A polymer material containing a C2v symmetrical fused ring unit and its preparation method and application

By copolymerizing fused-ring small molecule receptors with C2v symmetric structure and copolymerized units, the electronic energy level and optical band gap of the polymer material are optimized, which solves the problem of lack of efficient receptor types in all-polymer solar cells and realizes high-efficiency photovoltaics. Improved conversion and stability promote the improvement of photovoltaic device performance.

CN115433345BActive Publication Date: 2024-10-15FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211070134.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-02
Publication Date
2024-10-15
Estimated Expiration
2042-09-02

AI Technical Summary

Technical Problem

The development of all-polymer solar cells is limited by the lack of high-efficiency polymer acceptor types. Early polymer acceptor materials have shortcomings such as narrow absorption bands, low extinction coefficients, and difficult morphology control, which limits the improvement of photovoltaic device performance.

Method used

A trapezoidal fused-ring small molecule receptor with a C2v symmetric structure is copolymerized with different copolymerization units, and the crystallinity, electronic energy level and optical band gap of the material are optimized by introducing different electronegative terminal functional groups to prepare a material with excellent carrier transport. performance of polymer receptor materials.

Benefits of technology

It achieves high photoelectric conversion efficiency of polymer solar cells, broadens the selection range of high-efficiency polymer receptors, improves the photostability, mechanical stability and thermal stability of the device, and promotes the formation of nanoscale phase separation morphology. , improves short-circuit current and fill factor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115433345B_ABST
    Figure CN115433345B_ABST
Patent Text Reader

Abstract

The present application discloses a type of polymer material containing C2v symmetrical fused ring units and its preparation method and application. The structural formula of the polymer material containing C2v symmetrical fused ring units is shown in Formula I. The C2v symmetrical fused ring small molecule receptor selected by the present invention has a rigid planar structure, and the soluble alkyl side chain connected thereto is coplanar with the conjugated skeleton and is distributed in a cis structure. Introducing it into the polymer main chain can promote the π-π stacking of the molecular chain, thereby improving the electronic transmission performance of the target material; the pyrrole ring at the center of the fused ring can increase the electron cloud density of the conjugated system, which is conducive to raising the lowest unoccupied molecular orbital energy level of the polymer receptor material and broadening its absorption spectrum. The solar cell device prepared based on this type of material is expected to simultaneously obtain high photovoltaic performance and excellent stability#imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a polymer material containing a C2v symmetrical fused ring unit and a preparation method and application thereof, belonging to the technical field of preparation and application of organic solar cells. Background Art

[0002] Organic solar cells are lead-free and have the characteristics of being light, flexible, translucent, colorful and adjustable, and can be printed on a large area. Therefore, they have attracted much attention in recent years. The photoactive layer composed of a blend of electron donor materials and electron acceptor materials is the core component of solar cells, responsible for key tasks such as "absorption of photons" and "generation of electrons". According to the size of the molecular weight, the electron acceptor materials in the active layer can be divided into polymer acceptor materials and small molecule acceptor materials. Compared with small molecule materials, polymer materials have obvious advantages in morphological stability and mechanical flexibility, so they have greater application potential in wearable electronic devices.

[0003] Benefiting from the development of non-fullerene small molecule acceptor materials, organic solar cells based on small molecule acceptors have developed rapidly, and the photoelectric conversion efficiency (PCE) of single-cell devices has been increased to more than 19% (Nat. Mater. 2022, 21, 656). In contrast, the development of all-polymer solar cells is relatively backward, mainly due to the lack of efficient polymer acceptor types. Early polymer acceptors were mainly donor-acceptor (DA) alternating copolymers constructed with electron-deficient units such as perylene diimide, naphthalene diimide, and double boron nitrogen bond bridged pyridine, but this type of polymer acceptor generally has the disadvantages of narrow absorption band, low extinction coefficient, and difficult morphology control, which in turn limits the improvement of the performance of the corresponding photovoltaic devices. In recent years, a class of polymer acceptor materials developed based on the "small molecule acceptor polymerization strategy" has made a major breakthrough in the device performance of all-polymer solar cells (Angew. Chem. Int. Ed., 2017, 56, 13503). Non-fullerene small molecule receptors can maintain the outstanding advantages of small molecule receptors such as wide and strong absorption and suitable electronic energy levels, while also bringing advantages such as high morphological stability and thermal stability of polymers and strong mechanical stretchability, which has become an important research direction at present. The key to developing polymers based on condensed ring small molecule receptors is to develop efficient non-fullerene small molecule receptors. However, there are very few types of commonly used condensed ring small molecule receptors, and most of them are still limited to ITIC receptors and Y series receptors (Angew. Chem. Int. Ed. 2021, 60, 4422), which to a certain extent limits the development of all-polymer solar cells. Summary of the invention

[0004] This application uses a new type of ladder-shaped fused ring small molecule receptor with a C2v symmetric structure as a building unit, and obtains a series of polymer receptor materials by copolymerizing with different copolymerization units. At the same time, the crystallinity, electronic energy level and optical band gap of the material are fully optimized by introducing terminal functional groups with different electronegativity into the receptor molecules. This type of material will have excellent carrier transport performance, a narrow band gap and an electronic energy level that matches the polymer donor, and the corresponding photovoltaic device can show a higher photoelectric conversion efficiency. In addition, this type of polymer receptor is soluble in most common organic solvents, such as chlorobenzene, chloroform, toluene, etc., and has excellent solution processing performance.

[0005] According to the first aspect of the present application, a polymer material containing a C2v symmetric fused ring unit is provided, wherein the polymer material containing a C2v symmetric fused ring unit has a structure as described in Formula I:

[0006]

[0007] Wherein, R1 is selected from C1~C 30 Alkyl I, C1~C 30 The halogenated alkyl I, C4~C 20 Aryl I, C4~C 20 The substituted aryl group I has one of the groups shown in formula I-1;

[0008] Wherein, the substituent of the substituted aryl group I is selected from one of alkyl, haloalkyl, alkoxy, haloalkoxy, halogen, alkylthio, and haloalkylthio;

[0009] R'—M—* Formula I-1;

[0010] Wherein, R' is selected from C1~C 30 Alkyl II, C1~C 30 One of the haloalkyl II;

[0011] M is selected from O or S;

[0012] R2 is selected from C1~C 30 Alkyl I, C1~C 30 The halogenated alkyl I, C4~C 20 Aryl I, C4~C 20 Substituted aryl I;

[0013] Wherein, the substituent of the substituted aryl group I is selected from one of alkyl, haloalkyl, alkoxy, haloalkoxy, halogen, alkylthio, and haloalkylthio;

[0014] X1, X2 are independently selected from O, S or Se;

[0015] Ar1, Ar2 are independently selected from C4~C 20 Aryl II, which contains at least one thiophene ring and forms a condensed ring with the pyrrole ring in formula I;

[0016] EG is selected from one of the groups having the structure shown in Formula II; wherein the dotted line in Formula II is the double bond connection position;

[0017]

[0018] Wherein, Ar' is selected from C4~C 40 Aryl II, C4~C 40 Substituted aromatic II, C4~C 40 Heteroaryl, C4~C 40 substituted heteroaryl;

[0019] The substituents of the substituted aryl II and the substituted heteroaryl are independently selected from any one of halogen, cyano, haloalkyl, alkyl, alkoxy, alkylthio, ester and carbonyl;

[0020] Donor is selected from thiophene, One of the groups of the structure shown;

[0021] n is the number of repeating structural units, and the value range of n is 10 to 1000.

[0022] Optionally, R1 is selected from C3 to C 30 Branched alkoxy containing C3~C 30 Branched fluorinated alkoxy, C3~C 30 Branched alkylthio, C3~C 30 Branched fluorinated alkylthio, C3~C 30 Branched alkyl, C3~C 30 Branched fluorinated alkyl, C1~C 28 Straight chain alkoxy, C1~C 28 Straight chain fluorinated alkoxy, C1~C 28 Straight chain alkylthio, C1~C 28 Straight chain fluorinated alkylthio, C1~C 28 Straight chain alkyl, C1~C 28 Straight chain fluorinated alkyl, C4~C 20 Alkyl aromatic group, C4~C 20 Fluorinated alkyl aromatic groups, C4~C 20 Alkoxy aromatic group, C4~C 20 Fluorinated alkoxy aromatic groups, C4~C 20 Alkylthio aromatic group, C4~C 20 Fluorinated alkylthio aromatic groups, C4~C 20 Aromatic groups, C4~C20 Any one of the fluorinated aromatic groups.

