Current collector and preparation method thereof, negative electrode and electrochemical energy storage device
By designing a current collector structure with through holes in the lithium battery to induce lithium deposition on the metal foil layer, combined with the placement of a conductive layer on the inner wall of the through hole, the problems of uneven lithium deposition and lithium dendrites in lithium batteries are solved. , improves electrochemical performance and safety, and extends battery life.
Patent Information
- Application Number
- CN202110610629.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-06-01
AI Technical Summary
Uneven deposition of lithium metal on the current collector in lithium batteries leads to low cycle life and may produce lithium dendrites that are safety hazards, affecting performance.
Design a current collector, including a first polymer layer, a metal foil layer and a second polymer layer stacked in sequence. Through holes penetrate the current collector to improve electrochemical consistency and specific surface area. The metal foil layer induces lithium deposition, and the conductive layer Set on the inner wall of the through hole to reduce interface impedance and the generation of dead lithium.
It can effectively avoid the generation of lithium dendrites, improve the electrochemical performance and safety of the negative electrode, and extend the service life of the battery.
Smart Images

Figure CN115440987B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of energy storage technology, and in particular to a current collector and a preparation method thereof, a negative electrode and an electrochemical energy storage device. Background Art
[0002] Lithium batteries have high energy density, good cycle stability, safety and other characteristics, and are widely used in many fields such as mobile phones, computers, automobiles and grid energy storage. The use of thin lithium foil in lithium metal batteries will bring high costs and safety risks in the battery manufacturing process, so it is inspired to use only the current collector as the negative electrode material, that is, theoretically zero excess lithium lithium metal batteries, which theoretically have higher energy density, but in actual use, lithium will be unevenly deposited on the current collector, resulting in dead lithium and low cycle life, and will also produce serious lithium dendrites and bring safety risks, affecting the performance of lithium batteries and limiting the application of lithium batteries. Summary of the invention
[0003] The present application discloses a current collector to solve the problem of uneven lithium deposition, avoid the generation of lithium dendrites, and improve its performance.
[0004] In a first aspect, the present application provides a current collector, which includes a first polymer layer, a metal foil layer, and a second polymer layer stacked in sequence, and the current collector has a plurality of through holes penetrating two opposite surfaces of the current collector in a stacking direction.
[0005] In the present application, the through hole runs through the current collector, which is conducive to the effective infiltration of the current collector by the electrolyte and improves the electrochemical consistency inside the current collector. At the same time, the setting of the through hole increases the specific surface area and internal space of the current collector. These internal spaces accommodate the lithium precipitated during the charging and discharging process, and the metal foil layer is arranged in the middle, which can induce lithium to be deposited on the internal metal foil layer, inhibit the formation of lithium dendrites, avoid the generation of dead lithium (inactive lithium), and reduce the interface impedance and the loss of active lithium; the current collector provided in the present application can be used directly as a negative electrode to improve the electrochemical performance and safety of the negative electrode.
[0006] Wherein, the current collector further includes a conductive layer, and the conductive layer is arranged on the inner side wall of the through hole.
[0007] Wherein, the through holes are distributed in an array form.
[0008] Wherein, the aperture of the through hole is less than or equal to 10 μm.
[0009] Wherein, the thickness of the metal foil layer is less than or equal to 4 μm.
[0010] Wherein, the thickness of the first polymer layer is 11 μm-26 μm.
[0011] Wherein, the thickness of the second polymer layer is 11 μm-26 μm.
[0012] Wherein, the current collector further includes a lithium-containing metal layer, and the lithium-containing metal layer is arranged in the metal foil layer.
[0013] Wherein, the thickness of the lithium-containing metal layer is 10nm-2μm.
[0014] Wherein, the current collector further includes a flame retardant layer, which is arranged on a side of the first polymer layer away from the metal foil layer, and / or the flame retardant layer is arranged on a side of the second polymer layer away from the metal foil layer.
[0015] Wherein, the thickness of the flame retardant layer is 10nm-1μm.
[0016] The first polymer layer contains a lithium supplement material, the mass proportion of the lithium supplement material in the first polymer layer is 0.1wt%-5wt%, and the first polymer layer is insulated on a side away from the metal foil layer, and / or
[0017] The second polymer layer contains a lithium supplement material, the mass proportion of the lithium supplement material in the second polymer layer is 0.1wt%-5wt%, and the side of the second polymer layer away from the metal foil layer is insulated.
[0018] The lithium supplement material includes at least one of Li-Mg, Li-Al, Li-Si, Li-Ag, Li-Au, Li-Sn, Li-In and Li-Ge alloy.
[0019] In a second aspect, the present application further provides a method for preparing a current collector, the current collector comprising:
[0020] The first polymer film, the metal foil film and the second polymer film are stacked in sequence to form a first composite structure;
[0021] Disposing a first protective film on a surface of the first polymer film facing away from the metal foil film, and disposing a second protective film on a surface of the second polymer film facing away from the metal foil film, to form a second composite structure;
[0022] forming a plurality of through holes on the second composite structure, wherein the through holes penetrate two opposite surfaces of the second composite structure in the stacking direction;
[0023] The first protective film and the second protective film are removed to obtain a current collector.
[0024] In a third aspect, the present application further provides a negative electrode, which comprises a current collector prepared by the preparation method described in the first aspect or the second aspect.
