Catalyst shaped bodies with improved properties, their preparation and use
By designing a catalyst molded body with a trilobe structure and an outwardly curved arched top cover and bottom cover, the mechanical stability, filling density and heat exchange efficiency of the existing catalyst molded body in a fixed bed reactor is solved, and the problem of the mechanical stability, filling density and heat exchange efficiency of the existing catalyst molded body in a fixed bed reactor is achieved. Efficient catalytic conversion and low pressure drop effect.
Patent Information
- Application Number
- CN202180028592.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-26
- Filing Date
- 2021-05-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-05-17
AI Technical Summary
The existing catalyst molded bodies have problems such as insufficient mechanical stability, low filling density, poor diffusion performance, low heat exchange efficiency and high pressure drop in fixed bed reactors, especially in small-sized reactor tubes. Bed filling and efficient catalytic conversion.
A catalyst molded body with a trilobe structure is designed, including a top cover, a bottom cover and a side surface, three continuous substantially circular holes, and an outwardly curved arched top cover and bottom cover to ensure the catalyst molded body. The mechanical stability and high fill density are optimized while optimizing diffusion and heat exchange efficiency and reducing pressure drop.
High mechanical stability, low pressure drop, high filling density and efficient diffusion process are achieved, which improves the conversion and yield of the catalyst, reduces the wear and debris formation of the catalyst, and is suitable for gas-phase oxidation reactions in small-sized reactor tubes.
Smart Images

Figure GDA0004986916590000141 
Figure HDA0004986916600000011 
Figure HDA0004986916600000021
Abstract
Description
[0001] describe
[0002] The present invention relates to a catalyst shaped body for heterogeneous catalytic reaction of organic compounds in gas phase in a fixed bed reactor, which contains elements of Groups 3 to 12 of the periodic table and has a three-leaf structure, which has side surfaces around the blades, a top cover and a bottom cover, and three continuous holes extending from one cover side to the other cover side, wherein each hole is assigned to a blade, whereby the cover side is specially designed to have high mechanical stability, a low ratio of body volume to surface area, high diffusion path efficiency, high heat exchange efficiency, high packing density and low pressure drop at the same time.
[0003] Furthermore, the present invention also relates to a method for preparing the shaped catalyst body.
[0004] Additionally, the present invention relates to a reactor tube which is filled with the shaped catalyst body.
[0005] The present invention furthermore relates to a process for the heterogeneously catalyzed gas-phase oxidation of organic compounds in the presence of an oxygen-containing gas and the shaped catalyst body.
[0006] The shaped catalysts are used in particular for selective gas phase oxidations such as the oxidation of n-butane or benzene to maleic anhydride, the oxidation of propylene to acrolein, the oxidation of isobutene to methacrolein and for various other industrially important gas phase oxidations. Maleic anhydride is, for example, an important intermediate in the synthesis of gamma-butyrolactone, tetrahydrofuran and 1,4-butanediol (which in turn can be used as a solvent or as a precursor in the production of polytetrahydrofuran or polyvinylpyrrolidone).
[0007] The preparation of maleic anhydride by heterogeneously catalyzed gas phase oxidation of hydrocarbons is usually carried out using pelletized or extruded bulk catalysts based on vanadyl pyrophosphate (VO)2P2O7 (referred to as VPO catalysts). Various different geometries of such catalysts are described in the prior art, including pores, grooves, notches and serrations.
[0008] US 5,168,090 describes VPO catalysts of various shapes for the oxidation of n-butane to maleic anhydride which are believed to improve upon known catalyst systems such as tablets, pellets, spheres or spheroids, which is associated with reduced costs and increased yields of maleic anhydride. The US patents describe, inter alia, (a) a solid cylinder with or without a central continuous hole in the center and having a circular outer surface or an outer surface with circular or angular grooves extending from top to bottom, (b) a solid cylinder with a continuous angular spiral provided in the outer surface extending from top to bottom, (c) a solid cylinder with a central continuous hole and a continuous open groove between the outer surface and the central hole, (d) a square-based solid pyramid with circular grooves provided in the outer surface of the corner edges or inclined sides extending from the apex to the bottom, (e) a solid cone with circular grooves provided in the outer surface extending from the apex to the bottom, (f) a solid cube with angular grooves provided in the outer surface extending from top to bottom, (g) a solid cube with circular indentations provided in the four sides, top and bottom of the outer surface, and (h) a solid sphere with circular indentations provided in the outer surface. It is recognized that the indentations in the outer surface are important for achieving enhanced catalyst activity.
[0009] US 4,656,157 points out that cylinders, in particular hollow cylinders and annular bodies, have a lower pressure drop over the reactor cross section than spheres and also have lower wear resistance than spheres, which is disadvantageous in the end. Therefore, it is recommended to use hollow cylinders with convexly curved end faces instead of spheres, cylinders or hollow cylinders with flat end faces in gas phase oxidation reactions. Compared with flat end faces, convex end faces improve wear resistance and at the same time ensure low pressure drop and favorable catalytic activity.
[0010] US 2001 / 0,029,235 relates to the optimization of the pressure drop of shaped catalysts for heterogeneously catalyzed strongly exothermic gas phase reactions such as the oxychlorination of ethylene to 1,2-dichloroethane. It was found that hollow cylinders or annular tablets having end faces at the top and bottom, which are rounded at the outer edges and the edges of the central continuous hole, show a significantly lower pressure drop than hollow cylinders or annular tablets of the same size but whose end faces at the top and bottom are rounded only at the outer edges, i.e. convexly curved over the entire cross section (as taught in US 4,656,157).
[0011] In US2019 / 0,151,835, the effect of the end face shape of the hollow cylinder on the performance of the catalyst particles was further studied. The inventors found that an end face that rises gently from the peripheral edge to the center line can achieve a combination of low pressure drop with high catalytic conversion rate and high selectivity in the oxidation of acrolein to acrylic acid.
[0012] However, hollow cylinders or toroids with only a single central hole have limitations when aiming to combine low pressure drop and short intra-particle diffusion lengths (which would require thin walls) with high mechanical stability.
[0013] Another shape of a VPO catalyst for the oxidation of n-butane to maleic anhydride is disclosed in US2013 / 0,338,378. It describes a cylinder having four fillets and a wavy outer surface between the fillets along its cross section, a flat top side and bottom side, and at least one continuous hole extending from the top to the bottom. This geometry is described as having high mechanical stability and at the same time low density and short diffusion path. Compared with an annular body, the pressure drop of a packing containing particles having this shape is significantly reduced. It should be emphasized that the VPO catalyst having this shape shows improved performance over the classic annular body in the production of maleic anhydride.
[0014] WO 2019 / 156,953 adopts the concept of using vanadium phosphorus oxide in the form of a solid cylinder having circular grooves arranged in the outer surface extending from top to bottom and having a central continuous hole in the cylinder for partial oxidation of n-butane to maleic anhydride mentioned in US 5,168,090 and supplements the concept with other data on how to implement such catalysts. The publication shows that such cylinders are superior to corresponding cylinders without central continuous holes.