[0023] Optionally, R1 is selected from C3 to C 20 The branched alkoxy containing C3~C 20 Branched fluorinated alkoxy, C3~C 20 Branched alkylthio, C3~C 30 Branched fluorinated alkylthio, C3~C 20 Branched alkyl, C3~C 20 Branched fluorinated alkyl, C1~C 20 Straight chain alkoxy, C1~C 20 Straight chain fluorinated alkoxy, C1~C 20 Straight chain alkylthio, C1~C 20 Straight chain fluorinated alkylthio, C1~C 20 Straight chain alkyl, C1~C 20 Straight chain fluorinated alkyl, C4~C 20 Alkyl aromatic group, C4~C 20 Fluorinated alkyl aromatic groups, C4~C 20 Alkoxy aromatic group, C4~C 20 Fluorinated alkoxy aromatic groups, C4~C 20 Alkylthio aromatic group, C4~C 20 Fluorinated alkylthio aromatic groups, C4~C 20 Aromatic groups, C4~C 20 Any one of the fluorinated aromatic groups.

[0024] Further optionally, R1 is selected from C3~C 12 The branched alkoxy containing C3~C 12 Branched fluorinated alkoxy, C3~C 12 Branched alkylthio, C3~C 12 Branched fluorinated alkylthio, C3~C 12 Branched alkyl, C3~C 12 Branched fluorinated alkyl, C1~C 12 Straight chain alkoxy, C1~C 12 Straight chain fluorinated alkoxy, C1~C 12 Straight chain alkylthio, C1~C 12 Straight chain fluorinated alkylthio, C1~C 12 Straight chain alkyl, C1~C 12 Straight chain fluorinated alkyl, C4~C 12 Alkyl aromatic group, C4~C 12 Fluorinated alkyl aromatic groups, C4~C 12 Alkoxy aromatic group, C4~C 12Fluorinated alkoxy aromatic groups, C4~C 12 Alkylthio aromatic group, C4~C 12 Fluorinated alkylthio aromatic groups, C4~C 12 Aromatic groups, C4~C 12 Any one of the fluorinated aromatic groups.

[0025] Optionally, R2 is selected from C3~C 30 Branched alkyl, C3~C 30 Branched fluorinated alkyl, C1~C 28 Straight chain alkyl, C1~C 28 Straight chain fluorinated alkyl, C4~C 20 Alkyl aromatic group, C4~C 20 Fluorinated alkyl aromatic groups, C4~C 20 Aromatic groups, C4~C 20 Any one of the fluorinated aromatic groups.

[0026] Optionally, R2 is selected from C3~C 20 Branched alkyl, C3~C 20 Branched fluorinated alkyl, C1~C 20 Straight chain alkyl, C1~C 20 Straight chain fluorinated alkyl, C4~C 20 Alkyl aromatic group, C4~C 20 Fluorinated alkyl aromatic groups, C4~C 20 Aromatic groups, C4~C 20 Any one of the fluorinated aromatic groups.

[0027] Further optionally, R2 is selected from C3 to C 12 Branched alkyl, C3~C 12 Branched fluorinated alkyl, C1~C 12 Straight chain alkyl, C1~C 12 Straight chain fluorinated alkyl, C4~C 12 Alkyl aromatic group, C4~C 12 Fluorinated alkyl aromatic groups, C4~C 12 Aromatic groups, C4~C 12 Any one of the fluorinated aromatic groups.

[0028] Optionally, Ar' is selected from C4 to C 10 Substituted aromatic II, C4~C 10 substituted heteroaryl.

[0029] Optionally, the heteroaryl is a monocyclic heteroaryl.

[0030] Optionally, the heteroaryl group contains 5 skeleton ring atoms, wherein at least one ring atom is a heteroatom, and the heteroatom is selected from a sulfur atom.

[0031] Optionally, n represents the number of repeating units of the polymer material containing the C2v symmetrical fused ring unit, which is any natural number between 10 and 1000.

[0032] Optionally, the EG is selected from any one of Formula II-1, Formula II-2, Formula II-3, Formula II-4, Formula II-5, and Formula II-6.

[0033]

[0034] Optionally, the R 21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 , R 28 independently selected from hydrogen, halogen, cyano, C1-C 30 Alkyl, C1~C 30 Alkoxy, C1~C 30 Alkylthio, C1~C 30 Any one of an ester group and a carbonyl group.

[0035] Optionally, the R 21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 , R 28 Any one independently selected from hydrogen, halogen, cyano, haloalkyl, alkyl, alkoxy, alkylthio, ester and carbonyl; wherein the alkyl contained in the alkyl, alkoxy, alkylthio and ester groups are straight-chain or branched alkyl groups with 1 to 30 carbon atoms.

[0036] Optionally, the R 21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 , R 28 Independently selected from a straight chain or branched chain with 1 to 3 carbon atoms; the dotted double bond is the double bond connection position with the nitrogen-containing ladder heterocycle, and the dotted single bond is the single bond connection position with the electron-donating unit.

[0037] Optionally, the halogen is fluorine.

[0038] Optionally, the Donor is selected from any one of the groups having the structures shown in Formula III-1, Formula III-2, Formula III-3, Formula III-4, Formula III-5, Formula III-6, and Formula III-7.

[0039]

[0040] Optionally, X3 is selected from O, S or Se.

[0041] Optionally, the R 31 , R 32 , R 33 , R 34 , R 35 , R 36 independently selected from halogen, C1-C 30 Alkyl, C1~C 30 Alkoxy, C1~C 30 Any one of an alkylthio group and an ester group;

[0042] Optionally, the R 37 , R 38 Independently selected from C1 to C 30 One of the alkyl groups.

[0043] Optionally, R 37 , R 38 They are independently selected from linear or branched alkyl groups having 5 to 25 carbon atoms.

[0044] According to the second aspect of the present application, a method for preparing the above-mentioned polymer material containing a C2v symmetrical fused ring unit is provided, comprising:

[0045] In an inactive atmosphere, a mixture containing a compound represented by formula IV, a compound represented by formula V, and a catalyst undergoes a Stille coupling reaction to obtain a polymer material containing a C2v symmetrical fused ring unit having a structure represented by formula I;

[0046]

[0047] Optionally, Ar1, Ar2, EG, D2 contained in Formula IV and Formula V correspond to Ar1, Ar2, EG, D2 in the structure shown in Formula I.

[0048] Optionally, the catalyst is tetrakis(triphenylphosphine)palladium(0).

[0049] Optionally, the molar ratio of the compound represented by formula IV: the compound represented by formula V: tetrakis(triphenylphosphine)palladium(0) is 1:1:(0.01-0.5).

[0050] Optionally, the mixture contains a solvent, and the solvent is toluene.

[0051] Optionally, the inert atmosphere is selected from a nitrogen atmosphere and / or an argon atmosphere.

[0052] Optionally, after the Stille coupling reaction is completed, the reaction solution is poured into methanol for precipitation, filtered to obtain a residue, and the residue is extracted with methanol, acetone, n-hexane and chloroform in this order using a Soxhlet extractor, and finally the filtrate obtained by chloroform extraction is distilled under reduced pressure to obtain the product.

[0053] Optionally, the conditions of the Stille coupling reaction are: reaction temperature of 80 to 150° C., and reaction time of 24 to 96 hours.

[0054] Optionally, the reaction temperature is selected from any value of 80°C, 100°C, 110°C, 120°C, 130°C, 150°C or a range between any two of the above points.

[0055] Optionally, the reaction time is selected from any value of 24 hours, 48 ​​hours, 55 hours, 65 hours, 72 hours, 96 hours, or a range between any two of the above points.

[0056] Optionally, the conditions of the Stille coupling reaction are: reaction temperature of 100 to 130° C., and reaction time of 40 to 70 hours.