[0025] In a fourth aspect, the present application further provides an electrochemical energy storage device, which comprises a positive electrode and the negative electrode described in the third aspect.
[0026] Among them, the porosity β of the current collector, the surface capacity C of the positive electrode, the thickness d of the current collector in the stacking direction and the capacity-thickness constant k satisfy the formula:
[0027]
[0028] The β≥50%, the C≥5mAh / cm 2 , k = 5 × 10 -4 cm 3 / mAh. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes will be briefly introduced below. Obviously, the drawings described below are only some implementation modes of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0030] Figure 1 A schematic top view of a current collector provided in one embodiment of the present application.
[0031] Figure 2 for Figure 1 Schematic cross-sectional view along line II.
[0032] Figure 3 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.
[0033] Figure 4 A schematic cross-sectional view of a current collector provided in another embodiment of the present application
[0034] Figure 5 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.
[0035] Figure 6 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.
[0036] Figure 7 A schematic diagram of the current collector preparation process provided in one embodiment of the present application.
[0037] Figure 8 A schematic cross-sectional view of an electrochemical energy storage device provided in one embodiment of the present application.
[0038] Description of Figure Numbers:
[0039] Current collector-1, first polymer layer-11, metal foil layer-12, second polymer layer-13, through hole-14, first sub-through hole-141, second sub-through hole-142, third sub-through hole-143, conductive layer-15, lithium metal containing layer-16, flame retardant layer-17, electrochemical energy storage device-2, positive electrode-21, negative electrode-22, separator-23. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0041] This application provides a current collector 1, please refer to Figure 1 and Figure 2 , Figure 1 A schematic top view of a current collector provided in one embodiment of the present application; Figure 2 for Figure 1 The current collector 1 comprises a first polymer layer 11, a metal foil layer 12 and a second polymer layer 13, which are stacked in sequence, and the current collector 1 has a plurality of through holes 14 penetrating two opposite surfaces of the current collector 1 in the stacking direction.
[0042] The current collector 1 provided in the present application is provided with a through hole 14 that penetrates the current collector 1, which is conducive to the effective infiltration of the current collector 1 by the electrolyte and improves the electrochemical consistency inside the current collector 1; at the same time, the setting of the through hole 14 increases the specific surface area and internal space of the current collector 1, and these internal spaces accommodate the lithium precipitated during the charging and discharging process, and inhibit the generation of lithium dendrites; the stacked structure allows the metal foil layer 12 to be set inside the current collector 1, which can induce lithium to be deposited on the metal foil layer 12 inside the current collector 1, inhibit the generation of lithium dendrites, avoid the generation of dead lithium (inactive lithium), reduce the interface impedance, avoid the loss of active lithium, and improve the electrochemical performance and safety of use. Compared with the current collector of a single metal layer, the current collector 1 provided in the present application avoids the deposition of lithium on the surface of the current collector 1 by setting the first polymer layer 11 and the second polymer layer 13, effectively ensuring its performance and safety performance, and the setting of the through hole 14 further improves the performance, which is conducive to its application.
[0043] It can be understood that, since the current collector 1 has through holes 14 , the first polymer layer 11 , the metal foil layer 12 and the second polymer layer 13 are all porous layer structures.
[0044] In this embodiment, the material of the first polymer layer 11 can be selected from at least one of polyethylene, polypropylene, polyimide, polytetrafluoroethylene, polyvinylidene fluoride, polyester and polyacrylonitrile, and this application is not limited to this. In this embodiment, the material of the second polymer layer 13 can be selected from at least one of polyethylene, polypropylene, polyimide, polytetrafluoroethylene, polyvinylidene fluoride, polyester and polyacrylonitrile, and this application is not limited to this. In one embodiment, the material of the first polymer layer 11 and the second polymer layer 13 is the same. Specifically, the material of the first polymer layer 11 and the second polymer layer 13 can be, but is not limited to, polyethylene terephthalate.
[0045] In the present embodiment, the thickness of the first polymer layer 11 is 11 μm-26 μm. That is, the thickness of the first polymer layer 11 in the stacking direction. Further, the thickness of the first polymer layer 11 is 15 μm-23 μm. Specifically, the thickness of the first polymer layer 11 may be, but not limited to, 11 μm, 13 μm, 15 μm, 18 μm, 21 μm, 25 μm, 26 μm, etc. In the present embodiment, the thickness of the second polymer layer 13 is 11 μm-26 μm. That is, the thickness of the second polymer layer 13 in the stacking direction. Further, the thickness of the second polymer layer 13 is 15 μm-23 μm. Specifically, the thickness of the second polymer layer 13 may be, but not limited to, 12 μm, 14 μm, 17 μm, 23 μm, 24 μm, etc. In one embodiment, the thickness of the first polymer layer 11 is the same as the thickness of the second polymer layer 13.
