Secondary battery and power-using device
By designing the positive and negative electrode plates of lithium iron phosphate batteries and controlling the amount of VC added, the problem of difficulty in balancing cycle life and energy density in the existing technology is solved, achieving higher cycle life and energy density, and meeting the storage requirements. High cycle demand in areas such as energy and commercial vehicles.
Patent Information
- Application Number
- CN202211076998.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-05
AI Technical Summary
Existing lithium iron phosphate batteries are difficult to balance between cycle life and energy density, and cannot meet the needs of long cycle life and high energy density, especially in the use cycle of energy storage and commercial vehicles. Cost recovery and profitability needs.
By controlling the design of the positive and negative electrode plates and the amount of VC added, it is ensured that the positive active material has an olivine structure, the compacted density and thickness are within a specific range, the negative active material is artificial graphite, and the vinylene carbonate film-forming additive content is Within a reasonable range, ensure that the capacity does not decrease prematurely due to lithium precipitation during the cycle, and a reasonable CB value is designed to ensure cycle performance.
It achieves higher cycle life and service life of lithium iron phosphate batteries, has high energy density, meets the high cycle needs of energy storage, engineering vehicles and commercial vehicles, and improves the overall performance of the battery.
Smart Images

Figure BDA0003831931240000091 
Figure BDA0003831931240000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a secondary battery and an electrical device. Background Art
[0002] Lithium-ion batteries have outstanding advantages such as high energy density, long cycle life, high operating voltage, low self-discharge rate, and environmental friendliness, and can be used as an ideal power source for multi-purpose power supply. As a mainstream lithium battery, lithium iron phosphate batteries have more outstanding cost advantages, better safety performance and longer cycle life compared to lithium batteries using other positive electrode materials, such as ternary lithium batteries and lithium cobalt oxide batteries. Lithium iron phosphate batteries are also widely used due to their outstanding advantages. When used in passenger cars, the designed pole pieces and the batteries made with controlled VC content often only need a cycle life of 2000 to 3000 times to meet the 8 to 10 years of use of passenger cars. Lithium batteries for passenger cars require higher energy density, so pole piece design and VC addition often need to consider the balance between energy density and cycle life.
[0003] Because of its outstanding cost advantage, lithium iron phosphate batteries are also used in fields such as energy storage, engineering vehicles and commercial vehicles. The priority in these fields is to achieve cost recovery or even profit within the entire battery life cycle, so it often requires a 10-15 year service life and a cycle life of 4,000-6,000 or even higher. These existing lithium iron phosphate batteries cannot have both high cycle life and energy density, so a decision solution is urgently needed. Summary of the invention
[0004] The purpose of the present invention is to provide a secondary battery with excellent energy density, cycle life and service life in view of the shortcomings of the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A secondary battery comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode active material, the positive electrode active material is an olivine structure, and the positive electrode sheet and the negative electrode sheet satisfy the following relationship:
[0007] 0.25 <PDc*Tc<0.42;0.1<PDa*Ta<0.2;0.75<(CB-1.1) / VC<1.5;
[0008] Wherein, PDc is the compaction density of the positive electrode sheet;
[0009] Wherein, PDa is the compaction density of the negative electrode sheet;
[0010] Wherein, Tc is the thickness of the positive electrode sheet;
[0011] Wherein, Ta is the thickness of the negative electrode plate;
[0012] Wherein, CB is the excess ratio of negative electrode capacity per unit area to positive electrode capacity;
[0013] Among them, VC is the content of vinylene carbonate, a film-forming additive for lithium battery electrolyte, in the electrolyte.
[0014] Preferably, the positive electrode plate comprises a positive electrode current collector and a positive electrode active coating disposed on at least one surface of the positive electrode current collector, the positive electrode active coating comprises a positive electrode active material, a conductive agent, a binder and a dispersant, and the weight ratio of the positive electrode active material, the conductive agent, the binder and the dispersant is 80-99:1-20:1-5:1-5.
[0015] Preferably, the chemical formula of the positive electrode active material is LiFe x M 1-x PO4, wherein M is one or a combination of Mg, Ni, V, and Mn, and 0<x<1.
[0016] Preferably, the surface of the positive electrode active material is coated with a carbon coating layer, and the particle size distribution of the positive electrode active material satisfies the following relationship: 0.5 μm <Dc50<5μm,1<(Dc90-Dc10) / Dc50<8。
[0017] Preferably, the negative electrode plate comprises a negative electrode current collector and a negative electrode active coating disposed on at least one surface of the negative electrode current collector, the negative electrode active coating comprises a negative electrode active material, a conductive agent, a binder and a dispersant, and the weight ratio of the negative electrode active material, the conductive agent, the binder and the dispersant is 85-99:1-15:1-5:1-5.