[0057] According to the third aspect of the present application, a semiconductor material is provided, which comprises at least one of the polymer materials containing C2v symmetric fused ring units described in any of the above items or the polymer materials containing C2v symmetric fused ring units prepared by any of the preparation methods described in the above items.

[0058] According to a fourth aspect of the present application, a photoactive layer is provided, wherein the photoactive layer contains the organic semiconductor material described above.

[0059] According to a fifth aspect of the present application, a polymer solar cell device is provided, wherein the polymer solar cell device comprises the organic semiconductor material described above or comprises the photoactive layer described above;

[0060] Optionally, the polymer solar cell device includes a substrate, a cathode, a cathode modification layer, a photoactive layer, an anode modification layer and an anode, the photoactive layer contains an electron donor material and a polymer material containing a C2v symmetrical fused ring unit, and the mass ratio of the electron donor material to the polymer material containing a C2v symmetrical fused ring unit is (0.5 to 2.5):1.

[0061] Optionally, the mass ratio of the electron donor material to the polymer material containing a C2v symmetrical fused ring unit is selected from any value of 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 2:1, 2.5:1 or a range between any two of the above points.

[0062] Optionally, the mass ratio of the electron donor material to the polymer material containing a C2v symmetrical fused ring unit is 1:1.

[0063] Optionally, the electron donor material is a p-type semiconductor material.

[0064] Optionally, the electron donor material is selected from at least one of J71, PTQ10, PBDB T, and PM6.

[0065] Optionally, the method for preparing the all-polymer solar cell device comprises the following steps: dissolving an electron donor material and a polymer material containing a C2v symmetrical fused ring unit in a solvent, mixing them evenly, and then spin coating or scraping them on a transparent conductive electrode containing an interface layer to prepare a thin film photoactive layer, then coating an electron transport layer on the photoactive layer, and finally evaporating a metal electrode on the electron transport layer to obtain an all-polymer solar cell device.

[0066] Optionally, the substrate is a glass substrate, the anode is indium tin oxide (ITO); the anode modification layer is poly (3,4-ethylenedioxythiophene: polystyrene sulfonate) (PEDOT:PSS); the cathode modification layer is 2,9-bis(3-(dimethylamino)propyl)anthracene (2,1,9-def:6,5,10-d'e'f')diisoquinoline-1,3,8,10(2H,9H)-tetraketone (PDIN); and the cathode is aluminum (Al).

[0067] Optionally, the polymer material containing the C2v symmetrical fused ring unit is blended with an electron donor material to prepare a photoactive layer, wherein the electron donor material is at least one of PBDB-T and PM6.

[0068] Optionally, the mass ratio of the electron donor material to the polymer material containing the C2v symmetrical fused ring unit in the photoactive layer is (0.5-2.5):1.

[0069] Optionally, the solvent used in the photoactive layer is at least one of toluene, xylene, trimethylol, chloroform, chlorobenzene, dichlorobenzene, trichlorobenzene and tetrahydrofuran, the concentration of the electron donor material in the photoactive layer is 1 mg / mL to 20 mg / mL, preferably 5 mg / mL to 10 mg / mL, and the concentration of the polymer material containing C2v symmetrical fused ring units is 1.5 mg / mL to 9.5 mg / mL, preferably 5 mg / mL to 8 mg / mL.

[0070] Optionally, the photoactive layer is subjected to annealing treatment at a temperature of 50 to 150° C., preferably 60 to 90° C., and an annealing time of 1 to 30 minutes, preferably 5 to 10 minutes.

[0071] Optionally, the upper limit of the annealing temperature of the photoactive layer can be independently selected from 150°C, 140°C, 130°C, 120°C, 110°C, 100°C, 90°C, and the lower limit can be independently selected from 50°C, 60°C, 70°C, 80°C, 90°C, 100°C.

[0072] Optionally, the annealing time is selected from any value of 1 minute, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, or a range between any two of the above points.

[0073] In this application, all conditions involving numerical ranges can be independently selected at any point within the selected range, including the end points of the range.

[0074] In this application, C1~C 30 、C4~C 20 、C4~C 40 、C4~C 10 The numbers of carbon atoms in a group are all referred to, such as C1~C 30 The alkyl group refers to an alkyl group having 1 to 30 carbon atoms.

[0075] In the present application, a branched chain having 1 to 30 carbon atoms means that there is at least one or more branched chains in the alkyl group, and the position of the branching can be anywhere from the 1st to the 29th carbon atom;

[0076] In the present application, an alkyl group refers to a group formed by losing any hydrogen atom of an alkane compound, and the alkane compound includes straight-chain alkanes, branched-chain alkanes, and cycloalkanes;

[0077] In the present application, an aryl group refers to a group formed by losing any hydrogen atom on an aromatic ring in an aromatic compound molecule; the aromatic compound includes a compound containing an aromatic ring and a compound in which at least one hydrogen atom on the aromatic ring is replaced by an alkyl group. Aromatic group, as a type of aromatic group, refers to an optionally substituted aromatic hydrocarbon group having 6 to about 20, such as 6 to 20 or 6 to 10 ring-forming carbon atoms, which can be a monocyclic aromatic group, a bicyclic aromatic group or a multicyclic aromatic group. Bicyclic aromatic groups or multicyclic aromatic groups can be a monocyclic aromatic group or other independent rings, such as alicyclic, heterocyclic, aromatic, or aromatic heterocyclic fused groups. Non-limiting examples of monocyclic aromatic groups include monocyclic aromatic groups having 6 to about 12, 6 to about 10, or 6 to about 8 ring-forming carbon atoms, such as phenyl; bicyclic aromatic groups are, for example, naphthyl; polycyclic aromatic groups are, for example, phenanthrenyl and anthracenyl.

[0078] In the present application, the term "heteroaryl" used herein alone or in combination refers to an arbitrarily substituted heteroaryl group, which contains about 4 to about 20, such as 4 to 12 or 4 to 10 skeleton ring atoms, wherein at least one (such as 1-4, 1-3, 1-2) ring atom is a heteroatom, and the heteroatom is sulfur, but is not limited thereto. The ring of the group does not contain two adjacent O or S atoms. Heteroaryl includes monocyclic heteroaryl (having one ring), bicyclic heteroaryl (having two rings) or polycyclic heteroaryl (having more than two rings). In embodiments where two or more heteroatoms appear in the ring, the two or more heteroatoms may be the same as each other, or some or all of the two or more heteroatoms may be different from each other. Bicyclic heteroaryl or more cyclic heteroaryl may be a monocyclic heteroaryl fused with other independent rings, such as aromatic rings and aromatic heterocycles (collectively referred to as fused ring heteroaryl). Non-limiting examples of monocyclic heteroaryl groups include monocyclic heteroaryl groups of 5 to about 12, 5 to about 10, 5 to about 7 or 6 backbone ring atoms, for example, non-limiting examples thereof include thienyl; fused ring heteroaryl groups include bicyclic thiophene.

[0079] In the present application, a haloalkyl group refers to a group formed by replacing at least one hydrogen atom on an alkyl group with a halogen atom.

[0080] In the present application, a halogenated aromatic group refers to a group in which at least one hydrogen atom on an aromatic group is replaced by a halogen atom.

[0081] In the present application, an alkyl aromatic group refers to a group in which at least one hydrogen atom on an aromatic group is replaced by an alkyl group.

[0082] In the present application, a halogenated alkyl aromatic group refers to an alkyl aromatic group in which at least one hydrogen atom is substituted by a halogen atom.

[0083] In the present application, an alkoxy group is a group formed by losing a hydrogen atom from a hydroxyl group in an alkyl alcohol molecule.

[0084] In the present application, a haloalkoxy group is a group in which at least one hydrogen atom in an alkoxy group is replaced by a halogen atom.

[0085] In the present application, an alkylthio group is a group formed after losing a hydrogen atom on a mercapto group in an alkylthiol molecule.

[0086] In the present application, a haloalkylthio group is an alkylthio group in which at least one hydrogen atom is substituted by a halogen atom.