[0046] In this embodiment, the first polymer layer 11 and / or the second polymer layer 13 contain lithium supplement material. Thus, the consumed lithium is supplemented during the charge and discharge process, and the energy density and cycle life are improved. Furthermore, the lithium supplement material includes at least one of Li-Mg, Li-Al, Li-Si, Li-Ag, Li-Au, Li-Sn, Li-In and Li-Ge alloys. Thus, lithium can be supplemented effectively. In one embodiment, the mass proportion of the lithium supplement material in the first polymer layer 11 is 0.1wt%-5wt%. In another embodiment, the mass proportion of the lithium supplement material in the second polymer layer 13 is 0.1wt%-5wt%. The use of the above-mentioned content of lithium supplement material is not only conducive to the supplement of lithium, but also does not affect the insulation properties of the first polymer layer 11 and the second polymer layer 13. Specifically, the mass proportion of the lithium supplement material in the first polymer layer 11 may be, but not limited to, 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt% or 4wt%, and the mass proportion of the lithium supplement material in the second polymer layer 13 may be, but not limited to, 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt% or 4wt%, etc. In the present application, when the first polymer layer 11 adopts the lithium supplement material of the above content, the electronic conductivity of the side of the first polymer layer 11 away from the metal foil layer 12 is relatively low, thereby ensuring that the metal lithium will not be preferentially deposited on the surface of the first polymer layer 11, avoiding the generation of lithium dendrites and dead lithium, and at the same time extending the service life of the battery; when the second polymer layer 13 adopts the lithium supplement material of the above content, the electronic conductivity of the side of the second polymer layer 13 away from the metal foil layer 12 is relatively low, thereby ensuring that the metal lithium will not be preferentially deposited on the surface of the second polymer layer 13, avoiding the generation of lithium dendrites and dead lithium, and at the same time extending the service life of the battery. In one embodiment, the first polymer layer 11 contains lithium supplement material, and the side of the first polymer layer 11 facing away from the metal foil layer 12 is insulated. In another embodiment, the second polymer layer 13 contains lithium supplement material, and the side of the second polymer layer 13 facing away from the metal foil layer 12 is insulated.
[0047] In the present application, the metal foil layer 12 disposed inside the current collector 1 ensures the preferential deposition of lithium inside, avoids the generation of lithium dendrites, and is beneficial to the improvement of its electrochemical performance.
[0048] In this embodiment, the material of the metal foil layer 12 includes at least one of copper, gold, silver, magnesium, zinc, titanium and nickel, or stainless steel. Further, the material of the metal foil layer 12 includes at least one of copper, copper alloy, silver, titanium and nickel, or stainless steel. Specifically, the metal foil layer 12 can be, but is not limited to, copper foil, copper alloy foil, stainless steel foil, silver foil, titanium foil or nickel foil. In one embodiment, the metal foil layer 12 is copper foil or copper alloy foil.
[0049] In this embodiment, the thickness of the metal foil layer 12 is less than or equal to 4 μm. That is, the thickness of the metal foil layer 12 in the stacking direction. Further, the thickness of the metal foil layer 12 is less than or equal to 3 μm. Specifically, the thickness of the metal foil layer 12 can be, but is not limited to, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 3 μm, 4 μm, etc.
[0050] In this embodiment, the thickness of the metal foil layer 12 is less than the thickness of the first polymer layer 11, and the thickness of the metal foil layer 12 is less than the thickness of the second polymer layer 13. As a result, the metal foil layer 12 accounts for a relatively small proportion of the overall current collector 1, which can reduce the mass and volume proportion of the inactive components and improve the energy density of the current collector 1; it also ensures that the setting of the through hole 14 does not affect the strength of the current collector too much, which is beneficial to increase the aperture of the through hole 14 and the porosity of the current collector 1. In one embodiment, the thickness of the metal foil layer 12 is less than or equal to 4 μm, the thickness of the first polymer layer 11 is 11 μm-26 μm, and the thickness of the second polymer layer 13 is 11 μm-26 μm.
[0051] In the present application, the current collector 1 has a plurality of through holes 14, and the through holes 14 penetrate two opposite surfaces of the current collector 1 in the stacking direction. Figure 2 In one embodiment, the direction indicated by the arrow is the stacking direction.
[0052] In this embodiment, please refer to Figure 1 The through holes 14 are evenly distributed in an array, which is conducive to the uniform deposition of lithium precipitated during the charge and discharge process, avoiding excessive local lithium deposition and protrusion, and further improving the safety performance.
[0053] In this embodiment, the aperture of the through hole 14 is less than or equal to 10 μm. Further, the aperture of the through hole 14 is less than 8 μm. Specifically, the aperture of the through hole 14 can be, but is not limited to, 3 μm, 4 μm, 5 μm, 6 μm, 8 μm, etc. By providing the through hole 14 with a small aperture, it is further ensured that the electrolyte passes through the through hole 14 slowly, and the current collector 1 is well immersed in the electrolyte, thereby further improving the consistency of the electrochemical performance.
[0054] In this embodiment, if Figure 2As shown, the first polymer layer 11 has a first sub-through hole 141, the metal foil layer 12 has a second sub-through hole 142, and the second polymer layer 13 has a third sub-through hole 143. The first sub-through hole 141 and the third sub-through hole 143 are connected through the corresponding second sub-through hole 142 to form a through hole 14. Specifically, the first sub-through hole 141, the second sub-through hole 142, and the third sub-through hole 143 all have an accommodating space, so that when the current collector 1 is infiltrated with the electrolyte, the electrolyte can more evenly infiltrate the interior of the current collector 1, that is, the inner surfaces of the first sub-through hole 141, the second sub-through hole 142, and the third sub-through hole 143.