[0015] The catalyst shaped bodies described in US 2013 / 0,338,378 and WO 2019 / 156,953 can be seen as a further development of the hollow cylinders described in US 4,656,157, US 2001 / 0,029,235 and US 2019 / 0,151,835, but still show limitations in terms of combining high mechanical stability with low pressure drop and short intraparticle diffusion length as the goal.
[0016] US2011 / 0,257,413 discloses another progress of VPO catalyst for oxidation of n-butane to maleic anhydride. It describes a catalyst shaped body having a substantially cylindrical body of substantially circular cross section and having a longitudinal axis containing 2-5, preferably 4, internal continuous holes parallel to the axis of the cylinder, which are equidistant and symmetrical in cross section. In the case of a cylinder with four continuous holes, the center of the hole forms the corner of a regular square. Due to the inner hole, the catalyst shaped body has a large external surface area and shows a low pressure drop. In addition, it also shows satisfactory mechanical stability.
[0017] However, the disadvantage of the above-mentioned shape is that due to the wall thickness, the diffusion length is relatively uneven in the catalyst shape. There are 2-5 holes in the cylinder with a circular cross section, which essentially leads to weak points at each corner of the geometric shape, which can be drawn by connecting each hole. In the case where the catalyst shape is used for a relatively thin tube with an inner diameter of generally 20-35mm, such as in the case of a relatively thin tube with an inner diameter of generally 20-35mm used in many selective oxidation processes, the general challenge that also exists is to reduce the shape to a small size sufficient to achieve a reasonable uniform catalyst bed filling, which avoids excessive channeling (excessive channeling) or bypass of the reaction effluent. With the increasing complexity of the shape topology, such as with 4 continuous holes, this challenge is relatively serious. Another challenge related to the catalyst bed in the filling reactor tube and such tube is that, due to the flat top and bottom surfaces of the shape, particularly when the diameter of the shape is greater than its height, the stacking filling problem of several cylindrical catalyst shaped bodies with circumference and flat top.
[0018] US 5,330,958, US 5,326,915 and US 5,861,353 point out that the catalyst shapes described in the prior art generally show very limited diffusion properties, although the diffusion of reactant gases within the catalyst particles and the back-diffusion of reaction products outside the catalyst particles are a decisive feature of catalyst efficiency. In addition, it is emphasized that the catalyst used for gas phase exothermic reactions should also have a high surface area to volume ratio, good mechanical stability and low pressure drop on the reactor cross section. These patents teach that all these conditions, including enhanced diffusion properties, are achieved by using a catalyst shaped body with a cylindrical geometry containing three internal continuous holes, which are symmetrically arranged on the cross section of the cylinder, and the center forms an equilateral triangle. Regarding the outer side wall of the cylinder, these patents propose a three-leaf structure with a notch or a prismatic structure with a rounded vertex. It should be emphasized that these two shapes also show a high heat exchange coefficient, which is beneficial for high exothermic reactions. All three-leaf catalysts disclosed in these patents show that the spacing between two adjacent holes is less than the spacing between the continuous holes and the outer surface of the catalyst body. Irregular spacing can lead to uneven diffusion lengths and mechanical weak points.
[0019] The described catalyst body has incorporated several geometric features that enable improved performance relative to the prior art cited in the above paragraphs. However, there is no teaching as to which of the two alternative shapes is preferred. Nevertheless, another common problem with the described shapes is the problem of packing due to their flat top and bottom surfaces, as noted above for US2011 / 0,257,413.
[0020] Regarding the technical focus, US 5,330,958 and US 5,326,915 are concerned with the oxidation of methanol to formaldehyde, and US 5,861,535 is concerned with the oxychlorination of ethylene to 1,2-dichloroethane.
[0021] US2004 / 0,133,052 adopts the concepts mentioned in US 5,330,958, US 5,326,915 and US 5,861,535 and describes the use of a trilobate catalyst having three internal continuous pores for the hydrogenation of unsaturated hydrocarbons.
[0022] US2009 / 0,306,410 also adopts the concepts mentioned in US 5,330,958, US 5,326,915 and US 5,861,535 and describes the use of a trilobate VPO catalyst with three internal continuous pores and a prismatic VPO catalyst with a rounded vertex and three internal continuous pores for the oxidation of n-butane to maleic anhydride. Both catalyst bodies are rated as preferred embodiments, without giving priority to one of them. Both are described as having high mechanical stability, obtaining high maleic anhydride yields and having short diffusion paths, achieving high utilization of pores.
[0023] The disadvantage of the shapes specifically described by graphical reference in US2009 / 0,306,410 is that they have different wall thicknesses, because having a relatively large portion in the middle of the shaped body results in a relatively high transport restriction in this central portion of the catalyst shaped body. This may negatively affect the reaction performance. Different wall thicknesses within a single shape usually lead to weaker areas within the shape. In addition, these relatively unbalanced geometries may affect the powder feeding process during tableting, negatively affecting the mechanical stability or pore structure of the catalyst shaped body. In addition, the relatively large portion in the middle of the catalyst shaped body may provide a negative impact on the pressure drop along the catalyst packed bed. Finally, due to its flat top and bottom surfaces, there are also the usual problems of the shapes in terms of stacking and packing.
[0024] WO 2019 / 170,406 relates to the oxidation of sulfur dioxide to sulfur trioxide and describes a catalyst shaped body in the form of four leaves with four internal continuous holes (in which the center points form a regular square). This type of four-leaf body has a shape similar to a four-leaf clover. This geometry has a large external surface area relative to its body volume, is larger than the geometry with a substantially circular cross-section disclosed in US2011 / 0,257,413, and shows a low pressure drop on the reactor cross section. The specific discovery in WO2019 / 170,406 is that if the spacing between two adjacent continuous holes and those between the continuous holes and the outer surface of the catalyst body are substantially equal, the lateral compression strength of the wet, freshly extruded catalyst body and the calcined catalyst body is significantly higher than the catalyst body in which the spacing between two adjacent continuous holes is less than the spacing between the continuous holes and the outer surface of the catalyst body. In the process of manufacturing the catalyst by extrusion, high lateral compression strength is advantageous and also conducive to the disposal of the calcined catalyst body.
[0025] Even if the catalyst body has a four-leaf structure and substantially equal spacing between two adjacent continuous holes and between the continuous holes and the outer surface of the catalyst body, the body volume in the middle of the cross section of the four-leaf structure is still difficult to access and therefore only barely contributes to the catalytic reaction. This negatively affects the reaction performance. In addition, and similar to the disadvantages described for the catalyst shape disclosed in US2009 / 0,306,410, the relatively unbalanced geometry may affect the powder feeding process during the tableting process, negatively affecting the mechanical stability or pore structure of the catalyst molding. In addition, a relatively large portion in the middle of the catalyst molding may provide a negative impact on the pressure drop along the packed catalyst bed. Finally, in the case of using the catalyst shape in a relatively thin tube with an inner diameter of typically 20-35 mm, such as in a relatively thin tube with an inner diameter of typically 20-35 mm used in many selective oxidation processes, there is also a general challenge of reducing the shape to a small size sufficient to achieve a reasonable uniform catalyst bed filling, which avoids excessive channeling or bypassing of the reaction effluent.