[0087] In the present application, an alkoxy aromatic group refers to a group in which at least one hydrogen atom on an aromatic group is substituted by an alkoxy group.

[0088] In the present application, the halogenated alkoxy aromatic group refers to an alkoxy aromatic group in which at least one hydrogen atom on the alkoxy group is substituted by a halogen atom.

[0089] In the present application, an alkylthioaromatic group refers to a group in which at least one hydrogen atom on an aromatic group is substituted by an alkylthio group.

[0090] In the present application, the haloalkylthioaromatic group refers to an alkylthioaromatic group in which at least one hydrogen atom on the alkylthio group is substituted by a halogenated atom.

[0091] In the present application, the ester group refers to the ester functional group in the carboxylic acid derivative, with the structural formula -COOR, wherein R is an alkyl group or other non-H group.

[0092] The beneficial effects of this application include:

[0093] 1) The polymer material containing C2v symmetrical fused ring units provided by the present invention adopts a fused ring small molecule receptor with a C2v symmetrical structure as a building unit, and is obtained by copolymerization with different electron-rich units. This type of polymer is an n-type organic semiconductor and can be used as an electron transport material in the preparation of polymer solar cell devices. This type of polymer has a wide range of spectral absorption, suitable electronic energy levels, small exciton binding energy, high carrier transport performance, and moderate molecular aggregation characteristics. The active layer prepared by blending it with an electron donor material can show a phase separation morphology of a nanofiber structure, and has excellent photostability, mechanical stability, and thermal stability. This type of material will broaden the selectable range of high-efficiency polymer receptors, which will help promote the commercial application of organic solar cells.

[0094] 2) The fused ring unit selected in the present invention has a rigid and planar molecular structure, and its introduction into the polymer main chain is conducive to the formation of a more compact and orderly π-π stacking of the polymer main chain, thereby promoting the high efficiency of carriers.

[0095] 3) The conjugated skeleton of the fused ring electron acceptor selected in the present invention introduces a pyrrole heterocycle with electron-rich properties, which can increase the electron cloud density of the fused ring conjugated skeleton, enhance the intramolecular charge transfer, and thus broaden the absorption spectrum of the target acceptor while maintaining a high minimum unoccupied orbital energy level.

[0096] 4) The polymer of the present invention utilizes the unique steric hindrance effect of the adjacent side chains on the skeleton to regulate its molecular aggregation behavior. The photoactive layer prepared based on this type of polymer can form an ideal morphology of nanoscale phase separation scale, and the corresponding battery device can exhibit high short-circuit current and filling factor.

[0097] 5) The polymer material containing C2v symmetrical fused ring units provided by the present invention has the advantages of simple synthesis, mild conditions, low cost, etc., and is conducive to large-scale production.

[0098] 6) The present invention uses a condensed ring small molecule receptor with C2v symmetry as a building block, and obtains a series of polymer electron receptor materials by polymerization with different copolymerization units. The selected C2v symmetric condensed ring small molecule receptor has a rigid planar structure, and the soluble alkyl side chain connected thereto is coplanar with the conjugated skeleton and is distributed in a cis structure. Introducing it into the polymer main chain can promote the π-π stacking of the molecular chain, thereby improving the electron transport performance of the target material; the pyrrole ring at the center of the condensed ring can increase the electron cloud density of the conjugated system, which is conducive to raising the lowest unoccupied molecular orbital energy level of the polymer receptor material and broadening its absorption spectrum. The solar cell device prepared based on this type of material is expected to simultaneously obtain high photovoltaic performance and excellent stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0099] Figure 1 The monomer M17-1 involved in Examples 1 and 2 of the present invention 1 H NMR spectrum.

[0100] Figure 2 The monomer M17-2 involved in Examples 3 and 4 of the present invention 1 H NMR spectrum.

[0101] Figure 3 The monomer M17-3 involved in Example 5 of the present invention 1 H NMR spectrum.

[0102] Figure 4 Absorption spectra of the polymer receptors PW-S, PW-Se, PW2, PW5 and PW7 prepared in Examples 1, 2, 3, 4 and 5 of the present invention in chloroform solution.

[0103] Figure 5 Absorption spectra of the polymer receptors PW-S, PW-Se, PW2, PW5 and PW7 prepared in Examples 1, 2, 3, 4 and 5 of the present invention in the thin film state.

[0104] Figure 6 Cyclic voltammetry curves of the polymer receptors PW-S, PW-Se, PW2, PW5 and PW7 prepared in Examples 1, 2, 3, 4 and 5 of the present invention.

[0105] Figure 7 This is a current-voltage (JV) curve of the all-polymer solar cell prepared by blending the polymer acceptors PW-S, PW-Se, PW2, PW5, PW7 prepared in Examples 1, 2, 3, 4 and 5 of the present invention with the donor PM6.

[0106] Figure 8This is a graph showing the external quantum efficiency of a solar cell prepared by blending the polymers PW-S and PW-Se prepared in Examples 1 and 2 of the present invention with the electron donor PM6.

[0107] Fig. 9 This is a graph showing the external quantum efficiency of solar cells prepared by blending PW2, PW5 and PW7 prepared in Examples 3-5 of the present invention with the electron donor PM6.

[0108] Fig.10 JV curves of single-electron devices prepared by blending the polymers PW-S, PW-Se, PW2, PW5, and PW7 prepared in Examples 1-5 of the present invention with the respective donor PM6 in the dark state.

[0109] Fig.11 JV curves of single-hole devices prepared by blending the polymers PW-S, PW-Se, PW2, PW5, and PW7 prepared in Examples 1-5 of the present invention with the respective donor PM6 in the dark state.

[0110] Fig.12 The current density (J) of the solar cell prepared by blending the polymers PW-S and PW-Se obtained in Examples 1 and 2 of the present invention with the electron donor PM6 ph ) with effective voltage (V eff )’s change curve diagram.

[0111] Fig.13 The photocurrent density (J) of the solar cell prepared by blending the polymers PW2, PW5 and PW7 obtained in Examples 3-5 of the present invention with the electron donor PM6 ph ) with effective voltage (V eff )’s change curve diagram.

[0112] Fig.14 This is a curve diagram of the short-circuit current of a solar cell prepared by blending the polymers PW-S, PW-Se, PW2, PW5, PW7 prepared in Examples 1-5 of the present invention with the electron donor PM6 as a function of light intensity.

[0113] Fig.15 Grazing incidence wide angle X-ray diffraction (GIWAXS) patterns of the films of polymers PW2 and PW5 prepared in Examples 3 and 5 of the present invention.

[0114] Fig.16 Grazing incidence wide angle X-ray diffraction (GIWAXS) patterns of mixed films prepared by blending polymers PW2 and PW5 obtained in Examples 3 and 5 of the present invention with electron donor PM6. DETAILED DESCRIPTION

[0115] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0116] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0117] In the examples of the present application, the prepared polymer material containing a C2v symmetrical fused ring unit was characterized using the following instruments:

[0118] The obtained materials were tested by AVANCE III NMR spectrometer. 1 H NMR spectrum;

[0119] Lambda35 UV-visible spectrophotometer was used to test the UV-visible absorption spectra of the obtained materials in solution and film states;

[0120] The cyclic voltammetry curve of the obtained material in the thin film state was tested using Chenhua 604E electrochemical workstation;

[0121] The electron mobility and hole mobility of the single carrier device were tested using a semiconductor analyzer (Agilent 4155C) and the space charge limitation method. The polymer acceptor materials PW-S, PW-Se, PW2, PW5 and PW7 were blended with the electron donor material PM6 to prepare the single carrier device. The mass ratio of the electron donor material to the polymer acceptor material in the mixed film was 1:1. The thin film preparation method was the same as the method used in Example 6.

[0122] Grazing-incidence wide-angle X-ray diffraction (GIWAXS) measurements were obtained on the XEUSSSAXS / WAXS system at the National Center for Nanoscience and Technology. All test samples were prepared on silicon (Si) substrates with PEDOT:PSS coatings. The wavelength of the X-ray beam was The incident angle was set to 0.2°. The scattered X-rays were detected using a Dectris Pilatus 300K photon counting detector.