[0055] In this embodiment, the aperture shape of the through hole 14 in the current collector 1 includes at least one of a cylindrical shape, a rectangular tube shape, a cubic tube shape, a trapezoidal cylindrical shape, and a triangular pyramid shape. Specifically, as long as it does not affect the connection between the first sub-through hole 141 and the third sub-through hole 143 through the corresponding second sub-through hole 142, the present application does not limit the aperture shape of the through hole 14. Specifically, the cross-section of the through hole 14 may be, but not limited to, a polygon, a circle, an ellipse, an irregular shape, etc., and the longitudinal section of the through hole 14 may be, but not limited to, a rectangle, a trapezoid, a quasi-trapezoidal shape, a cone, a quasi-conical shape, an irregular shape, etc. In one embodiment, the inner side wall of the through hole 14 is inclined, and the cross-section of the through hole 14 gradually increases from the metal foil layer 12 to the first polymer layer 11, and the cross-section of the through hole 14 gradually increases from the metal foil layer 12 to the second polymer layer 13. Thereby, the specific surface area of the through hole 14 is increased, which is beneficial to the deposition of lithium. Please refer to Figure 1 and Figure 2 , wherein the aperture shape of the through hole 14 is cylindrical. Figure 3 , is a schematic cross-sectional view of a current collector provided in another embodiment of the present application, wherein the longitudinal cross-sectional shape of the aperture of the through hole 14 is a trapezoid. In one embodiment, when the cross-sectional shape of the through hole 14 is circular and the longitudinal cross-sectional shape is a trapezoid, the through hole 14 is a trapezoidal cylinder. Further, the longitudinal cross-sectional shape of the aperture of the through hole 14 is a trapezoid, and the trapezoid is a shape where the short sides of two trapezoids intersect, and the cross-sectional shape of the through hole 14 gradually increases from the metal foil layer 12 to the two ends of the current collector 1. In this embodiment, as Figure 3 As shown, the cross-sectional area at the maximum aperture of the second sub-through hole 142 is less than or equal to the cross-sectional area at the minimum aperture of the first sub-through hole 141 and the third sub-through hole 143. It can be understood that this arrangement makes it easier for the conductive material to be deposited on the inner sidewalls of the first sub-through hole 141, the second sub-through hole 142 and the third sub-through hole 143 when the current collector 1 has the conductive layer 15.
[0056] In this implementation, see Figure 4, is a schematic cross-sectional view of a current collector provided in another embodiment of the present application, the current collector 1 also includes a conductive layer 15, and the conductive layer 15 is arranged on the inner side wall of the through hole 14. It can be understood that the conductive layer 15 does not block the through hole 14, and the interior of the current collector 1 still has a hollow space. By arranging the conductive layer 15 in the through hole 14, the metallic lithium can be deposited in the internal space of the current collector 1, avoiding deposition on the surface of the current collector 1, effectively reducing the formation of dead lithium, and improving the electrochemical performance.
[0057] In one embodiment, the conductive layer 15 is formed by depositing or impregnating a conductive material on the inner side wall of the through hole 14. Further, the inner side walls of the first sub-through hole 141, the second sub-through hole 142, and the third sub-through hole 143 are deposited with a conductive material, which can effectively reduce the phenomenon of by-product generation, thereby extending the service life of the current collector 1. In one embodiment, the material of the conductive layer 15 includes at least one of a metal material, a carbon material, and a conductive polymer material. Specifically, the material of the conductive layer 15 includes at least one of gold, silver, copper, nickel, iron, aluminum, germanium, tin, zinc, indium, vanadium, magnesium, cobalt, carbon, polyaniline, and polypyrrole.
[0058] See also Figure 5 , is a schematic cross-sectional view of a current collector provided in another embodiment of the present application, wherein the current collector 1 also includes a lithium-containing metal layer 16, and the lithium-containing metal layer 16 is disposed in the metal foil layer 12. By providing the lithium-containing metal layer 16, the lithium consumed by the reaction between the electrolyte and the deposited lithium can be supplemented, thereby improving the energy density and cycle life. In one embodiment, the material of the lithium-containing metal layer 16 may include at least one of lithium and a lithium alloy. Specifically, the lithium alloy includes at least one of Li-Ag, Li-Mg, Li-Zn, Li-AL, Li-Au, Li-Si, Li-Sn and Li-Ge alloys. In one embodiment, the thickness of the lithium-containing metal layer 16 is 10nm-2μm. Further, the thickness of the lithium-containing metal layer 16 is 100nm-1.5μm. Further, the thickness of the lithium-containing metal layer 16 is 300nm-1000nm. Specifically, the thickness of the lithium-containing metal layer 16 can be, but is not limited to, 100 nm, 400 nm, 500 nm, 800 nm, 1 μm, 1.5 μm, 1.8 μm, 2 μm, etc. In one embodiment, the lithium-containing metal layer 16 is disposed inside the metal foil layer 12. In other words, the lithium-containing metal layer 16 is coated by the metal foil layer 12. In another embodiment, the metal foil layer 12 includes a first porous metal layer and a second porous metal layer, and the first porous metal layer, the lithium-containing metal layer 16 and the second porous metal layer are stacked in sequence. It should be noted that the through hole 14 also penetrates the lithium-containing metal layer 16 of the flame retardant layer.