[0026] PCT / EP2019 / 078,696 describes a silver-containing catalyst shaped body with a leaf-shaped geometry for the gas phase oxidation of ethylene to ethylene oxide, the catalyst body having a cylindrical structure with n folded spaces and n holes extending from one flat cover side to the other, wherein each hole is assigned to a leaf and n is 2, 3, 4, 5 or 6.
[0027] The prior art cited above shows that various shapes of catalyst bodies have been studied for heterogeneously catalyzed gas-phase oxidation of hydrocarbons and their influence on important properties and parameters has been demonstrated. It shows that for a given active substance, the shape of the catalyst body has a huge influence on: (a) the ratio of body volume to surface area; (b) mechanical stability such as lateral compression strength or wear resistance; (c) the length and efficiency of diffusion paths within the body volume; (d) the efficiency of heat exchange; and last but not least (e) the pressure drop over the reactor cross section during gas-phase reaction.
[0028] According to the present invention, it is recognized that changes in the shape of the catalyst body that positively affect one or more properties or parameters may negatively affect other properties or parameters. Although various improvements have been proposed in the prior art by adjusting the macroscopic texture of the catalyst body, there may still be some room for further improvement.
[0029] The object of the present invention is to provide a catalyst shaped body for the catalytic conversion of organic compounds in the gas phase in a fixed bed reactor, which no longer exhibits or only exhibits the above-mentioned disadvantages to a lesser extent, and which can have high conversion, high yield, high selectivity and long catalyst life. In particular, mechanical stability, packing density per reactor volume, efficiency of diffusion path in the bulk volume, packing density in a typical reactor tube and heat exchange efficiency of the catalyst shaped body should preferably be high, and the ratio of bulk volume to surface area, pressure drop over the reactor cross section during gas phase reaction, formation of fragments during handling of the catalyst and filling it into the reactor and its wear should preferably be low. In particular, an object of the present invention is to provide a catalyst shaped body for a catalyst bed in a relatively confined space such as a reactor tube with an inner diameter of 20-40 mm (such as is usually used for selective gas phase oxidation reactions). In addition, the catalyst shaped body should be easy to produce by using conventional methods and devices, except for minor adjustments.
[0030] Another object of the present invention is to provide a process for preparing the shaped catalyst bodies of the present invention.
[0031] Furthermore, it was an object of the present invention to provide a reactor tube filled with shaped catalyst bodies which are suitable for use in the conversion of organic compounds.
[0032] Finally, it is an object of the present invention to provide a process for producing oxidized organic compounds in high yield and with high selectivity by heterogeneously catalyzed gas-phase oxidation of organic compounds, for example acrolein or acrylic acid from propylene or maleic anhydride from n-butane.
[0033] Surprisingly, a shaped catalyst body has been found for heterogeneously catalyzed reactions of organic compounds in the gas phase in a fixed bed reactor, wherein the shaped catalyst body is characterized in that:
[0034] (a) contains at least one element from Groups 3 to 12 of the Periodic Table of Elements, wherein the total amount of elements from Groups 3 to 12 of the Periodic Table of Elements is 0.01 to 85% by weight;
[0035] (b) A cylindrical structure having a top cover (A), a bottom cover (B) and a side surface (C) having three notches extending in the periphery of the cylinder along the height of the cylinder, forming a trilobal structure;
[0036] (c) three continuous substantially circular holes extending from one cover side to the other cover side as void spaces, having a diameter d1 and a tolerance of d1 of each hole of 15% based on the shortest diameter of the corresponding hole, wherein each hole is assigned to a blade and wherein the center points of the three holes are arranged substantially equidistantly in a horizontal cross section of the cylindrical structure with a tolerance of 15% based on the shortest distance between two center points of two holes;
[0037] in
[0038] (d) the wall thickness d2 between two consecutive holes at the imaginary connecting line between the center points of the two consecutive holes on the horizontal cross-section of the cylindrical structure is substantially the same for all three walls between the two consecutive holes, wherein the tolerance of d2 is 15% based on the shortest wall thickness;
[0039] (e) for each of the three blades, the wall thickness d3 between the continuous hole and the side surface within a 180° section (defined as the section on the horizontal cross section of the cylindrical structure, the chord of which is parallel to the imaginary connecting line between the two center points of two adjacent continuous holes) is substantially constant within the corresponding section and substantially the same for all three sections of the three blades, wherein the tolerance of d3 is 15% based on the shortest wall thickness;
[0040] (f) Each of the three wall thicknesses d2 and the three wall thicknesses d 3x The ratio of each of them is 0.9-1.1, where d 3x is the wall thickness on a horizontal section of the cylindrical structure located at the extension of an imaginary connecting line between the center point of the cylinder and the center points of the consecutive holes of the corresponding blade;
[0041] (g) The top cover (A) and the bottom cover (B) have an outwardly curved arched body having a maximum height h2 for the top cover (A) and a maximum height h3 for the bottom cover (B), wherein
[0042] h2 is the distance between:
[0043] - an imaginary planar top cover area of an imaginary circular cylinder (D) comprising a circular side surface, which circular side surface just surrounds the three vanes of the shaped catalyst body, whereby the imaginary planar top cover area contacts the circular side surface at a right angle at the highest level at which the circular side surface of the imaginary circular cylinder (D) just contacts at least one vane; and
[0044] - the highest height of the tectum (A) above the imaginary plane tectum area, measured perpendicular to the imaginary plane tectum area;
[0045] h3 is the distance between:
[0046] - an imaginary flat bottom cover region of an imaginary circular cylinder (D) comprising a circular side surface, which circular side surface just surrounds the three vanes of the shaped catalyst body, whereby the imaginary flat bottom cover region contacts the circular side surface at a right angle at the lowest horizontal position where the circular side surface of the imaginary circular cylinder (D) just contacts at least one vane; and
[0047] - the maximum height of the base cap (B) above the imaginary plane base cap area, measured perpendicular to the imaginary plane base cap area; and
[0048] The imaginary circular cylinder (D) has a height h1 measured as the distance between an imaginary planar top cover region and an imaginary planar bottom cover region; and
[0049] (h) The diameter d1 is independently 1-5 mm, the wall thicknesses d2 and d3 are independently 0.5-3 mm, the heights h2 and h3 are independently 0.2-3 mm, and the height h1 is 2-10 mm.
[0050] The shaped catalyst body is characterized by its material as defined by feature (a) and by its particular geometry as defined by features (b) to (h).
[0051] According to feature (a), the catalyst body of the present invention contains at least one element from Groups 3 to 12 of the Periodic Table of Elements, wherein the total amount of elements from Groups 3 to 12 of the Periodic Table of Elements is 0.01 to 85% by weight. These elements can exist in various chemical forms, including metallic forms and ionic forms. Metallic forms are, for example, metals including alloys, and ionic forms are, for example, oxides and any other salts. Preferably, these elements include at least one element of Sc, Y, La, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Re, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag and Zn, more preferably at least one element of Zr, V, Nb, Mo, W, Fe, Co, Ni, Pd, Pt, Cu, Ag and Zn, particularly preferably at least one element of V, Nb, Mo, Fe, Co, Ni, Pd, Pt, Cu, Ag and Zn.