[0018] Preferably, the negative electrode active material includes at least one of artificial graphite, natural graphite, silicon, silicon oxide, tin, and lithium titanate.
[0019] Preferably, the negative electrode active material is artificial graphite, and the particle size distribution satisfies the following relationship: 3 μm <Da50<30μm,0.5<(Da90-Da10) / Da50<3。
[0020] Preferably, the secondary battery further comprises a separator, an electrolyte and a shell, wherein the separator is used to separate the positive electrode sheet from the negative electrode sheet, and the shell is used to package the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte.
[0021] Preferably, the compaction density PDc of the positive electrode sheet is in the range of 2.2 g / cm 3 <PDc<2.4g / cm 3The thickness Tc of the positive electrode sheet is in the range of 0.065 mm. <Tc<0.185mm。
[0022] Preferably, the compaction density PDa of the negative electrode sheet is in the range of 1.45 g / cm 3 <PDa<1.6g / cm 3 The thickness Ta of the negative electrode sheet ranges from 0.065 mm <Ta<0.185mm。
[0023] Preferably, the value range of CB is 1.12﹤CB﹤1.2.
[0024] Preferably, the value range of VC is 2% < VC < 8%.
[0025] The second purpose of the present invention is to provide an electrical device with good quality and service life in view of the shortcomings of the prior art.
[0026] In order to achieve the above object, the present invention adopts the following technical solutions:
[0027] An electrical device comprises the secondary battery mentioned above.
[0028] Compared with the prior art, the beneficial effect of the present invention is that the present invention controls the design of the positive and negative electrode plates and the amount of VC added, so that the lithium iron phosphate battery has a higher cycle life and service life, and has the advantages of high energy density to meet the growing needs of energy storage, engineering vehicles and commercial vehicles. DETAILED DESCRIPTION
[0029] A secondary battery comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode active material, the positive electrode active material is an olivine structure, and the positive electrode sheet and the negative electrode sheet satisfy the following relationship:
[0030] 0.25 <PDc*Tc<0.42;0.1<PDa*Ta<0.2;0.75<(CB-1.1) / VC<1.5;
[0031] Wherein, PDc is the compaction density of the positive electrode sheet;
[0032] Wherein, PDa is the compaction density of the negative electrode sheet;
[0033] Wherein, Tc is the thickness of the positive electrode sheet;
[0034] Wherein, Ta is the thickness of the negative electrode plate;
[0035] Wherein, CB is the excess ratio of negative electrode capacity per unit area to positive electrode capacity;
[0036] Among them, VC is the content of vinylene carbonate, a film-forming additive for lithium battery electrolyte, in the electrolyte.
[0037] The present invention controls the design of the positive and negative electrode plates and the amount of VC added, so that the lithium iron phosphate battery can obtain a higher cycle life and service life. Specifically, the present invention discloses a pole piece design for a lithium iron phosphate battery, which uses a lower compaction density to make the structure of the positive and negative electrode plate materials more complete and ensure a higher liquid retention amount. The thickness of the corresponding positive and negative electrode plates is also within the preferred range. At the same time, the design of high CB value can also ensure that the capacity does not drop prematurely due to lithium precipitation during the cycle. Too low VC content will affect the integrity of SEI film formation during the cycle period, thereby affecting the cycle performance. Too high VC content will excessively consume negative electrode graphite, thereby causing excessive and insufficient negative electrode during the cycle period to cause lithium precipitation, which will also affect the cycle life. Therefore, the VC content under a specific CB value should also be controlled within a reasonable range. Within the specified range, the battery has excellent cycle performance and can meet the increasingly high cycle requirements of energy storage, engineering vehicles and commercial vehicles.
[0038] Among them, the electrode thickness represented by Tc and Ta is the total thickness of the double-sided active material coating after removing the foil thickness.