[0123] The method for preparing a polymer material containing a C2v symmetrical fused ring unit provided by the present invention comprises the following steps:

[0124]

[0125] In an inert atmosphere, M-Br and the electron-donating copolymer unit Donor-Sn undergo Stille coupling reaction under the catalysis of Pd(PPh3)4 to obtain a polymer material containing a C2v symmetrical fused ring unit as shown in formula I.

[0126] Example 1

[0127] The fused ring unit shown in formula I is BTP-C8C10, and the EG unit is When the electron donating unit is thiophene, the preparation method of the corresponding polymer material PW-S is as follows:

[0128] (1) Compound 1 is subjected to chlorination under DMF catalysis to obtain compound 2;

[0129]

[0130] Synthesis of compound 2: Compound a (10 g, 44 mmol) was dispersed in chloroform (100 mL), cooled to 0°C and stirred, oxalyl chloride (10.6 g, 84 mmol) was added dropwise, and then a catalytic amount of DMF was injected. After returning to room temperature, the reaction was continued for 8 h. After the reaction was completed, the organic phase was concentrated using a rotary evaporator to obtain the product as a yellow solid (10.5 g, 98%). It was directly used in the next step without further purification.

[0131] (2) Compound 2 is subjected to a Friedel-Crafts acylation reaction catalyzed by aluminum chloride to obtain compound 3;

[0132]

[0133] Synthesis of compound 3: Compound 2 (10.5 g, 44.2 mmol) and aluminum chloride (28.0 g, 0.21 mol) were dissolved in nitrobenzene (50 mL), nitrogen was introduced to remove dissolved oxygen in the system, and then malonyl chloride (11.59 g, 82.2 mmol) was added dropwise to the system, and heated at 100°C for 12 h. After the reaction was completed, the reaction was quenched with 1 mol / L hydrochloric acid, extracted with dichloromethane, and the organic phase was washed with deionized water for several times, the organic phases were combined and dried with anhydrous magnesium sulfate, and the organic phase was concentrated with a rotary evaporator, and the product was purified by column chromatography (the eluent was pure dichloromethane). After removing the solvent, the product was a yellow solid powder (5.0 g, 47%). 1 H NMR (400 MHz, CDCl 3, δ):7.64-7.55(m,1H),4.21(d,J=4.8Hz,2H).

[0134] (3) Compound 3 was subjected to Knoevenagel reaction to give IC-FBr.

[0135]

[0136] Synthesis of IC-FBr: Under nitrogen conditions, a mixture of compound 3 (11.90 g, 0.05 mol) and sodium acetate (8.23 g, 0.1 mol) was placed in a 100 mL two-necked bottle, 30 mL of ethanol solution was added, nitrogen was passed for 15 minutes, malononitrile (19.80 g, 0.3 mol) was added, nitrogen was passed for 15 minutes, and then heated to 60 ° C and reacted for 5 hours. Then it was returned to room temperature, 30 mL of dilute hydrochloric acid (1M) was added and stirred for 3 hours, the residue was filtered and purified by rapid silica gel column chromatography (dichloromethane) to obtain a dark green solid compound IC-FBr. It is worth noting that IC-FBr is a mixture with isomers. 1 H NMR (400MHz, CDCl3) δ8.89(d,J=5.6Hz,1H),8.34(d,J=7.9Hz,1.6H),8.22(d,J=6.3Hz,1.6H),7.07(d,J=6.4Hz,1H),3.78(s,2H).

[0137] (4) BTP-C8C10 and IC-FBr were reacted by Knoevenagel reaction to obtain monomer M17-1. The synthesis of BTP-C8C10 was based on our previous research (Chemical Engineering Journal 2021, 418, 129497) and patent (CN202111208166.9).

[0138]

[0139] Synthesis of M17-1: Under nitrogen conditions, the compound BDTPT-C8C10 (1.79 g, 0.001 mol) was placed in a 50 mL two-necked flask, 20 mL of chloroform solvent was added, and after passing nitrogen for 15 minutes, IC-FBr end group (1.45 g, 0.005 mol) was added. After passing nitrogen for 15 minutes, pyridine solution (0.1 mL) was added as an acid binding agent, and the mixture was heated to 50°C and reacted for 5 hours. After purification by rapid silica gel column chromatography (the polarity of the eluent was dichloromethane: petroleum ether = 1:1), the mixture was precipitated in methanol and filtered to obtain a black purple solid compound M17-1 (yield 90%). Figure 1 This is the NMR spectrum of M17-1: 1H NMR (400MHz, CDCl3) δ8.87(m,2H),8.39(d,J=8.4Hz,1.4H),8.05(d,J=6.4Hz,1.4H),7.89(s,2.4H),7.56(d, J=6.16Hz,0.8H),4.78(s,4H),4.23(d,J=7.12Hz,4H),2.00(s,4H),1.50-1.10(m,128H),0.86-0.71(m,24H).

[0140] (5) The monomer M17-1 and the ditinthiophene reagent are reacted by Stille reaction to obtain the final polymer PW-S;

[0141]

[0142] Synthesis of polymer PW-S: Under nitrogen conditions, M17-1 (213 mg, 0.1 mmol) and 2,5-di(trimethyltin)thiophene (40.9 mg, 0.1 mmol) were placed in a 25 mL two-necked flask, 10 mL of toluene solvent was added, nitrogen was passed for 15 minutes, and the catalyst tetrakis(triphenylphosphine)palladium (5.8 mg, 0.005 mmol) was added. After passing nitrogen for 15 minutes, it was heated to 100°C and reacted for 96 hours. The reaction solution was precipitated and filtered in methanol to obtain a black solid, and then washed with methanol solution, acetone solution, n-hexane solution, and chloroform solution by Soxhlet extraction for 12 hours each. Finally, the product obtained by washing with chloroform solution was collected, precipitated in methanol and filtered to obtain a black solid polymer PW-S with a yield of 55% (GPC: M n =26.8 kDa, M w =54.5 kDa, PDI =2.02).

[0143] Example 2

[0144] The fused ring unit shown in formula I is BTP-C8C10, and the EG unit is IC-FBr When the electron donating unit is selenophene, the preparation method of the corresponding polymer acceptor material PW-Se is as follows:

[0145] (1) The monomer M17-1 and the ditin selenophene reagent are reacted by Stille reaction to obtain the final polymer PW-Se;

[0146]

[0147] M17-1 (0.1 g, 0.046 mmol), 2,5-bis(trimethyltin)selenophene (0.021 g, 0.046 mmol) and Pd(PPh3)4 (0.0014 g, 0.0012 mmol) were accurately weighed into a 10 mL pressure bottle, and 2 mL of ultra-dry toluene was added under a nitrogen atmosphere. The mixture was heated to 130 °C for reaction. Heating was stopped after 72 h, and after the system was cooled to 25 °C, the reaction product was poured into methanol, the precipitate was collected, and the Soxhlet extraction method was used to extract with methanol, acetone, n-hexane and chloroform, respectively, the chloroform component was collected, the solution was concentrated and dripped into a large amount of methanol solution with a glass dropper to precipitate, the precipitate was collected, and the target polymer was obtained after drying as black solid particles with a yield of 54%, (GPC: M n =7.4 kDa, M w =15.1 kDa, PDI =2.04).

[0148] Example 3

[0149] The C2v symmetrical fused ring unit shown in formula I is BTP-C8C10, and the EG unit is IC-2FBr When the electron-donating unit is thiophene, the preparation method of the polymer material PW2 containing the C2v symmetrical fused ring unit is as follows:

[0150] (1) Compound a is subjected to chlorination reaction under DMF catalysis to obtain compound b;

[0151]

[0152] Synthesis of compound b: Compound a (10 g, 42 mmol) was dispersed in chloroform (100 mL), cooled to 0°C and stirred, oxalyl chloride (10.6 g, 84 mmol) was added dropwise, and then a catalytic amount of DMF was injected. After returning to room temperature, the reaction was continued for 8 h. After the reaction was completed, the organic phase was concentrated using a rotary evaporator to obtain the product as a yellow solid (10.5 g, 98%). It was directly used in the next step without further purification.