[0052] In addition to the elements of the 3rd to 12th groups of the periodic table, other elements are present and the percentage of the composition reaches 100%. Basically, these are elements from the 1st to 2nd groups and the 13th to 17th groups of the periodic table, such as H, Na, K, Mg, Ca, Ba, B, Al, C, Si, Sn, N, P, Ge, Sb, Bi, O, S or Cl. For example, these can be part of the catalytically active main component, such as phosphorus in VPO catalysts or chlorine in CuCl2 catalysts, can be promoters, such as bismuth, or can be part of the carrier material, such as Al of Al2O3 carriers or Si of SiO2 carriers. In addition, alkali metals and alkaline earth metals can also be present. Finally, lubricants such as graphite can also be present. Other lubricants can also be Cu powder, whereby Cu is already an element of the 11th group of the periodic table. The lubricant supports the tableting of the catalyst molding.
[0053] Depending on its composition and structure, the catalyst shaped body of the present invention can be widely used to catalyze various different reactions of various organic compounds. For example, the catalyst shaped body can be a supported catalyst, in which the catalytically active components are impregnated or otherwise deposited on a support material, a full body catalyst, which is more or less completely made of catalytically active components, or any type in between. Possible support materials for supported catalysts can be any support material, which can be formed into a desired shape and which can be used as a support material for the catalyst. Typical support materials are, for example, Al2O3, SiO2, MgO, TiO2 or ZrO2, but other support materials can also be used.
[0054] Without limiting the scope, the following list contains some catalytically active materials which are usually used as main components for certain reactions of organic compounds. Possible promoters and adjuvants such as lubricants are intended to be omitted from the following list, but should not be excluded.
[0055] - Noble metals such as Pt or Pd on support materials such as Al2O3 (for example for the hydrogenation of unsaturated hydrocarbons).
[0056] - Ag on a support material such as Al2O3 (eg for the oxidation of ethylene to ethylene oxide).
[0057] - CuCl2 on support materials such as Al2O3 (eg for the oxychlorination of hydrocarbons).
[0058] -(VO)2P2O7 (for example, for the oxidation of n-butane to maleic anhydride).
[0059] -V-Mo-oxide (for example for the oxidation of benzene to maleic anhydride).
[0060] - mixed metal oxides containing at least Mo, Fe and Bi, CoMoO4, Fe2(MoO4)3 or Bi-Mo oxides (for example for the oxidation of propene to acrolein or of isobutene to methacrolein).
[0061] - Co—Mo oxide or Mo—V oxide (for example for the oxidation of acrolein to acrylic acid or of methacrolein to methacrylic acid).
[0062] - Ag on a support material such as Al2O3 (eg for the oxidation of methanol to formaldehyde).
[0063] - Fe-Mo-V-oxide (for example for the oxidation of methanol to formaldehyde).
[0064] - V2O3 (for example for the oxidation of sulfur dioxide to sulfur trioxide).
[0065] Catalysts in which Pt or Pd are the main catalytically active components preferably contain only 0.01-1% by weight, more preferably ≥0.02% by weight, particularly preferably ≥0.05% by weight, and more preferably ≤0.8% by weight, particularly preferably ≤0.5% by weight of these metals. They are preferably supported catalysts, in which the noble metal is impregnated on a support material. Preferred support materials are Al2O3 and alumina-based materials. However, other support materials such as those known in the prior art can also be used in general.
[0066] Independently of the above-mentioned catalysts in which noble metals such as Pt or Pd are the main catalytically active components and are characterized by a low Pt and Pd content, preference is given to catalyst shaped bodies which preferably contain ≥1% by weight, more preferably ≥5% by weight, particularly preferably ≥10% by weight, and preferably ≤80% by weight, more preferably ≤75% by weight, of the total amount of elements of Groups 3 to 12 of the Periodic Table of the Elements.
[0067] Catalysts in which base metals other than Pt or Pd such as Cu or Ag are the main catalytically active components and catalysts in which one or more elements of the periodic table of elements Group 3-12 are present in the form of ions other than oxides are also preferably supported catalysts, in which the active compound is impregnated or otherwise deposited on a support material. As an example, Ag on Al2O3 and CuCl2 on Al2O3 are mentioned. In addition to Al2O3, other support materials such as those known in the prior art can also be used generally. The total amount of elements of the periodic table of elements Group 3-12 used for such catalysts is preferably ≥1% by weight, more preferably ≥5% by weight, particularly preferably ≥10% by weight, and preferably ≤50% by weight, more preferably ≤40% by weight, particularly preferably ≤30% by weight. The supported catalyst may also contain a promoter, a lubricant and any other auxiliary agent. As a possible example related to the above-mentioned catalyst containing CuCl2, it is mentioned that in addition to CuCl2, KCl is also present in the oxychlorination catalyst.
[0068] Another important catalyst group that the catalyst shaped body of the present invention has special significance is the complete catalyst group, wherein the catalyst shaped body is more or less completely made of catalytically active components. Such complete catalysts mainly contain one or more oxidized forms of the periodic table of elements Group 3-12. The term oxidized form also includes mixed oxides with other metals and non-metallic compounds such as P. The total amount of one or more periodic table of elements Group 3-12 of such catalysts is preferably ≥10 weight %, more preferably ≥20 weight %, particularly preferably ≥25 weight %, and preferably ≤80 weight %, more preferably ≤75 weight %. As the periodic table of elements Group 3-12, preferred V, Nb, Mo, Fe, Co, Ni and Zn. The complete catalyst can also contain a promoter, a lubricant and any other auxiliary agent.
[0069] Particularly preferably, the shaped catalyst bodies of the invention contain an oxidic material comprising vanadium and phosphorus, very particularly preferably vanadyl pyrophosphate.
[0070] With respect to the material of the shaped catalyst body, its volume is expressed as "bulk volume" and its density is expressed as "bulk density". More specifically, the "bulk volume" is defined as the macroscopic volume including the pores. For the sake of completeness, it should be emphasized that continuous substantially circular pores as defined in feature (c) and any surface structures such as grooves, notches or serrations are not part of the macroscopic volume. Similarly, the "bulk density" is defined as the ratio between the mass of the particle and its bulk volume.
[0071] Regardless of whether it is a supported catalyst, a complete catalyst or anything in between, and regardless of whether it contains the active components in metallic form or in ionic form such as oxides or any other salts, the material from which the shaped catalyst bodies are made generally has a relative humidity of 1 to 15 g / cm 3, preferably ≥1g / cm 3 And preferably ≤10g / cm 3 , more preferably ≤8g / cm 3 , especially preferably ≤5g / cm 3 The body volume.