[0059] See also Figure 6, is a schematic cross-sectional view of a current collector provided in another embodiment of the present application, wherein the current collector 1 further includes a flame retardant layer 17, and the flame retardant layer 17 is disposed on the side of the first polymer layer 11 away from the metal foil layer 12, and / or the flame retardant layer 17 is disposed on the side of the second polymer layer 13 away from the metal foil layer 12. When the current collector 1 is used in the electrochemical energy storage device 2, the metal lithium has high activity, and it is easy to cause the electrochemical energy storage device 2 to burn when a short circuit occurs, causing a safety accident. By providing the flame retardant layer 17, at the initial stage of the short circuit, the flame retardant layer 17 can be melted by heat, can block the holes, and wrap the metal lithium deposited in the through hole 14, to prevent the metal lithium from further contacting the electrolyte to cause thermal runaway, and the melted flame retardant layer 17 can block the first sub-through hole 141 in the adjacent first polymer layer 11, and / or the second sub-through hole 142 in the second polymer layer 13, to isolate the ion channel, eliminate safety hazards, and improve the safety of use. Further, the melting point of the material of the flame retardant layer 17 is 120°C-155°C. The use of low melting point flame retardant materials is more conducive to flame retardancy. It should be noted that when the flame retardant layer 17 is arranged on the side of the first polymer layer 11 away from the metal foil layer 12, and / or the second polymer layer 13 away from the side of the metal foil layer 12, the through hole 14 also penetrates the flame retardant layer 17; that is, the flame retardant layer 17 is also provided with a plurality of holes, and the holes are correspondingly connected to the first sub-through hole 141 and / or the third sub-through hole 143. In this embodiment, the material of the flame retardant layer 17 includes one or more of polyethylene wax, polypropylene wax and polyethylene oxide wax. In this embodiment, in order not to affect the overall thickness of the current collector 1, the thickness of the flame retardant layer 17 is relatively small, and its thickness range can be but is not limited to 10nm-1μm, 50nm-0.8μm, 100nm-0.7μm or 200nm-0.5μm, etc.
[0060] The present application does not specifically limit the specific preparation method of the current collector 1. Next, an example of a preparation method of the current collector 1 provided in the present application will be described.
[0061] See also Figure 7 , is a schematic diagram of a current collector preparation process provided in an embodiment of the present application. The current collector 1 preparation method comprises: steps S701, S702, S703, and S704. Steps S701, S702, S703, and S704 are described in detail as follows.
[0062] S701: A first polymer film, a metal foil film, and a second polymer film are stacked in sequence to form a first composite structure.
[0063] In one embodiment, the first polymer film, the metal foil film, and the second polymer film are sequentially stacked and arranged, including: depositing metal on the first polymer film to form a metal foil film; and then forming a second polymer film on the metal foil film by at least one of liquid phase coating, atomic deposition, and melt extrusion calendering processes. In another embodiment, the first polymer film, the metal foil film, and the second polymer film are sequentially stacked and arranged, including: providing a substrate, depositing metal on the substrate, and peeling off to form a metal foil film; and then forming the first polymer film and the second polymer film on two opposite surfaces of the metal foil film by at least one of liquid phase coating, atomic deposition, and melt extrusion calendering processes. Specifically, deposition can be, but is not limited to, by magnetron sputtering, ion plating, vacuum evaporation, etc. Specifically, the process parameters of deposition can be selected as needed, and this application does not limit this. In one embodiment, the first polymer film, the metal foil film, and the second polymer film are sequentially stacked and arranged, including installing the first polymer film in a vacuum magnetron sputtering coating machine, and evacuating the chamber with a vacuum pump to make the vacuum degree of the cavity reach 8×10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 -1 Pa, the first polymer film is surface cleaned by ion source, the cleaning time is 5min-15min, after the cleaning is completed, the ion source power is turned off; the metal plating power is started to magnetron sputter the metal foil film, the sputtering time of the metal foil film is 5min-100min, and a metal foil film with a thickness less than or equal to 4μm is obtained.
[0064] S702: disposing a first protective film on a surface of the first polymer film that is away from the metal foil film, and disposing a second protective film on a surface of the second polymer film that is away from the metal foil film, to form a second composite structure.
[0065] In this embodiment, the protective film may be, but is not limited to, at least one of transparent adhesive, engineering paper, and plastic wrap.
[0066] S703: forming a plurality of through holes on the second composite structure, wherein the through holes penetrate two opposite surfaces of the second composite structure in the stacking direction.
[0067] In this embodiment, the through holes 14 are formed by forming a plurality of first sub-through holes 141 in the first polymer film to form the first polymer layer 11, forming a plurality of second sub-through holes 142 in the metal foil film to form the metal foil layer 12, and forming a plurality of third sub-through holes 143 in the second polymer film to form the second polymer layer 13. In this embodiment, the plurality of through holes are formed on the second composite structure by ultrafast laser.
[0068] S704, removing the first protective film and the second protective film to obtain a current collector.
[0069] In this embodiment, the preparation method of the current collector 1 further includes depositing a conductive material on the inner side wall of the through hole 14 to form a conductive layer 15. Specifically, the conductive material can be disposed on the inner side wall of the through hole 14 by thermal evaporation sputtering, magnetron sputtering or impregnation to form a conductive layer 15, such as being disposed on the inner side wall of the first sub-through hole 141, the second sub-through hole 142 and the third sub-through hole 143. It should be noted that by controlling the length of time for depositing the conductive material, the conductive material can be controlled to be partially deposited on the inner side wall of the first sub-through hole 141, the second sub-through hole 142 and the third sub-through hole 143, so as to avoid the conductive material blocking the through hole 14 due to too long deposition time.