[0153] (2) Compound b undergoes Friedel-Crafts acylation reaction under the catalysis of aluminum chloride to obtain compound c;

[0154]

[0155] Synthesis of compound c: Compound b (10.5 g, 41.1 mmol) and aluminum chloride (28.0 g, 0.21 mol) were dissolved in nitrobenzene (50 mL), nitrogen was introduced to remove dissolved oxygen in the system, and then malonyl chloride (11.59 g, 82.2 mmol) was added dropwise to the system, and heated at 100°C for 12 h. After the reaction was completed, the reaction was quenched with 1 mol / L hydrochloric acid, extracted with dichloromethane, and the organic phase was washed with deionized water for several times, combined and dried with anhydrous magnesium sulfate, concentrated with a rotary evaporator, and the product was purified by column chromatography (the eluent was pure dichloromethane). After removing the solvent, the product was a yellow solid powder (5.0 g, 47%). 1 H NMR (400 MHz, CDCl 3, δ):7.64-7.55(m,1H),4.21(d,J=4.8Hz,2H).

[0156] (3) Compound c was subjected to Knoevenagel reaction to give IC-2FBr.

[0157]

[0158] Synthesis of IC-2FBr: Compound c (5.0 g, 22 mmol) and anhydrous sodium acetate (2.1 g, 33 mmol) were dissolved in anhydrous ethanol (50 mL), and nitrogen was introduced to deoxygenate for 5 min. Then, malononitrile (2.2 g, 33 mmol) was injected into the system with a syringe, and the reaction was heated at 50 ° C for 2 h. After completion, the system was poured into sufficient water to quench, and acidified with 1 mol / L hydrochloric acid to pH < 1.0. The precipitated solid was filtered to obtain a crude product, which was a green solid powder, and then purified by column chromatography (eluent: dichloromethane) to obtain a pure product as a yellow solid powder (3.5 g, 51%). 1 H NMR (400 MHz, CDCl 3, δ):7.56(m,1H),3.34(s,2H).

[0159] (4) BTP-C8C10 and IC-2FBr were reacted by Knoevenagel reaction to obtain monomer M17-2.

[0160]

[0161] Synthesis of M17-2: Compounds BTP-C8C10 (0.2 g, 0.12 mmol) and IC-2FBr (0.15 g, 0.48 mmol) were dissolved in 20 mL of chloroform in turn, and bubbled for 30 min under a nitrogen atmosphere. Pyridine was then injected as an acid-binding agent, and the reaction was heated at 45°C for 3 h. After the reaction, the solvent was removed by a rotary evaporator, and the product was purified by column chromatography (the polarity of the eluent was petroleum ether: dichloromethane = 1:1). The final pure product was precipitated in methanol and dried to obtain a blue-black solid (yield of 75%). Figure 2 As shown, 1 H NMR (400 MHz, CDCl 3, δ):9.05(s,2H),8.53(d,J=8.0Hz,2H),7.85(s,1H),4.75(d,J=7.6Hz,4H),4.01(d ,J=7.6Hz,4H),2.11(m,2H),2.00(m,2H),1.75-0.99(m,128H),0.97-0.82(m,24H).

[0162] (5) The monomer compound M17-2 and the thiophene ditin reagent are reacted through Stille reaction to obtain the final polymer PW2.

[0163]

[0164] Synthesis of polymer PW2: M17-2 (0.1 g, 0.046 mmol), 2,5-di(trimethyltin)thiophene (0.0188 g, 0.046 mmol) and Pd(dba)3 (0.0028 g, 0.0024 mmol) were accurately weighed into a 10 mL pressure bottle, and 3 mL of ultra-dry toluene was added under a nitrogen atmosphere. The mixture was heated to 130 ° C for reaction. Heating was stopped after 72 hours, and after the system was cooled to room temperature, the reaction product was poured into methanol, the precipitate was collected, and the Soxhlet extraction method was used to extract with methanol, acetone, n-hexane and chloroform, respectively, and the chloroform component was collected. The solution was concentrated and dripped into a large amount of methanol solution with a glass dropper to precipitate, and the precipitate was collected. After drying, the target polymer was obtained as black solid particles with a yield of 51% (GPC: M n =6.78 kDa, M w =12.0 kDa, PDI = 1.77).

[0165] Example 4

[0166] The C2v symmetrical fused ring unit shown in formula I is BDTPT-C8C10, and the EG unit is When the electron donating unit is thienothiophene, the preparation method of the polymer material PW7 containing the C2v symmetrical fused ring unit:

[0167] (1) The monomer compound M17-2 and the thiophene ditin reagent are reacted by Stille reaction to obtain the final polymer PW7.

[0168]

[0169] Synthesis of PW7: Under nitrogen conditions, compound monomer M17-2 (215.6 mg, 0.1 mmol), 2,5-bis(trimethyltin)thieno[3,2-b]thiophene (46.7 mg, 0.1 mmol) and catalyst tetrakis(triphenylphosphine)palladium (11.6 mg, 0.01 mmol) were placed in a 25 mL thick-walled pressure bottle and 10 mL of toluene was added. Complete sealing. Use a 130°C oil bath to heat the reaction for 96 hours, precipitate the reaction liquid in methanol, and filter it. Then use Soxhlet extraction to wash with methanol solution, acetone solution, n-hexane solution, and chloroform solution for 12 hours each, and finally collect the product obtained when washing with chloroform solution, precipitate in methanol and filter it to obtain black solid polymer PW7 with a yield of 65% (GPC: Mn=5.0 kDa, Mw=11.6 kDa, PDI=2.34).

[0170] Example 5

[0171] The fused ring unit shown in formula I is BTP-C6C8, and the EG unit is IC-2FBr When the electron-donating unit is thiophene, the preparation method of the polymer material PW5 containing the C2v symmetrical fused ring unit is as follows:

[0172] (1) BDTPT-C6C8 and IC-2FBr were reacted by Knoevenagel reaction to obtain monomer M17-3.

[0173]

[0174] Synthesis of M17-3: Compounds BTP-C6C8 (0.2 g, 0.13 mmol) and IC-2FBr (0.15 g, 0.48 mmol) were dissolved in 20 mL of chloroform in turn, and bubbled for 30 min under a nitrogen atmosphere. Pyridine was then injected as an acid-binding agent, and the reaction was heated at 45 °C for 3 h. After the reaction, the solvent was removed by a rotary evaporator, and the product was purified by column chromatography (the polarity of the eluent was petroleum ether: dichloromethane = 1:1). The final pure product was precipitated in methanol and dried to obtain a blue-black solid (yield of 75%). Figure 3 As shown, 1 H NMR (400 MHz, CDCl 3,δ):9.05(s,2H),8.53(d,J=8.0Hz,2H),7.85(s,1H),4.75(d,J=7.6Hz,4H),4.01(d ,J=7.6Hz,4H),2.11(m,2H),2.00(m,2H),1.75-0.99(m,128H),0.97-0.82(m,24H).

[0175] (2) The monomer compound M17-3 and the thiophene ditin reagent are reacted through Stille reaction to obtain the final polymer PW5.

[0176]

[0177] Synthesis of polymer PW5: M17-3 (0.050 g, 0.023 mmol), 2,5-di(trimethyltin)thiophene (0.0094 g, 0.023 mmol) and Pd(PPh3)4 (0.0014 g, 0.0012 mmol) were accurately weighed into a 10 mL pressure bottle, and 2 mL of ultra-dry toluene was added under a nitrogen atmosphere. The mixture was heated to 130 °C for reaction. After 72 hours, the heating was stopped, and after the system was cooled to room temperature, the reaction product was poured into methanol, and the precipitate was collected. The precipitate was extracted with methanol, acetone, n-hexane and chloroform by Soxhlet extraction, and the chloroform component was collected. The solution was concentrated and dripped into a large amount of methanol solution with a glass dropper to precipitate. The precipitate was collected and dried to obtain the target polymer, which was black solid particles (yield 51%). GPC: Mn = 14.0 kDa, Mw = 38.4 kDa, PDI = 2.73.

[0178] Example 6

[0179] A solar cell device was prepared using the polymer material containing a C2v symmetrical fused ring unit obtained in Example 1 and tested.