[0072] The geometry of the shaped catalyst body is defined by features (b) to (h). Figure 1 For illustrative purposes, a block diagram of a possible embodiment of a shaped catalyst body according to the invention is shown. It shows a horizontal overall section in view a) and a vertical overall section in view b). The bold lines represent the outer shape, while the dashed lines are reference lines. These designations correspond to the nomenclature in the claims. Capital letters refer to surfaces and lower case letters refer to spacings and dimensions.
[0073] The basic shape of the catalyst body defined by feature (b) is a cylindrical structure having a top cover (A), a bottom cover (B) and a side surface (C) having three notches extending in the periphery of the cylinder along the height of the cylinder, forming a trilobal structure. Figure 1 In the horizontal section shown in a), the trilobal structure with three notches is easily visible. The three notches appear as three V-shaped notches.
[0074] In addition to the cylindrical structure and as defined in feature (c), the shaped catalyst body contains as void spaces three continuous substantially circular holes extending from one cover side to the other cover side, having a diameter d1 and a tolerance of d1 of each hole of 15% based on the shortest diameter of the corresponding hole, wherein each hole is assigned to a blade and wherein the center points of the three holes are arranged substantially equidistantly on a horizontal cross section of the cylindrical structure with a tolerance of 15% based on the shortest distance between two center points of two holes. Figure 1 In a), the center point of each hole is represented by a small dot and the diameter d1 of a hole is exemplarily shown by a double arrow.
[0075] Continuous means that each hole has two openings and a substantially straight passage between the two openings. The three holes are oriented so that they extend in a vertical direction from one cover side to the other cover side of the cylinder. The holes are substantially parallel to the side surface (C).
[0076] The horizontal total cross section of each hole is substantially circular. The term "substantially circular" includes a precise circular geometry and deviations from a precise circular geometry, such as a slightly elliptical geometry, a slight cone in the vertical direction, or a regular or irregular geometry with saw teeth, notches or grooves, etc., wherein the tolerance of the diameter d1 of each hole is 15% based on the shortest diameter of the corresponding hole. The shortest diameter of the hole refers to the shortest straight line distance across the center point of the corresponding hole. The tolerance is preferably 10%, more preferably 8%, particularly preferably 5%, and very particularly preferably 3% based on the shortest diameter of the corresponding hole. The slightly conical form of the hole reduces the push-out force generated by the pressing tool on the pressed tablet after the catalyst shaped body is compacted in the tablet press and thus enables a more favorable preparation process.
[0077] The diameter d1 of a hole is the average of the diameters across the vertical extension of the corresponding hole, while the diameter at the horizontal general section is the average of the straight-line distances across the center point of the horizontal general section. In the case of a perfectly circular hole, the diameter of each horizontal general section and the diameter across the vertical extension of the hole are the same, so that the diameter d1 is equal to the diameter measured at the opening.
[0078] The three consecutive substantially circular holes are positioned such that each hole is assigned to one leaf of the trilobal structure and the center points of the three holes are arranged substantially equidistantly in a horizontal section of the cylindrical structure with a tolerance of 15% based on the shortest distance between the two center points of two holes. Thus, the center points of the three holes are located at the corners of a substantially equilateral triangle. The tolerance means that one or two of the three distances between two center points can be up to 15% longer than the shortest distance between two center points in the triangular arrangement. The tolerance is preferably 10%, more preferably 8%, particularly preferably 5%, very particularly preferably 3% based on the shortest distance.
[0079] An important feature of the catalyst shaped body of the present invention is feature (d), which relates to the wall thickness d2 between two consecutive holes. According to this feature, the wall thickness d2 between two consecutive holes at the imaginary connecting line between the center points of the two consecutive holes on the horizontal cross section of the cylindrical structure is substantially the same for all three walls between the two consecutive holes, wherein the tolerance of d2 is 15% based on the shortest wall thickness. The wall thickness d2 between two consecutive holes is the average value of the wall thickness across the vertical extension of the corresponding hole. For illustration purposes, Figure 1 In a), the wall thickness d2 of the wall between two holes and the dashed connecting line between the center points of the two holes are shown by way of example.
[0080] The term "substantially the same" includes completely identical wall thicknesses as well as two or three different wall thicknesses. The tolerance of each wall thickness d2 is 15%, preferably 10%, more preferably 8%, particularly preferably 5%, very particularly preferably 3%, based on the shortest wall thickness.
[0081] Another important feature of the catalyst molded body of the present invention is feature (e), which relates to the wall thickness d3 between the continuous hole and the side surface. According to this feature, for each of the three blades, the wall thickness d3 between the continuous hole and the side surface is substantially constant within the corresponding portion within a 180° portion (defined as a portion on a horizontal cross-section of a cylindrical structure whose chord is parallel to the imaginary connecting line between the two center points of two adjacent continuous holes) and is substantially the same for all three portions of the three blades, wherein the tolerance of d3 is 15% based on the shortest wall thickness. The wall thickness d3 between the continuous hole and the side surface is the average value of the wall thickness across the vertically extending portion and within the 180° portion of the corresponding hole. For illustrative purposes, Figure 1 a) shows a reference line representing the 180° portion, a dashed connecting line between two center points of two adjacent continuous holes (the 180° portion reference line is parallel thereto) and a double arrow representing the wall thickness d3 within the 180° portion. Figure 1 A specific wall thickness within the 180° portion in a) is denoted as d 3x , which is also part of d3, but in a specific geometric position. 3x With feature (f).
[0082] The terms "substantially constant" and "substantially the same" include exactly equal wall thicknesses as well as different wall thicknesses within the tolerance range. The tolerance for each wall thickness d3 is 15%, preferably 10%, more preferably 8%, particularly preferably 5%, very particularly preferably 3%, based on the shortest wall thickness.
[0083] Another important feature of the catalyst shaped body according to the invention is feature (f), which relates to the wall thickness d2 and the wall thickness d 3x The ratio of the wall thickness d 3x is the wall thickness on a horizontal section of the cylindrical structure located at the extension of the imaginary connecting line between the center point of the cylinder and the center point of the continuous hole of the corresponding blade. According to feature (f), the wall thickness d2 is equal to the wall thickness d 3x The ratio is 0.9 to 1.1. One of the three wall thicknesses d2 and the three wall thicknesses d 3x An example of this is shown in Figure 1 a). This ratio involves all nine possible ratios d2 / d 3x , because there are three wall thicknesses d2 and three wall thicknesses d 3x .
[0084] Ratio d2 / d 3x It is preferably ≥0.95, more preferably ≥0.98, particularly preferably ≥0.99, and preferably ≤1.05, more preferably ≤1.02, particularly preferably ≤1.01, and in particular 1.
[0085] The above features (b) to (f) define the geometry of the catalyst body across a horizontal cross section by specifying its trilobal structure, the diameter d1 of the continuous substantially circular holes, and the wall thicknesses d2 and d3. By these data, the geometry across a horizontal cross section is clearly and completely defined. However, one other practical horizontal dimension is the outer diameter d0. The outer diameter d0 is the diameter of the smallest circle that just surrounds the catalyst body in a horizontal cross section. Figure 1 a) also shows the surrounding circle as a dotted circle around the three blades. Its diameter is denoted by d0.