[0039] In some embodiments, the positive electrode plate includes a positive current collector and a positive active coating disposed on at least one surface of the positive current collector, and the positive active coating includes a positive active material, a conductive agent, a binder and a dispersant. The weight ratio of the positive active material, the conductive agent, the binder and the dispersant is 80-99:1-20:1-5:1-5. Preferably, the weight ratio of the positive active material, the conductive agent, the binder and the dispersant is 80-99:1-20:1-5:1-5, 80-95:3-20:2-5:2-5, 80-92:3-20:2-5:2-5, 80-95:5-20:3-5:3-5. Among them, the conductive agent includes one or more of Ketjen black, mesophase carbon microspheres, activated carbon, graphite, conductive carbon black, acetylene black, carbon fiber, carbon nanotubes, graphene, etc.; the binder includes one or more of vinylidene fluoride, hexafluoropropylene, pentafluoropropylene, tetrafluoropropylene, trifluoropropylene, perfluorobutylene, hexafluorobutadiene, hexafluoroisobutylene, trifluoroethylene, chlorotrifluoroethylene and tetrafluoroethylene; the dispersant includes one or more of carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, and casein.
[0040] In some embodiments, the chemical formula of the positive electrode active material is LiFe x M 1-xPO4, wherein M is one or a combination of Mg, Ni, V, and Mn, and 0<x<1. Doping lithium iron phosphate with elements can improve the structural stability of iron phosphate, thereby improving the performance of the positive electrode active material and achieving a high cycle life.
[0041] In some embodiments, the surface of the positive electrode active material is coated with a carbon coating layer, and the particle size distribution of the positive electrode active material satisfies the following relationship: 0.5 μm <Dc50<5μm,1<(Dc90-Dc10) / Dc50<8。
[0042] D in positive electrode active material 50 If it is too large, the porosity of the electrode will be too large, the compaction density will be too low, and the capacity density will be too low; D 50 If it is too small, the electrode porosity will be too small, the compaction density will be too high, the electrode liquid retention performance will be poor, the dynamic performance will be poor, and the high rate performance will be poor; D 50 The pole piece within the range can meet the requirements of high energy density and high rate performance at the same time. (Dc 90 -Dc 10 ) / Dc 50 It reflects the degree of discreteness of the particle size distribution of the positive electrode active material, which will affect the uniformity of the pores of the positive electrode sheet. If the positive electrode particle size distribution satisfies the relationship, the pore size distribution of the positive electrode sheet is relatively uniform, the battery consistency is good, and the electrochemical performance and safety performance are good. If the positive electrode particle size distribution does not satisfy the relationship, the pore size distribution of the positive electrode sheet is relatively uneven, the battery consistency is poor, and the electrochemical performance and safety performance are poor. A carbon coating layer is arranged on the surface of the positive electrode active material, which can improve the conductivity of the positive electrode active material. The particle size of the positive electrode active material has a certain fineness, so that the positive electrode active material can be evenly distributed in the positive electrode sheet, so that the performance of the positive electrode sheet is better.
[0043] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active coating disposed on at least one surface of the negative electrode current collector, the negative electrode active coating includes a negative electrode active material, a conductive agent, a binder and a dispersant, and the weight ratio of the negative electrode active material, the conductive agent, the binder and the dispersant is 85-99:1-15:1-5:1-5. Preferably, the weight ratio of the negative electrode active material, the conductive agent, the binder and the dispersant is 80-99:1-20:1-5:1-5, 80-95:3-20:2-5:2-5, 80-92:3-20:2-5:2-5, 80-95:5-20:3-5:3-5. Among them, the conductive agent includes one or more of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanotubes, and graphene; the binder includes one or more of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin, and nylon; the dispersant includes one or more of carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, and casein.
[0044] In some embodiments, the negative electrode active material includes at least one of artificial graphite, natural graphite, silicon, silicon oxide, tin, and lithium titanate.
[0045] In some embodiments, the negative electrode active material is artificial graphite, and the particle size distribution satisfies the following relationship: 3 μm <Da50<30μm,0.5<(Da90-Da10) / Da50<3。
[0046] D in negative electrode active material 50 If it is too large, the porosity of the electrode will be too large, the compaction density will be too low, and the capacity density will be too low; D 50 If it is too small, the electrode porosity will be too small, the compaction density will be too high, the electrode liquid retention performance will be poor, the dynamic performance will be poor, and the high rate performance will be poor; D 50 The pole piece within the range can meet the requirements of high energy density and high rate performance at the same time. 90 -Da 10 ) / Da 50It reflects the degree of discreteness of the particle size distribution of the negative electrode active material, which will affect the uniformity of the pores of the negative electrode plate. If the negative electrode particle size distribution satisfies the relationship, the pore size distribution of the negative electrode plate is more uniform, the battery consistency is better, and the electrochemical performance and safety performance are good. If the negative electrode particle size distribution does not satisfy the relationship, the pore size distribution of the negative electrode plate is more uneven, the battery consistency is poor, and the electrochemical performance and safety performance are poor.