[0180] The solar cell device adopts an upright device structure:

[0181] Glass substrate / ITO / PEDOT:PSS / active layer / PDIN / Al. Among them, the ITO layer is attached to the glass substrate. Subsequently, ITO and glass substrate are collectively referred to as ITO glass. The ITO glass is washed with detergent, water, acetone and isopropanol in sequence under ultrasound for thirty minutes each. Then it is dried in an oven at 90°C overnight. After the ITO glass is treated with ultraviolet ozone for 15 minutes, PEDOT:PSS is spin-coated on the ITO layer and placed in a 140°C oven for heating for 15 minutes, and then quickly transferred to a glove box for standby use. The polymer donor PM6 (purchased from Shuo Lun Organic Optoelectronics Technology (Beijing) Co., Ltd.) and the polymer receptor material PW-S (PM6:PW-S) obtained in Example 1 are dissolved in chloroform at a weight ratio of 1:1, and 1-chloronaphthalene with a volume ratio of 1% is added as an additive. The total concentration of the solution is 16 mg / mL, and the solution is stirred at 50°C for 4 hours, and then the solution is spin-coated on the PEDOT:PSS film as an active layer with a thickness of about 100 nm. In order to improve the electron injection efficiency, a methanol solution of PDIN (1.5 mg / mL containing 0.2% acetic acid) was spin-coated on the active layer. -5 100nm aluminum electrode was deposited under Pa conditions, and the device area was 4mm 2 .

[0182] The structure of PM6 is as follows:

[0183]

[0184] Example 7

[0185] Same as Example 6, the only difference is that the active layer is PM6:PW-Se.

[0186] Example 8

[0187] Same as Example 6, the only difference is that the active layer is PM6:PW2.

[0188] Example 9

[0189] Same as Example 6, the only difference is that the active layer is PM6:PW7.

[0190] Example 10

[0191] Same as Example 6, the only difference is that the active layer is PM6:PW5.

[0192] The performance tests were performed on the devices obtained in Examples 6 to 10:

[0193] The device was tested using an Oriel sol3A (Newport) solar simulator simulating AM 1.5G (100mW / cm2 ) and measured using a Keithley 2400 digital source meter tester.

[0194] The parameters of the solar cell devices obtained in Examples 6 to 10 are summarized in Table 1, and the corresponding current-voltage (JV) curves are shown in Table 1. Figure 7 .

[0195] Table 1. Parameters of solar cell devices prepared based on the acceptor materials

[0196] Active layer <![CDATA[V oc [V]]> <![CDATA[J sc [mA / cm 2 ]]> FF[%] PCE [%] PM6:PW-S 0.87 11.24 50.95 4.97 PM6:PW-Se 0.87 13.89 51.25 6.22 PM6:PW2 0.85 15.73 50.03 6.73 PM6:PW5 0.85 16.79 54.71 7.83 PM6:PW7 0.87 17.88 47.17 7.33

[0197] Figure 4 The ultraviolet absorption spectra of the polymer materials prepared in Examples 1-5 in the solution state are normalized for a more intuitive comparison. It can be seen from the figure that the absorption peaks of PW-S, PW-Se, PW2, PW5 and PW7 in the solution state are 788, 796, 794, 778 and 811 nanometers, respectively. Compared with PW-S based on thiophene electron-donating units, the absorption spectrum of PW-Se containing selenophene electron-donating units is red-shifted by 8 nanometers, which is mainly due to the strong electron-rich nature of the selenophene units. When the thiophene electron-donating unit (PW2) is further changed to a thiophene-thiophene copolymer unit (PW7) with stronger electron-donating ability, the absorption spectrum of the corresponding polymer is red-shifted by 17 nanometers. In addition, changing the terminal functional group from IC-FBr (PW-S) containing 1 fluorine atom to IC-2FBr (PW2) containing 2 fluorine atoms can also lead to a red-shifted absorption spectrum (red-shifted by 6 nanometers).

[0198] Figure 5 is the UV-visible absorption of five polymer materials in the thin film state. Compared with the absorption in the solution state, the absorption of the five polymers in the thin film state all shows a red shift phenomenon, which is mainly because the polymer molecular chains in the thin film state can form an orderly stacking. In addition, the change trend of the absorption spectrum in the thin film state is consistent with that in the solution state, and the length of the alkyl side chain has little effect on the absorption of the polymer in the thin film state. The absorption peaks of PW-S, PW-Se, PW2, PW5 and PW7 in the thin film are 795, 793, 797, 798 and 821 nanometers, respectively. According to the absorption cutoff edges of the five polymer materials, it can be calculated that the optical band gaps of PW-S, PW-Se, PW2, PW5 and PW7 are 1.38, 1.35, 1.38, 1.36 and 1.38 eV, respectively, which can form complementary absorption with wide band gap polymers.

[0199] from Figure 6It can be calculated that the initial oxidation potential and initial reduction potential of polymers PW-S, PW-Se, PW2, PW5 and PW7 are 0.87 / -0.81V, 0.82 / -0.87V, 0.91 / -0.79V, 0.90 / -0.82V and 0.80 / -0.87V, respectively. The highest occupied molecular orbital / lowest unoccupied molecular orbital calculated from this are -5.69 / -4.01eV, -5.64 / -3.95eV, -5.73 / -4.03eV, -5.72 / -4.00eV and -5.62 / -3.95eV, respectively. It can be found that compared with PW-S, PW2 with two fluorine atoms at the end group has a deeper electronic energy level, the length of the side chain has little effect on the energy level of the target polymer material, and the introduction of electron-rich units of selenophene or thienothiophene will lead to an upward shift in the electronic energy level. Although the energy levels of the five polymers obtained are different due to structural differences, they can still be well matched with the energy levels of common polymer donors, which is beneficial to improving the short-circuit current density of the corresponding devices.

[0200] from Figure 7 From Table 1, we can see that the device based on PM6:PW-S has the lowest efficiency, although its open circuit voltage (V oc ) up to 0.87V, but with a relatively low short-circuit current (J sc =11.24 mA cm -2 ) and fill factor (FF = 50.95%) resulted in a device conversion efficiency (PCE) of 4.97%. Under the same conditions, the device prepared based on the selenophene polymer PW-Se obtained a PCE of 6.22%, where V oc =0.87V, J sc =13.89 mA cm -2 , FF = 51.25%. The improvement of short-circuit current should be attributed to the wider absorption spectrum of PW-Se. With the introduction of the double fluorinated end group IC-2FBr, the PCE of the PW2-based device is further improved to 6.73%. oc and FF drop to 0.85V and 50.03% respectively, but this part of the loss can be overcome by its higher short-circuit current (J sc =15.73 mA cm -2 ) to make up for it. sc The substantial improvement may be due to the more regular main chain structure of PW2 promoting more ordered molecular stacking, leading to improved carrier transport performance of polymer materials. Although the side chain has little effect on absorption and energy levels, it has a great impact on the photovoltaic performance of the polymer. The device based on PM5 obtained a PCE of 7.83%, with V oc =0.85V, J sc =16.79 mA cm -2, FF = 54.71%. Compared with PW2, the use of thienothiophene as a copolymer unit can also improve the photovoltaic performance of the corresponding polymer material. The device efficiency based on PW7 is 7.33%, where V oc =0.87V, J sc =17.88 mA cm -2 , FF = 47.17%. The increase in open circuit voltage is mainly due to the higher LUMO energy level of PW7, while the larger short-circuit current is due to the wider absorption spectrum of PW7.

[0201] Figure 8 and Fig. 9 These are the EQE spectrum test results of PW-S and PW-Se as well as PW2, PW5, and PW7. This further verifies the reliability of the JV test. It can be seen that the range and peak shape of photon absorption by PW-S and PW-Se molecules are almost the same, but the PW-Se material shows a stronger absorption ability, and the absorption efficiency is about 5% higher than that of PW-S in the wavelength range of 450-800nm, which is also reflected in its integrated current. At the same time, it can be found that PW2 has a spectral response range and response peak shape close to that of PW5, but in the absorption range of 400-800nm ​​wavelength, its EQE value is relatively low by nearly 10%. This shows that PW5 molecules have better absorption and dissociation functions for photons than PW2 molecules. This may be related to the carrier migration performance of the two. Compared with the PW2 molecule, the PW7 molecule has a higher EQE value in the range of 400-800nm, and can still show a relatively ideal ability to absorb photons at 800-850nm. This is related to the relatively wider spectral absorption of PW7 molecules, and also reflects the difference in carrier migration performance between the two materials. sc The deviations are all within 5%, verifying the reliability of the experimental results.