[0086] In the case of an exact equilateral triangle with three hole center points, equal d1 values, equal d2 values and equal d3 values, the outer diameter d0 can be easily calculated by the following formula:
[0087]
[0088] Surprisingly, it was found that, based on geometric features (b) to (f), the dome-shaped bodies that are bent outward at the top cover (A) and the bottom cover (B) can have high mechanical stability, efficient diffusion paths within the body volume, high packing density within a typical reactor tube, efficient heat exchange between the body and its adjacent areas, as well as a low ratio of body volume to surface area, low pressure drop over the reactor cross section during gas phase reactions and low wear in the same catalyst shaped body.
[0089] Thus, basic feature (g) relates to a top cover (A) and a bottom cover (B) having an outwardly curved arch having a maximum height h2 for the top cover (A) and a maximum height h3 for the bottom cover (B), wherein
[0090] h2 is the distance between:
[0091] - an imaginary planar top cover area of an imaginary circular cylinder (D) comprising a circular side surface, which circular side surface just surrounds the three vanes of the shaped catalyst body, whereby the imaginary planar top cover area contacts the circular side surface at a right angle at the highest level at which the circular side surface of the imaginary circular cylinder (D) just contacts at least one vane; and
[0092] - the highest height of the tectum (A) above the imaginary plane tectum area, measured perpendicular to the imaginary plane tectum area;
[0093] h3 is the distance between:
[0094] - an imaginary flat bottom cover region of an imaginary circular cylinder (D) comprising a circular side surface, which circular side surface just surrounds the three vanes of the shaped catalyst body, whereby the imaginary flat bottom cover region contacts the circular side surface at a right angle at the lowest horizontal position where the circular side surface of the imaginary circular cylinder (D) just contacts at least one vane; and
[0095] - the maximum height of the base cap (B) above the imaginary plane base cap area, measured perpendicular to the imaginary plane base cap area; and
[0096] The imaginary circular cylinder (D) has a height h1 measured as the distance between an imaginary planar top cover region and an imaginary planar bottom cover region.
[0097] Figure 1 b) shows a vertical section through a shaped catalyst body according to the invention. Figure 1 1). The same trefoil structure as shown in a). Again, the bold lines represent the outer shape, while the dashed lines are reference lines. It illustrates how the outwardly curved arched bodies of the top cover (A) and bottom cover (B) may look. In addition, the imaginary circular cylinder (D) shown in dashed lines also illustrates the imaginary planar top and bottom cover areas represented by horizontal dashed lines, the upper and lower edges of the height h1. The heights h2 and h3 are shown above and below the imaginary planar top and bottom cover areas with dashed arrows.
[0098] Similar to the outer diameter d0 being a practical dimension, the overall height h0 is also a practical dimension because it can also be easily measured. It is the sum of h1, h2 and h3 as shown below:
[0099] h0=h1+h2+h3 (2).
[0100] The outwardly curved arched bodies of the catalyst molding of the present invention can have different geometric shapes. The common feature of these outwardly curved arched bodies is their arched body shape. For example, the arched body shape can have a continuous arc shape on the corresponding cover, or be divided into independent arcs on different walls of the three-leaf structure. Although it is possible for the top cover (A) and the bottom cover (B) to have outwardly curved arched bodies with different shapes, it is preferred that the two covers have at least more or less, particularly substantially the same shape.
[0101] In a preferred embodiment of the shaped catalyst body, at least one of the two outwardly curved arches has a convex shape on the corresponding cover, more preferably the two outwardly curved arches have a convex shape on the corresponding cover. Convex means that the corresponding arch has the shape of a chord. The diameter of the circle from which the chord is obtained is defined by the height of the corresponding cover, which means that it is defined by h2 of the top cover (A) and h2 of the bottom cover (B). Figure 2 a) A vertical cross section of the convexly shaped cover is shown as a schematic example.
[0102] In another preferred embodiment of the shaped catalyst body, at least one of the two outwardly curved arches has a compressed convex shape on the corresponding cover, and more preferably both outwardly curved arches have a compressed convex shape on the corresponding cover. Compressed convex means that the basic shape is a convex shape that is compressed in the vertical direction.
[0103] Similar to the compressed convex shape, the convex shape can also be stretched. Therefore, in another preferred embodiment of the catalyst shaped body, at least one of the two outwardly curved arches has a stretched convex shape on the corresponding cover, and more preferably both outwardly curved arches have a stretched convex shape on the corresponding cover. The stretched convex shape means that the basic shape is a convex shape stretched in the vertical direction.
[0104] The convex shape of the cover or a shape based on the convex shape is only one possible basic form of a continuous arc on the corresponding cover. In another preferred embodiment of the catalyst shaped body, at least one of the two outwardly curved arches has the shape of a compressed semicircle on the corresponding cover, and more preferably both outwardly curved arches have the shape of a compressed semicircle on the corresponding cover. Compressed semicircle means that the basic shape is a semicircle with a diameter d0, which is compressed in the vertical direction. Figure 2 b) A vertical cross section of the compressed semicircular shaped cover is shown as a schematic example.
[0105] Figure 2 a) and b) also show the internal angle α at the edge where the side surface of the imaginary circular cylinder (D) contacts the outwardly curved arch. It can be easily determined by measuring the external angle β at the edge where the side surface of the imaginary circular cylinder (D) contacts the outwardly curved arch, which is a complementary angle to α and from which α can be easily calculated according to the following formula:
[0106] α=360°-β (3).
[0107] The angle α is >90° and is usually ≤180°. It is preferably ≥100°, more preferably ≥110°, particularly preferably ≥120°, and preferably ≤170°, more preferably ≤160°. Particularly preferred are shaped catalyst bodies in which the inner angle α at the edge where the side surface of the imaginary circular cylinder (D) contacts the outwardly curved arched body of the top cover (A) and the outwardly curved arched body of the bottom cover (B) is independently 120 to 160°.
[0108] As already mentioned above, the outwardly curved arches can also be divided into separate arcs on different walls of the trefoil structure, for example. In one embodiment of this type, at least one of the two outwardly curved arches is divided in such a way that each dividing wall between the hole and the outer surface and between the two holes is rounded at both edges. The rounded dividing walls can have different geometric shapes. In one embodiment, for example, they can have Figure 3 a) or a compressed or stretched convex shape, or in another embodiment, for example, it may have a convex shape as shown in Figure 3 b), or in another embodiment, it may also have a semicircular shape as shown in Figure 3 c) The shape of a compressed semicircle shown. Of course, the aforementioned shapes are non-limiting examples.
[0109] In addition to the shape of the circular partition wall, the arc of the circular partition wall can also have different geometric shapes. For example, it can have Figure 3 a) and 3c), a convex shape as shown in compression or tension, or a convex shape as shown in Figure 3 b) A compressed semicircle as shown. The aforementioned shapes are also only non-limiting examples.
[0110] In the case of this division into individual arcs, usually both covers of the shaped catalyst body are divided in the same way.
