used as the second conductive layer;

[0103] 2) The prepared electrode tab was welded to an electrode assembly having a length of 91 mm, a width of 66 mm, and a thickness of 6.0 mm to prepare an electrochemical device.

[0104] Comparative Example 2

[0105] 1) Take an aluminum foil with a thickness of 90 μm and prepare it into a tab;

[0106] 2) The prepared electrode tab was welded to an electrode assembly having a length of 91 mm, a width of 66 mm, and a thickness of 6.0 mm to prepare an electrochemical device.

[0107] The difference between Comparative Example 2 and Example 7 is that the tabs in Comparative Example 2 are made of aluminum foil only, while the tabs in Example 7 are made of aluminum foil and steel foil bonded by a conductive adhesive layer.

[0108] Example 8

[0109] 1) Bonding an aluminum foil with a thickness of 60 μm and a steel foil with a thickness of 20 μm together with conductive glue to prepare a tab, wherein the thickness of the conductive glue is 10 μm, the aluminum foil is used as the first conductive layer, and the steel foil is used as the second conductive layer;

[0110] 2) The prepared electrode tab was welded to an electrode assembly having a length of 87 mm, a width of 64 mm, and a thickness of 4.8 mm to prepare an electrochemical device.

[0111] The difference between Example 7 and Example 8 is that the sizes of their electrode assemblies are different.

[0112] Comparative Example 3

[0113] 1) Take an aluminum foil with a thickness of 90 μm and prepare it into a tab;

[0114] 2) The prepared electrode tab was welded to an electrode assembly having a length of 87 mm, a width of 64 mm, and a thickness of 4.8 mm to prepare an electrochemical device.

[0115] The difference between Comparative Example 3 and Example 8 is that the tabs in Comparative Example 3 are made of aluminum foil only, while the tabs in Example 8 are made of aluminum foil and steel foil bonded by a conductive adhesive layer.

[0116] The electrochemical devices prepared in Example 7, Example 8, Comparative Example 2 and Comparative Example 3 were assembled into batteries, and 10 repetitions were set for each example. The side of the electrode assembly close to the pole ear was facing the steel plate, and the battery was dropped from a height of 10 cm, and repeated 5000 times. The voltage and internal resistance of the battery were measured after every 1000 drops. During the test, the appearance of the battery cell was checked. If the battery had abnormal conditions such as leakage or fire, the drop was stopped. The battery cells that completed the drop test were disassembled, and the proportion of broken aluminum foil in the pole ear was counted.

[0117] Please refer to Table 4, which shows the percentage of aluminum foil breakage in the batteries that have undergone the drop test.

[0118] Table 4 Aluminum foil fracture ratio

[0119] Group Aluminum foil breakage ratio Example 7 0 / 10 Comparative Example 2 7 / 10 Example 8 0 / 10 Example 8 0 / 10

[0120] It can be seen from Table 4 that the tabs provided with steel foil have better anti-collision ability and can significantly reduce the proportion of aluminum foil breakage.

[0121] In a third aspect, the present application further provides an electrical device, comprising the electrochemical device provided in the first aspect, and the electrochemical device is used to provide electrical energy.

[0122] Specific product types of electrical devices include but are not limited to mobile terminals, smart wearables, power tools, electric vehicles, mobile power supplies, etc.

[0123] Since the battery has the aforementioned beneficial effects, the electrical device has higher safety and reliability and longer service life.

[0124] In addition, the term "and / or" in this article is only a description of the association relationship between the associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0125] It should be understood that in the embodiment of the present application, "B corresponding to A" means that B is associated with A, and B can be determined according to A. However, it should also be understood that determining B according to A does not mean determining B only according to A, and B can also be determined according to A and / or other information.

[0126] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. An electrochemical device, characterized in that: include: An electrode assembly, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet and the negative electrode sheet are wound around the central axis of the electrode assembly; A tab extending from the electrode assembly, the tab comprising a first conductive layer and a second conductive layer stacked together, the first conductive layer being electrically connected to the electrode assembly, the first conductive layer and the second conductive layer being electrically conductive, and the second conductive layer being at least disposed on one side of the first conductive layer close to the central axis of the electrode assembly; The tensile strength of the second conductive layer is greater than that of the first conductive layer, the tab further comprises a conductive composite layer disposed between the first conductive layer and the second conductive layer, and the first conductive layer and the second conductive layer are hot-rolled to form the conductive composite layer.

2. The electrochemical device according to claim 1, characterized in that The electrode assembly includes a first end and a second end, the first end and the second end are arranged opposite to each other along a first direction, the electrode tab is bent and extended from the first end toward a direction close to the central axis of the electrode assembly, and the extension direction of the central axis is perpendicular to the first direction.

3. The electrochemical device according to claim 2, characterized in that The electrode tab is at least partially bent into an arc shape protruding toward the central axis of the electrode assembly.

4. The electrochemical device according to claim 1, characterized in that The second conductive layer is coated on the outside of the first conductive layer, or the first conductive layer is coated on the outside of the second conductive layer.

5. The electrochemical device according to claim 1, characterized in that The number of the first conductive layers is two. Along the thickness direction of the first conductive layer, the two first conductive layers are arranged on two opposite sides of the second conductive layer.

6. The electrochemical device according to any one of claims 1 to 5, characterized in that: At least a portion of the surface of the second conductive layer is a passivated surface.

7. The electrochemical device according to any one of claims 1 to 5, characterized in that The thickness of the first conductive layer is 10-100 μm, and the thickness of the second conductive layer is 5-30 μm.

8. The electrochemical device according to any one of claims 1 to 5, characterized in that The first conductive layer is an aluminum layer, and the second conductive layer is a steel layer.

9. The electrochemical device according to any one of claims 1 to 5, characterized in that: The electrochemical device further includes an insulating member connected to the tab, and the peel strength between the tab and the insulating member is greater than 1.5 N / mm.

10. An electrical device, characterized in that: The invention comprises an electrochemical device according to any one of claims 1 to 9, wherein the electrochemical device is used to provide electrical energy.

Citation Information

Patent Citations

  • Electrochemical device and electronic apparatus

    CN114447530A

  • Positive pole lug of lithium ion battery

    CN203150646U