[0202] The hole and electron mobility parameters of the mixed films prepared based on the polymer materials obtained in Examples 6 to 10 are summarized in Table 2. The JV curves of the corresponding single hole devices in the dark state are shown in Table 2. Fig.10 The JV curve of the single electron device in the dark state is shown in Fig.11 The hole mobility of PM6:PW-S and PM6:PW-Se mixed films is 1.5×10 -5 cm 2 V -1 s -1 , 1.1×10 -4 cm 2 V -1 s -1 , and the electron mobility is 1.1×10 -4 cm2 V -1 s -1 , 1.2×10 -4 cm 2 V -1 s -1 It can be seen that the two materials have similar electron mobility. Since PM6:PW-Se exhibits better hole mobility, it produces a more balanced carrier transport, which reduces the recombination of carriers during transport. This also explains the J of PM6:PW-Se devices. sc The hole mobility of PM6:PW2, PM6:PW5 and PM6:PW7 mixed films is 2.3×10 -5 , 3.97×10 -5 , 1.88×10 -5 cm 2 V -1 s -1 , and the electron mobility is 1.12×10 -4 cm 2 V -1 s -1 , 1.41×10 -4 cm 2 V -1 s -1 , 7.5×10 -5 cm 2 V -1 s -1 Therefore, the hole / electron mobility ratios of the three are 0.21, 0.28, and 0.25, respectively. The PM6:PW5-based devices exhibit higher and more balanced carrier transport, which explains the J sc The reason for the higher FF value.

[0203] Fig.12 and 13 The photocurrent density (J) of the solar cell devices prepared based on PM6:PW-S, PM6:PW-Se, PM6:PW2, PM6:PW5 and PM6:PW7 mixed films are shown in Figure 2. ph ) and effective voltage (V eff ) under short-circuit current conditions, J ph / J sat The ratio of the exciton dissociation probability of the material (P diss ), where J sat is the saturation photocurrent density. The results are shown in the figure. eff =1.3V, the device's J phAll reached saturation. Based on this, it can be calculated that the exciton dissociation efficiencies of PM6:PW-S and PM6:PW-Se devices are 86% and 92%, respectively. The exciton dissociation efficiencies of PM6:PW2, PM6:PW5 and PM6:PW7 are 81%, 87% and 81%, respectively. Compared with PM6:PW-S devices, PM6:PW-Se devices exhibit stronger exciton dissociation ability, which is consistent with their higher photovoltaic performance parameters. This may be due to the more suitable phase separation size of the PM6:PW-Se active layer, which in turn improves the dissociation of excitons. In addition, compared with PM6:PW2 devices, PM6:PW5 devices have higher exciton dissociation ability, which is also consistent with their better device efficiency. The exciton dissociation efficiency of PM6:PW7 devices is close to that of PM6:PW2 devices, indicating that the two have similar exciton dissociation and collection efficiencies.

[0204] Fig.14 The J of five groups of devices were analyzed. sc Dependence on light intensity. Usually, J sc It has a power law relationship with the incident light intensity (P), that is, J sc ∝P ɑ , where the exponential factor ɑ describes the bimolecular recombination in the device. The closer ɑ is to 1, the less bimolecular recombination there is in the device. As shown in the figure, the ɑ values ​​of photovoltaic devices based on PW-S, PW-Se, PW2, PW5 and PW7 are 0.83, 0.81, 0.96, 0.94 and 0.91 respectively. It can be found that when the end groups are the same, the recombination of the molecules is relatively close, among which the probability of bimolecular recombination of the material is lower when the IC-2FBr end group is used.

[0205] Fig.15 and 16 The grazing incidence wide angle X-ray diffraction (GIWAXS) spectra of the single component films of PW2 and PW5 and the blended films are shown in Figure 1. z ) directions, there are obvious (010) diffraction peaks, located at and . This shows that both molecules are more inclined to stack in the "face-on" orientation in the thin film state, which is beneficial to charge transport. In addition, PW5 molecules show shorter stacking distances and larger crystal coherence lengths than PW2. This shows that PW5 molecules have stronger crystallinity and tighter molecular stacking, which is beneficial to more efficient charge transport. In the GIWAXS images of PM6:PW2 and PM6:PW5 blends, the (010) diffraction peak representing the π-π stacking structure also appears in the out-of-plane direction, while the (100) diffraction representing the layered stacking structure appears in the in-plane direction. This shows that the introduction of polymer PM6 does not change the orientation behavior of the molecules, and the molecules in the two mixed films still tend to stack in the "face-on" orientation. Compared with the PM6:PW2 blend film, the PM6:PW5 blend film still shows a shorter π-π stacking distance and a longer crystal coherence length, which is beneficial to improving carrier transport and reducing charge recombination losses, thereby improving the photovoltaic performance of the corresponding devices. This is consistent with the better carrier transport and photovoltaic performance of PM6:PW5 hybrid films.

[0206] Table 2. Hole and electron mobility of the hybrid films prepared based on the acceptor materials

[0207]

[0208]

[0209] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A polymer material containing a C2v symmetrical fused ring unit, It is characterized in that The polymer material containing a C2v symmetrical fused ring unit is selected from one of the structures shown in PW-S, PW-Se, PW2, PW7, and PW5; n is the number of repeating structural units, and the value range of n is 10 to 1000.

2. The method for preparing the polymer material containing C2v symmetrical fused ring units according to claim 1, It is characterized in that include: In an inactive atmosphere, subjecting a mixture containing the compound represented by formula IV, the compound represented by formula V, and a catalyst to a Stille coupling reaction to obtain the polymer material containing the C2v symmetrical fused ring unit; Among them, R 1 Selected from One of; R 2 Selected from At least one of; X 1 , X 2 independently selected from S; Ar 1 ,Ar 2 independently derived from thiophene; EG comes from One of; DonorSelected One of the following, where * is a connection point.

3. The preparation method according to claim 2, It is characterized in that The catalyst is tetrakis(triphenylphosphine)palladium(0).

4. The preparation method according to claim 2, It is characterized in that The molar ratio of the compound represented by formula IV: the compound represented by formula V: tetrakis(triphenylphosphine)palladium(0) is 1:1:(0.01-0.5).

5. The preparation method according to claim 2, It is characterized in that The mixture contains a solvent, and the solvent is toluene.

6. The preparation method according to claim 2, It is characterized in that The inert atmosphere is selected from a nitrogen atmosphere and / or an argon atmosphere.

7. The preparation method according to claim 2, It is characterized in that The conditions of the Stille coupling reaction are: reaction temperature is 80-150° C., and reaction time is 24-96 hours.

8. The preparation method according to claim 2, It is characterized in that The conditions of the Stille coupling reaction are: reaction temperature is 100-130° C., and reaction time is 40-70 hours.

9. A semiconductor material, It is characterized in that The semiconductor material comprises at least one of the polymer material containing a C2v symmetrical fused ring unit according to claim 1 or the polymer material containing a C2v symmetrical fused ring unit prepared by the preparation method according to any one of claims 2 to 8.

10. A photoactive layer, It is characterized in that The photoactive layer contains the semiconductor material according to claim 9.

11. A polymer solar cell device, It is characterized in that The polymer solar cell device comprises the semiconductor material of claim 9 or comprises the photoactive layer of claim 10.

12. The polymer solar cell device according to claim 11, It is characterized in that The polymer solar cell device comprises a substrate, a cathode, a cathode modification layer, a photoactive layer, an anode modification layer and an anode, wherein the photoactive layer comprises an electron donor material and a polymer material containing a C2v symmetrical fused ring unit, and the mass ratio of the electron donor material to the polymer material containing a C2v symmetrical fused ring unit is (0.5-2.5):