[0047] In some embodiments, the secondary battery further includes a separator, an electrolyte and a shell, wherein the separator is used to separate the positive electrode plate and the negative electrode plate, and the shell is used to install and package the positive electrode plate, the negative electrode plate, the separator and the electrolyte. Among them, the separator is one of a polypropylene separator and a polybutylene separator. Among them, the preparation method of the electrolyte is to mix EC, PC and DEC (weight ratio of 1:1:1) under a dry argon environment, add LiPF6 and mix evenly, wherein the concentration of LiPF6 is 1.15 mol / L. Based on the total weight of the electrolyte, 3% of fluoroethylene carbonate is added to the electrolyte. The material of the shell is stainless steel or aluminum-plastic film.
[0048] In some embodiments, the compaction density PDc of the positive electrode sheet is in the range of 2.2 g / cm 3 <PDc<2.4g / cm 3 The compaction density PDc of the positive electrode sheet can be in the range of 2.2 g / cm 3 <PDc<2.4g / cm 3 , 2.2g / cm 3 <PDc<2.25g / cm 3 , 2.25g / cm 3 <PDc<2.4g / cm 3 .
[0049] In some embodiments, the compaction density PDa of the negative electrode sheet is in the range of 1.45 g / cm 3 <PDa<1.6g / cm 3 The compaction density PDa of the negative electrode sheet ranges from 1.45 g / cm 3 <PDa<1.5g / cm 3 , 1.5g / cm 3 <PDa<1.55g / cm 3 , 1.55g / cm 3 <PDa<1.6g / cm 3 .
[0050] In some embodiments, the thickness Tc of the positive electrode plate ranges from 0.065 mm < Tc < 0.185 mm. The thickness Tc of the positive electrode plate ranges from 0.065 mm < Tc < 0.090 mm, 0.090 mm < Tc < 0.100 mm, 0.100 mm < Tc < 0.185 mm.
[0051] In some embodiments, the thickness Ta of the negative electrode plate ranges from 0.065 mm < Ta < 0.185 mm. The thickness Ta of the negative electrode plate ranges from 0.065 mm < Ta < 0.090 mm, 0.090 mm < Ta < 0.100 mm, 0.100 mm < Ta < 0.185 mm.
[0052] In some embodiments, the value range of CB is 1.12 < CB < 1.2. The value range of CB is 1.12 < CB < 1.15, 1.15 < CB < 1.16, 1.16 < CB < 1.18, 1.18 < CB < 1.2.
[0053] In some embodiments, the value range of VC is 2% < VC < 8%. The value range of VC is 2% < VC < 4%, 4% < VC < 6%, 6% < VC < 8%.
[0054] In some embodiments, the value of PDc is 2.2 g / cm 3 、2.23 g / cm 3 、2.25 g / cm 3 、2.28 g / cm 3 、2.29 g / cm 3 、2.3 g / cm 3 、2.35 g / cm 3 、2.37 g / cm 3 、2.39 g / cm 3 、2.4 g / cm 3 , the value of Pda is 1.45 g / cm 3 、1.48 g / cm 3 、1.49 g / cm 3 、1.52 g / cm 3 、1.53 g / cm 3 、1.57 g / cm 3 、1.59 g / cm 3 、1.6 g / cm 3; The values of Tc are 0.065mm, 0.068mm, 0.072mm, 0.085mm, 0.091mm, 0.098mm, 0.1mm, 0.13mm, 0.15mm, 0.16mm, 0.17mm, 0.175mm, 0.18mm, 0.185mm. The values of Ta are 0.065mm, 0.068mm, 0.072mm, 0.085mm, 0.091mm, 0.098mm, 0.1mm, 0.13mm, 0.15mm, 0.16mm, 0.17mm, 0.175mm, 0.18mm, 0.185mm. The values of CB are 1.122, 1.124, 1.126, 1.128, 1.129. The values of VC are 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.075, 0.078, and 0.079.
[0055] In some embodiments, the separator can be any material suitable for lithium-ion battery separators in the art, for example, it can be a combination of one or more of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fibers, etc., but not limited to.
[0056] The lithium-ion battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. Among them, the electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in anti-overcharge electrolytes; it can also be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; it can also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to at least one of film-forming additives, conductive additives, flame retardant additives, anti-overcharge additives, additives for controlling the content of H2O and HF in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.
[0057] An electrical device, comprising the above-mentioned secondary battery. The electrical device of the present application may include, but is not limited to: a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini CD, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.