[0070] The present application also provides a negative electrode 22, and the negative electrode 22 includes the current collector 1 in any of the above embodiments. Specifically, the current collector 1 is described above and will not be repeated here. In the present application, the current collector 1 can be used directly as the negative electrode 22, and the negative electrode 22 does not need to be provided with a negative electrode active material layer. At this time, the negative electrode 22 is a lithium-free negative electrode. When the current collector 1 provided in the present application is used as the negative electrode 22, the electrochemical performance and safety performance of the negative electrode 22 can be greatly improved.
[0071] The present application also provides an electrochemical energy storage device 2, which includes the negative electrode 22 as described above. Figure 8 , is a cross-sectional schematic diagram of an electrochemical energy storage device provided in one embodiment of the present application, wherein the electrochemical energy storage device 2 includes a positive electrode 21 and a negative electrode 22. In one embodiment, the current collector 1 serves as the negative electrode 22 of the electrochemical energy storage device 2.
[0072] Specifically, in the present embodiment, the electrochemical energy storage device 2 is a lithium-free negative electrode-lithium battery, that is, a negative electrode-free battery. In other possible embodiments, the electrochemical energy storage device 2 may also be other types of batteries, which is not limited in the present application.
[0073] In this embodiment, the porosity β of the current collector 1, the surface capacity C of the positive electrode 21, the thickness d of the current collector 1 in the stacking direction, and the capacity-thickness constant k satisfy the formula:
[0074]
[0075] Where k = 5 × 10 -4 cm 3 / mAh.
[0076] It should be noted that, in general, the electrochemical energy storage device 2 includes a positive electrode 21 and a negative electrode 22, and the current collector 1 serves as the negative electrode 22 of the electrochemical energy storage device 2. The porosity β of the current collector 1 refers to the percentage of the total volume of the through hole 14 to the total volume of the current collector 1, and the surface capacity of the positive electrode 21 refers to the total number of electrons that can be released per unit surface area of the positive electrode 21 of the electrochemical energy storage device 2. By setting the porosity of the current collector 1 and the thickness of the current collector 1, the surface capacity of the positive electrode 21 can be increased, thereby increasing the overall energy density. In one embodiment, β ≥ 50%, C ≥ 5mAh / cm 2 The higher porosity can ensure that the space required for lithium deposition can be met when the thickness of the current collector 1 is relatively low, avoiding the volume expansion caused by disordered lithium deposition and improving the safety performance of the current collector 1. Furthermore, β ≥ 60%, C ≥ 6 mAh / cm 2 .
[0077] In this embodiment, the positive electrode 21 includes a positive electrode current collector and a positive electrode active material layer. In one embodiment, the material of the positive electrode active material layer includes LiFe a Mn b M c PO4, Li3V2(PO4)3, Li3V3(PO4)3, LiNi 0.5-d Mn 1.5-e N d + e O4, LiVPO4F, Li1+ f L 1-g-h H g R h O2, Li2CuO2, Li5FeO4 or more; wherein 0≤a≤1, 0≤b≤1, 0≤c≤1, a+b+c=1, M is at least one of Al, Mg, Ga, Ti, Cr, Cu, Zn, and Mo; -0.1≤d≤0.5, 0≤e≤1.5, N is at least one of Li, Co, Fe, Al, Mg, Ca, Ti, Mo, Cr, Cu, and Zn; -0.1≤f≤0.2, 0≤g≤1, 0≤h≤1, 0≤g+h≤1.0, L, H, and R are independently selected from at least one of Li, Co, Mn, Ni, Fe, Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo, F, I, S, and B. In a specific embodiment, the material of the positive electrode active material layer includes LiAl 0.05 Co 0.15 Ni 0.80 O2、LiNi 0.80 Co 0.10 Mn 0.10 O2、LiNi 0.90 Co 0.05 Mn 0.05O2、LiNi 0.60 Co 0.20 Mn 0.20 O2, LiCoO2, LiMn2O4, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, LiNi 0.5 Mn 1.5 At least one of O4 and Li3V3(PO4)3. In another specific embodiment, the material of the positive electrode active material layer includes at least one of lithium sulfide, lithium-intercalated V2O5, lithium-intercalated MnO2, lithium-intercalated TiS2 and lithium-intercalated FeS2.
[0078] In this embodiment, the electrochemical energy storage device 2 further includes a separator 23 disposed between the positive electrode 21 and the negative electrode 22. The separator 23 is used to separate the positive electrode 21 and the negative electrode 22 of the electrochemical energy storage device 2, and the present application does not limit the material of the separator 23.
[0079] The electrochemical energy storage device 2 provided in the embodiment of the present application includes the above-mentioned current collector 1, and the current collector enables the electrochemical energy storage device 2 to have a high energy density, a high charge and discharge capacity, is not prone to the generation of lithium dendrites, has high safety performance, and a long cycle life.
[0080] Next, the implementation methods of the present application will be further described with reference to a number of examples.