[0111] Furthermore, it may be advantageous to have some offset between the edge where the outwardly curved arch and the vertical periphery of the trefoil structure meet the cover side in the production of the shaped catalyst body. In the case of this offset, the outwardly curved arch does not directly contact the vertical periphery of the trefoil structure, but is slightly recessed and there is a flat peripheral area between the outwardly curved arch and the edge where the vertical periphery of the trefoil structure meets the cover side. This offset may also be present between the outwardly curved arch and the edge where the substantially circular hole meets the cover side.
[0112] If the catalyst body according to the invention contains an outwardly curved arch or an offset towards the vertical periphery of the trilobal structure or towards the essentially circular hole or towards both, the width of the flat surrounding area is preferably ≤ (0.2 x d2), more preferably ≤ (0.1 x d2). If there is no offset, then of course there is no flat surrounding area and its width has the value 0 x d2.
[0113] Besides the material properties of which the shaped catalyst bodies are at least partially made, and besides the geometric shape of the shaped catalyst bodies, the shaped catalyst bodies according to the invention are also characterized by their dimensions. Characteristic (h) relates to the dimensions d1, d2, d3 and h1, h2, h3.
[0114] The diameter d1 is independently of one another in the range from 1 to 5 mm, preferably ≥1.5 mm, more preferably ≥1.8 mm, particularly preferably ≥2 mm, and preferably ≤4 mm, more preferably ≤3 mm.
[0115] The wall thicknesses d2 and d3 are independently of one another 0.5 to 3 mm, preferably ≥0.8 mm, more preferably ≥0.9 mm, particularly preferably ≥1 mm, and preferably ≤2.5 mm, more preferably ≤2 mm and particularly preferably ≤1.8 mm.
[0116] Thus, the outer diameter d0, ie the diameter of the smallest circle which surrounds the shaped catalyst body in horizontal section, is 3.7 to 20 mm, preferably ≥4 mm, more preferably ≥5 mm, and preferably ≤15 mm, more preferably ≤12 mm, particularly preferably ≤10 mm.
[0117] The heights h2 and h3 are independently from one another in the range of 0.2 to 3 mm, preferably ≥0.3 mm, more preferably ≥0.4 mm, and preferably ≤2.5 mm, more preferably ≤2 mm, particularly preferably ≤1.5 mm.
[0118] The height h1 is 2 to 10 mm, preferably ≥3 mm, more preferably ≥4 mm, and preferably ≤9 mm, more preferably ≤8 mm, particularly preferably ≤7 mm.
[0119] Therefore, the total height h0, ie the sum of d1, d2 and d3, is 2.4 to 16 mm, preferably ≥3 mm, more preferably ≥4 mm, particularly preferably ≥5 mm, and preferably ≤15 mm, more preferably ≤12 mm, particularly preferably ≤10 mm.
[0120] Particular preference is given to shaped catalyst bodies having an outer diameter d0 of 5 to 15 mm and an overall height h0 of 4 to 12 mm.
[0121] As described in feature (b), the side surface (C) has three notches extending in the periphery of the cylinder along the height of the cylinder, forming a trilobal structure. The simplest geometry of these notches is shown in Figure 1 a). It has the form of a V-shaped notch with a vertical centerline located at the intersection of two adjacent circles, forming a leaf-shaped structure. The V-shaped notch can have an efficient diffusion path and efficient heat exchange even at the intersection of two adjacent circles of the leaf-shaped structure.
[0122] Although this V-shaped recess has shown various advantages, it has surprisingly been found that a slight flattening of the V-shape at the intersection significantly improves the mechanical stability of the catalyst shaped body, while the diffusion performance, heat exchange and the ratio of bulk volume to surface area are only insignificantly reduced. Based on the above findings, preference is given to catalyst shaped bodies in which the inner area of the recess at the side surface between two adjacent blades (defined as the area between imaginary vertical lines and where the chord of the imaginary 180° section as specified in feature (e) intersects the side surface of the blade) is at least partially filled with oxidic material as specified in feature (a).
[0123] Figure 4 a) shows a horizontal cross section of a shaped catalyst body as an example of this embodiment. In this embodiment, the inner area of the notch between the imaginary vertical lines (where the chord of the imaginary 180° section intersects the side surface of the blade) is filled and a uniform side surface is shown in the inner area. Figure 4 In the horizontal cross section shown in a), these fillers are represented by the straight line between two adjacent points where the imaginary 180° section intersects the side surface.
[0124] In another and more preferred embodiment, the filling of the recess at the side surface has a concave shape. A horizontal section of the catalyst shaped body is shown in Figure 4 b) The transition between the rounded portion of the respective blade and the concave rounded portion of the filler is preferably smooth, more preferably forms a wavy line.
[0125] It is explicitly mentioned that the shape of the filler of the V-shaped notch is not limited to the above-mentioned shapes and other shapes that deviate from the straight line and the concave circular portion can also be adopted. Without limitation, such shapes include compressed or stretched circular portions and any other shapes. In addition, it is explicitly mentioned that the filler also only covers a part of the surface of the inner area. For illustration purposes, Figure 4 c) shows an example of an embodiment, wherein only a small part of the surface of the inner area is covered with the filling.
[0126] Figure 5 Three different views of a preferred shape of a shaped catalyst body of the present invention are shown. It contains two convex shaped caps and three concave shaped fillers of recesses located at the side surface between each adjacent vane. Figure 5 a) is an oblique view of the flat catalyst body, Figure 5 b) is a slightly oblique view of an upright catalyst body, and Figure 5 c) is a view of the lid in a more or less upright position.
[0127] The catalyst shaped bodies of the present invention combine various very advantageous physical properties in the same shaped body and are therefore significantly different from known shaped bodies. The basic physical properties are as follows:
[0128] - High mechanical stability.
[0129] Due to its three-lobed shape and despite the presence of three essentially circular holes, the catalyst molded body of the present invention has a very high mechanical stability, in particular compared to annular bodies of the same material. The symmetrically arranged blades with their combined walls in the central region significantly enhance the mechanical stability. This is indicated by a high side crushing strength and leads to the formation of significantly less fragments during the handling of the catalyst and during its filling into the reactor, in particular compared to annular bodies of the same material. Since a large part of the surface is protected as the surface of the three essentially circular holes or as the surface of the three recesses at the outer surface at the contact area of two adjacent blades, and due to the outwardly curved arched body, sharp angles are generally avoided, the catalyst molded body of the present invention is also characterized by low wear, in particular compared to annular bodies of the same material, and compared to three-lobed bodies of the same material with flat cover sides. However, the mechanical stability of the catalyst molded body of the present invention is roughly comparable to the three-lobed bodies of the prior art with flat cover sides.
[0130] The mechanical stability of the shaped catalyst bodies according to the invention can be further increased by partially filling the recesses in the side surface between two adjacent blades.
[0131] - Low bulk volume to surface area ratio.
[0132] The low bulk volume to surface area ratio (which can also be expressed as characteristic length) means that the catalyst shaped body has a large surface area compared to its bulk volume. The surface area is the contact area between the reaction fluid and the catalyst. The larger the surface area, the higher the transfer of the educts from the reaction fluid to the catalyst body and the product back to the reaction fluid. Due to its geometric shape, the catalyst shaped body of the present invention has a low bulk volume to surface area ratio. Compared with the trilobes of the prior art of similar size with flat cover sides, the arched body that bends outward at the two covers even reduces the above ratio. Therefore, the catalyst shaped body of the present invention is slightly better than the trilobes of the prior art mentioned above.