[0058] The present invention will be described in further detail below in conjunction with specific implementation modes, but the implementation modes of the present invention are not limited thereto.
[0059] Example 1
[0060] 1. Preparation of positive electrode sheet: Mix positive electrode material powder, conductive carbon black, binder and dispersant PVDF in a ratio of 97:1:1:1, add dry NMP, and stir evenly to obtain cathode slurry. Apply the slurry on the current collector and dry it at 80-120℃, and finally cold press and cut it to obtain positive electrode sheet for use.
[0061] 2. Preparation of negative electrode sheet: artificial graphite powder, conductive carbon black, binder SBR and dispersant CMC are mixed in a ratio of 96.7:1:1.4:0.9, then deionized water is added and stirred evenly to obtain anode slurry. The slurry is coated on the current collector and air-dried at 80-120°C, and finally cold-pressed and cut to obtain negative electrode sheets for use.
[0062] 3. Preparation of electrolyte:
[0063] Lithium hexafluorophosphate (LiPF6) is dissolved in a mixed solvent of dimethyl carbonate (DEC), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (the mass ratio of the three is 3:5:2) to obtain an electrolyte.
[0064] 4. Battery preparation: The positive electrode sheet, polypropylene separator, and negative electrode sheet are wound together to form a roll core, in which the separator ensures that the positive electrode or negative electrode can be completely wrapped to prevent the two from directly contacting and causing a short circuit. The roll core is wrapped with aluminum-plastic film and the electrolyte is injected into it. Finally, after the formation, capacity separation and other processes and completely sealed, the battery product is obtained.
[0065] Positive and negative electrode sheets were prepared according to the raw materials with different material properties in Example 1 and Table 1 below, and different porosities and thicknesses were set to obtain Examples 2-21. The electrode gram capacity test and the full battery 2C charge / 2C discharge charge and discharge cycle test were carried out, and the test results were recorded in Table 2.
[0066] Table 1
[0067] D50 / μm (D90-D10) / D50 Lithium iron phosphate 1 1.08 1.83 Lithium Iron Phosphate 2 1.14 1.96 Lithium iron phosphate 3 1.59 2.64 Artificial graphite 1 12.31 1.36 Artificial graphite 2 10.88 1.25 Artificial graphite 3 14.97 1.68
[0068] The cycle test method is to prepare a soft-pack lithium-ion battery with a capacity of 10A for testing, and perform charge and discharge cycles at a current of 10A charging / 10A discharging in a voltage range of 2.5V-3.65V, and count the number of cycles experienced when the battery capacity retention rate is reduced to 80%.
[0069] Table 2
[0070]
[0071]
[0072] As can be seen from Table 2 above, by controlling the design of the positive and negative electrode plates and the addition amount of VC in the present invention, the lithium iron phosphate battery can obtain a higher cycle life and service life, and has the advantage of high energy density to meet the needs of growing fields such as energy storage, engineering vehicles, and commercial vehicles. Specifically, by comparing Examples 1-9, when the positive electrode active material is set as lithium iron phosphate 1 and the negative electrode active material is artificial graphite 1 / 2 / 3, the secondary battery set satisfies the following relational expressions: 0.25 < PDc * Tc < 0.42; 0.1 < PDa * Ta < 0.2; 0.75 < (CB - 1.1) / VC < 1.5, and the value of (CB - 1.1) / VC is 1. After cyclic voltammetry tests, the number of cycles is above 4321, and the highest number of cycles is in Example 4, up to 4566, with good cycling performance. By comparing Examples 10-12, it can be obtained from Examples 11 and 12 that when the value of (CB - 1.1) / VC does not satisfy the relational expression, it will affect the cycling performance of the secondary battery and reduce the number of cycles; moreover, it can be obtained from Example 10 that when the content of the film-forming additive vinylene carbonate is as low as 0.01 and the value of (CB - 1.1) / VC does not satisfy the relational expression, the cycling performance of the manufactured secondary battery is even worse, and the content of the film-forming additive vinylene carbonate is insufficient, resulting in an unstable SEI film, which is prone to cracking and lithium deposition after multiple cycles, thus affecting the cycle life. It can be obtained from Examples 13-15 that the secondary battery prepared with lithium iron phosphate 2 as the positive electrode and artificial graphite 2 as the negative electrode has better performance, and the average number of cycles is 6400, which has a certain advantage compared with using lithium iron phosphate 1 as the positive electrode. It can be obtained from Examples 17 and 18 that when the value of (CB - 1.1) / VC does not satisfy the relational expression and lithium iron phosphate 3 is used as the positive electrode and artificial graphite 3 is used as the negative electrode, the performance of the prepared secondary battery decreases; it can be obtained from Example 16 that when the excess ratio CB of the negative electrode capacity per unit area relative to the positive electrode capacity is not within the range of 1.12 to 1.2 and the value of (CB - 1.1) / VC does not satisfy the relational expression, the performance of the prepared secondary battery is even worse, and the cycle life decreases to 3614. It can be obtained from Examples 19-21 that when lithium iron phosphate 3 is used as the positive electrode and artificial graphite 3 is used as the negative electrode, the prepared secondary battery has better cycling performance, and the number of cycles is as high as 5387.