[0081] Example 1
[0082] A method for preparing a current collector, comprising:
[0083] (1) The first PET film (thickness 18 μm) was installed in a vacuum magnetron sputtering coating machine, and the vacuum degree of the chamber was evacuated by a vacuum pump to 8×10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 -1 Pa, the first PET film is cleaned by a surface ion source for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform a magnetron sputtering copper plating process for 30 minutes to obtain a metal copper foil with a thickness of 4 μm;
[0084] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the metal copper foil away from the first PET film to prepare a second PET film with a thickness of about 18 μm;
[0085] (3) a transparent adhesive protective film is provided on the surfaces of the first PET film and the second PET film facing away from the metal copper foil to obtain a composite structure; an ultrafast laser (wavelength 355 nm) is used to form a plurality of through holes arranged in an array on the composite structure, the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the aperture of the through holes is 10 μm, to obtain a porous composite structure;
[0086] (4) The porous composite structure was transferred to the thermal evaporator and the vacuum pump was evacuated to a vacuum degree of 4×10 -1 Pa, raise the temperature to 400°C, deposit metal magnesium on the inner wall surface of the through hole for 10 minutes, cool to 100°C, turn off the vacuum, take out and peel off the transparent adhesive protective film to obtain the current collector Z1, whose porosity is 75%.
[0087] Example 2
[0088] A method for preparing a current collector, comprising:
[0089] It is substantially the same as Example 1, except that the thickness of the first PET film and the second PET film is 16.75 μm, the porosity and the pore size are 80% and 10 μm, respectively, to obtain a current collector Z2.
[0090] Example 3
[0091] A method for preparing a current collector, comprising:
[0092] It is substantially the same as Example 1, except that the thickness of the first PET film and the second PET film is 28 μm, the porosity and the pore size are 50% and 5 μm, respectively, to obtain a current collector Z3.
[0093] Example 4
[0094] A method for preparing a current collector, comprising:
[0095] The method is substantially the same as Example 1, except that the transparent adhesive protective film is directly removed after step (3) and step (4) is not performed, thereby obtaining current collector Z4.
[0096] Example 5
[0097] A method for preparing a current collector, comprising:
[0098] It is substantially the same as Example 1, except that a plurality of through holes are arranged in a disordered manner to obtain a current collector Z5.
[0099] Example 6
[0100] A method for preparing a current collector, comprising:
[0101] The method is substantially the same as Example 1, except that the thickness of the metal copper foil is 8 μm, and the thickness of the first PET film and the second PET film is 16 μm, to obtain a current collector Z6.
[0102] Example 7
[0103] A method for preparing a current collector, comprising:
[0104] The method is substantially the same as Example 1, except that the porosity and pore size are 50% and 10 μm, respectively, to obtain current collector Z7.
[0105] Example 8
[0106] A method for preparing a current collector, comprising:
[0107] It is substantially the same as Example 1, except that a porous polypropylene wax flame retardant layer is provided on the surface of the first PET film facing away from the metal copper foil and on the surface of the second PET film facing away from the metal copper foil, thereby obtaining a current collector Z8.
[0108] Example 9
[0109] A method for preparing a current collector, comprising:
[0110] The method is substantially the same as Example 1, except that the second PET film contains magnesium-aluminum alloy particles, the mass proportion of the magnesium-aluminum alloy particles in the second PET film is 1 wt %, and the surface of the second PET film is insulated, thereby obtaining a current collector Z9.
[0111] Example 10
[0112] A method for preparing a current collector, comprising:
[0113] The method is substantially the same as Example 1, except that the porosity and pore size are 80% and 10 μm, respectively, to obtain a current collector Z10.
[0114] Comparative Example 1
[0115] The method is substantially the same as Example 1, except that in step (4), the transparent adhesive protective film on the surface is first peeled off and removed, and then the same evaporation process is performed to obtain the current collector DZ1.
[0116] Comparative Example 2
[0117] It is roughly the same as Example 1, except that the processing time of each laser pore making in step (3) is reduced by half, and a non-through hole array porous structure with a pore size of 10 μm is obtained. Due to the non-through holes, the porosity is 67.5%, and the current collector DZ1 is obtained.
[0118] In order to illustrate the electrochemical performance of the current collector provided in the embodiment of the present application, the following test steps are now performed:
[0119] (1) Preparation of full battery and electrochemical cycle testing:
[0120] ① Use a vacuum mixer to mix 49g of positive electrode active material (LiFePO4), 0.5g of conductive agent (acetylene black) and 0.5g of binder (polyvinylidene fluoride, PVDF) in NMP to form a stable and uniform slurry, wherein the stirring speed is 1000rpm and the time is 12h; then the obtained slurry is coated on the current collector aluminum sheet, and the surface density is controlled to be 220g / m 2 , and then dried at 80℃, and then cut into 61×72mm positive electrode sheets; then dried at 80℃, and rolled by a roller press to obtain positive electrode sheets, one of which was cut into 13mm diameter sheets to assemble button batteries for capacity calibration, and the calibrated capacity was 6mAh / cm 2 .
[0121] ② The current collector Z or DZ obtained in the above embodiments and comparative examples is directly used as the negative electrode, and is stacked layer by layer with the separator and the positive electrode sheet to assemble into a battery, and 2.2mL / Ah electrolyte is added dropwise, and the electrolyte is 1wt% LiNO3 dissolved in 4MLiFSI ethylene glycol dimethyl ether (DME), and then packaged to obtain batteries S1-S10 and DS1-DS2, respectively.
[0122] Take 5 batteries S1-S10 and DS1-DS2 respectively, and test the battery charge and discharge cycle at 0.2C at 25℃ on the secondary battery performance test device. The steps are as follows: leave for 10 minutes; charge at 0.2C constant current to 3.8V, charge at constant voltage to 3.8V / 0.05C; leave for 10 minutes; discharge at 0.5C to 2.7V, which is 1 cycle. Repeat this step. When the battery capacity is lower than 80% of the initial discharge capacity during the cycle, the cycle is terminated. The number of cycles is the cycle life of the battery. The average value is taken for each group. The data of this parameter and the average initial discharge capacity of the battery, as well as the thickness change rate before and after the battery cycle are shown in Table 1.
[0123] Table 1 Data of average initial discharge capacity of the battery and thickness change rate before and after battery cycling
[0124]
[0125] (2) Impedance (EIS) test: Two batteries S1-S10 and 2 batteries DS1-DS2 were injected with liquid and left to stand. Impedance tests (amplitude 5 mV, frequency 1000-0.01 Hz) were performed every 0.5 h. The experimental results are shown in Table 2.
[0126] Table 2 Battery impedance change table (Ω)
[0127]
[0128] (3) Energy density: Energy density was evaluated based on the experimental results in Table 1. The experimental results are shown in Table 3.
[0129] Table 3 Battery energy density evaluation table
[0130]
[0131] (4) Lithium metal deposition experiment: Two batteries S1-S10 and 2 batteries DS1-DS2 were used for the first lithium deposition. 2 The battery was charged to 3.8 V at a current density of , and the lithium deposition position was observed. The experimental results are shown in Table 4.
[0132] Table 4 Battery lithium deposition location table
[0133]
[0134]
[0135] It can be understood that from the data in the above table, although the comparative example has a mass energy density and volume energy density that are basically equivalent to those of the embodiment in the initial stage, the lithium metal in the comparative example is easily deposited on the surface of the negative electrode, the capacity decays rapidly after the cycle, the battery volume expands greatly, and the volume energy density is lowest in the later stage of the cycle. The battery provided in the embodiment of the present application includes the current collector provided in the present application, so that the battery has a high energy density, a high charge and discharge capacity, is not easy to generate lithium dendrites, has a high safety performance, and a long cycle life.
[0136] This article uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above implementation methods is only used to help understand the core idea of the present application. At the same time, for general technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A current collector, It is characterized in that The current collector includes a first polymer layer, a metal foil layer and a second polymer layer stacked in sequence, and the current collector has a plurality of through holes penetrating two opposite surfaces of the current collector in the stacking direction; the current collector also includes a conductive layer, and the conductive layer is arranged on the inner side wall of the through hole. The thickness of the metal foil layer is less than or equal to 4μm, the thickness of the first polymer layer is 11μm-26μm, and the thickness of the second polymer layer is 11μm-26μm.
2. The current collector according to claim 1, It is characterized in that The plurality of through holes are distributed in an array, and the aperture of the through holes is less than or equal to 10 μm.
3. The current collector according to claim 1, It is characterized in that The current collector further includes a lithium-containing metal layer, which is disposed in the metal foil layer, and has a thickness of 10 nm to 2 μm.
4. The current collector according to claim 1, It is characterized in that The current collector further includes a flame retardant layer, which is disposed on a side of the first polymer layer away from the metal foil layer, and / or the flame retardant layer is disposed on a side of the second polymer layer away from the metal foil layer; the thickness of the flame retardant layer is 10 nm-1 μm.
5. The current collector according to claim 1, It is characterized in that The first polymer layer contains a lithium supplement material, the mass proportion of the lithium supplement material in the first polymer layer is 0.1wt%-5wt%, and the first polymer layer is insulated on a side away from the metal foil layer, and / or The second polymer layer contains a lithium supplement material, the mass proportion of the lithium supplement material in the second polymer layer is 0.1wt%-5wt%, and the side of the second polymer layer away from the metal foil layer is insulated. The lithium supplement material includes at least one of Li-Mg, Li-Al, Li-Si, Li-Ag, Li-Au, Li-Sn, Li-In and Li-Ge alloy.
6. A method for preparing a current collector, It is characterized in that include: The first polymer film, the metal foil film and the second polymer film are stacked in sequence to form a first composite structure; Disposing a first protective film on a surface of the first polymer film layer facing away from the metal foil film, and disposing a second protective film on a surface of the second polymer film layer facing away from the metal foil film, to form a second composite structure; forming a plurality of through holes on the second composite structure, wherein the through holes penetrate two opposite surfaces of the second composite structure in the stacking direction; forming a conductive layer on the inner side wall of the through hole; The first protective film and the second protective film are removed to obtain a current collector, the thickness of the metal foil layer is less than or equal to 4 μm, the thickness of the first polymer layer is 11 μm-26 μm, and the thickness of the second polymer layer is 11 μm-26 μm.
7. A negative electrode, It is characterized in that The negative electrode comprises a current collector prepared by the preparation method described in any one of claims 1 to 5 or claim 6.
8. An electrochemical energy storage device, It is characterized in that The electrochemical energy storage device comprises a positive electrode and the negative electrode according to claim 7.
9. The electrochemical energy storage device according to claim 8, It is characterized in that The porosity β of the current collector, the surface capacity C of the positive electrode, the thickness d of the current collector in the stacking direction and the capacity-thickness constant k satisfy the formula: The β≥50%, the C≥5mAh / cm 2 , k = 5 × 10 -4 cm 3 / mAh.