[0073] According to the disclosure and teachings of the above specification, those skilled in the art to which the present invention pertains can also make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the above specific embodiments, and any obvious improvements, substitutions, or variations made by those skilled in the art on the basis of the present invention fall within the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for convenience of description and do not constitute any limitation to the present invention.
Claims
1. A secondary battery, characterized in that: It includes a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet includes a positive electrode active material, the positive electrode active material is an olivine structure, and the positive electrode sheet and the negative electrode sheet satisfy the following relationship: 0.25 <PDc*Tc<0.42;0.1<PDa*Ta<0.2;0.8<(CB-1.1) / VC<1.2; Wherein, PDc is the compaction density of the positive electrode sheet; Wherein, PDa is the compaction density of the negative electrode; Wherein, Tc is the thickness of the positive electrode sheet; Wherein, Ta is the thickness of the negative electrode plate; Wherein, CB is the excess ratio of negative electrode capacity per unit area to positive electrode capacity; Wherein, VC is the content of vinylene carbonate, a film-forming additive for lithium battery electrolyte, in the electrolyte; The surface of the positive electrode active material is coated with a carbon coating layer. The chemical formula of the positive electrode active material is LiFexM1-xPO4, where M is one or a combination of Mg, Ni, V, and Mn, 0 < x < 1. The particle size distribution of the positive electrode active material satisfies the following relationship: 1.08μm < Dc50 < 1.59μm, 1 < (Dc90 - Dc10) / Dc50 < 8. The negative electrode sheet includes a negative electrode current collector and a negative electrode active coating provided on at least one surface of the negative electrode current collector. The negative electrode active coating includes a negative electrode active material, and the negative electrode active material is artificial graphite, and the particle size distribution satisfies the following relationship: 10.88μm < Da50 < 14.97μm, 0.5 < (Da90 - Da10) / Da50 < 3. The tap density PDc of the positive electrode sheet has a value range of 2.2 g / cm 3 < PDc < 2.4 g / cm 3 , the thickness Tc of the positive electrode sheet has a value range of 0.065 mm < Tc < 0.185 mm, and the tap density Pda of the negative electrode sheet has a value range of 0.45 g / cm 3 < Pda < 1.6 g / cm 3 , the thickness Ta of the negative electrode sheet has a value range of 0.065 mm < Ta < 0.185 mm, the value range of CB is 1.12 < CB < 1.2, and the value range of VC is 2% < VC < 8%.
2. The secondary battery according to claim 1, characterized in that: The positive electrode plate includes a positive electrode collector and a positive electrode active coating arranged on at least one surface of the positive electrode collector, the positive electrode active coating includes a positive electrode active material, a conductive agent, a binder and a dispersant, and the weight ratio of the positive electrode active material, the conductive agent, the binder and the dispersant is 80-99:1-20:1-5:1-5.
3. The secondary battery according to claim 1, characterized in that: The negative electrode active coating comprises a negative electrode active material, a conductive agent, a binder and a dispersant, wherein the weight ratio of the negative electrode active material, the conductive agent, the binder and the dispersant is 85-99:1-15:1-5:1-5.
4. The secondary battery according to claim 3, characterized in that: The negative electrode active material includes at least one of artificial graphite, natural graphite, silicon, silicon oxide, tin, and lithium titanate.
5. The secondary battery according to claim 1, characterized in that: The secondary battery further comprises a separator, an electrolyte and a shell, wherein the separator is used to separate the positive electrode sheet and the negative electrode sheet, and the shell is used to install and package the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte.
6. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 1 to 5.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
CN101017915A
Electrochemical device and electronic device
CN113097438A
Secondary battery, preparation method thereof and power utilization device
CN114914547A
Non-aqueous electrolyte secondary battery
CN1776954A