[0133] Partially filling the recess at the side surface between two adjacent blades only slightly increases the body volume to surface area ratio, which is ultimately not detrimental.
[0134] -Efficient diffusion process.
[0135] In addition to a large accessible surface area, it is also important that a large part of the catalytically active substances is easily accessible and that as little substance as possible is inaccessible. The disadvantage of inaccessible substances is that they bind to the catalytically active substances and increase the weight of the catalyst shaped body without significantly promoting the reaction. Due to the special geometry, the catalyst shaped body according to the invention exhibits the same or almost the same wall thicknesses d2 and d3 almost everywhere in its horizontal section and is therefore easily accessible. Only small areas at the three recesses of the outer surface at the contact area of two adjacent blades and the area around the center of the trilobite are slightly less accessible. In this respect, the catalyst shaped body according to the invention is roughly comparable to a trilobite of similar dimensions of the prior art with a flat cover side.
[0136] Partially filling the recess at the side surface between two adjacent blades has only a slight effect on the efficiency of the diffusion path, wherein the very small amount of active material around the recess of the outer surface at the triangular area between the two holes of two adjacent blades and the contact area of two adjacent blades is slightly less accessible.
[0137] - Efficient heat exchange.
[0138] Especially for highly exothermic reactions, high heat exchange efficiency is very important. It is achieved by the interaction of high surface area relative to the bulk volume and efficient diffusion paths. These two criteria enable the reaction heat to be quickly removed from the catalyst shaped body so that it is carried away by the reaction fluid. Due to the slightly favorable bulk volume to surface area ratio of the catalyst shaped body of the present invention, it also shows a slight advantage in the efficiency of heat exchange over the prior art trilobes of similar size with flat cover sides.
[0139] -High packing density.
[0140] In addition, the catalyst shaped body of the present invention is characterized by a high packing density. The high packing density can provide a large amount of catalytically active material per reactor volume and thus enable the use of a smaller reactor. However, the packing density of the catalyst shaped body of the present invention is significantly less than the packing density of a comparable annular body, but such annular bodies show a huge pressure drop as shown in the following figure. Compared with the trilobes of the prior art of similar size with flat cover sides, the catalyst shaped body of the present invention shows a significantly higher packing density due to the outwardly curved arched body at the two covers. This is a huge advantage.
[0141] -Low pressure drop.
[0142] Compared to the high packing density of the catalyst shaped body according to the invention, it surprisingly has a low pressure drop over the reactor cross section during the gas phase reaction. This is due to its special geometry. The three-lobed structure with three essentially circular holes enables a good flow of the reaction fluid through the catalyst bed. The pressure drop of the packing of the catalyst shaped body according to the invention is significantly lower by up to one third than the pressure drop of the packing of annular bodies with common dimensions. However, compared to the three-lobed bodies of the prior art of similar dimensions with flat cover sides, the pressure drop of the catalyst shaped body according to the invention is measurably higher, but only within a range that does not adversely affect the operation of the reactor.
[0143] As mentioned above, the single properties listed above may be more favorable to other shaped bodies, but other properties of such other shaped bodies may be less favorable or even worse. The key and surprising advantage of the catalyst shaped bodies of the present invention is that they have overall favorable properties as a whole. For example, compared with annular bodies of conventional size, the catalyst shaped bodies of the present invention are more stable mechanically and show significantly lower pressure drops on the reactor cross section during gas phase reactions. Compared with the trilobate bodies of the prior art of similar size with flat cover sides, the catalyst shaped bodies of the present invention have higher mechanical stability, slightly lower ratio of body volume to surface area, and can have significantly higher packing density per reactor volume. Overall, these advantages are much more important than the higher pressure drop that can be measured on the reactor cross section during gas phase reactions, which is within a harmless range. The above-mentioned various advantages are caused by the outwardly curved arched bodies at the two cover sides of the present invention.
[0144] Partial filling of the recess of the side surface between two adjacent blades increases the mechanical stability and slightly facilitates the forming process without showing significant disadvantages in terms of other properties.
[0145] Another aspect of the present invention is the preparation of the catalyst shaped body of the present invention. It can be roughly divided into two main steps. The first step is to prepare the precursor material that forms the shape of the catalyst shaped body and the second step is to shape the shape of the catalyst shaped body. Depending on the nature of the catalyst shaped body, the precursor material that forms the shape of the catalyst shaped body may already be a precursor of the catalytically active compound, which is usually the case for example of a complete catalyst, or it may be only a precursor of a support material, which is usually the case for example of a supported catalyst, or it may be both together. In the case of a supported catalyst, the catalytically active material is then usually impregnated or otherwise deposited on the shaped structure in a subsequent step.
[0146] In a preferred embodiment of the present invention, the shaped catalyst body of the present invention is prepared by a process comprising the following steps:
[0147] (a) preparing a powdery or granular precursor material containing at least one element from Groups 3 to 12 of the Periodic Table of Elements, and
[0148] (b) compacting it into a catalyst shaped body.
[0149] This method mainly refers to the preparation of complete catalysts.
[0150] The preparation of the precursor material in step (a) can generally be carried out in the same manner as the preparation of the precursor material described in the prior art for the preparation of the annular body or the trilobal body, etc. This is indeed also applicable to the composition of the precursor material. For the catalysts of the prior art, the composition of the precursor material depends on the intended use of the catalyst. In addition to the elements of the 3rd to 12th groups of the periodic table, the precursor material may additionally contain other elements. Such other elements are in particular part of the catalytically active substance, such as phosphorus of the VPO catalyst or catalytically active promoters such as bismuth in some VPO catalysts, may be part of the support material, such as Al2O3 or SiO2, part of the pore former, such as cellulose or stearic acid, or may be part of any auxiliary agent for different purposes, for example, auxiliary materials for the molding process such as graphite powder, or auxiliary materials for improving the mechanical stability of the catalyst molding. The preparation of the precursor material includes mixing the corresponding raw materials in solid or fluid form, chemical reactions between the raw materials, processing steps such as heating, cooling, filtering, dissolving, drying, mechanical processing such as grinding, crushing or screening, etc., and any other steps. Typical preparation methods are described in the prior art and are well known to the skilled person.
[0151] In order to be compacted into a catalyst body in step (b), the precursor material prepared in step (a) has a powdery or granular consistency. If necessary, the precursor material can be processed by compacting, grinding, crushing or screening to obtain the desired state. The powdery or granular material can usually be easily poured or otherwise transported, and therefore can be easily processed in the compacting step (b). Without limiting the scope of the method of the present invention, the particle size of the powdery or granular precursor material is usually 0.1 μm to 2 mm.
[0152] The compaction into the catalyst shaped body in step (b) is usually carried out in a tablet press or similar equipment. Tablet presses are well known to those skilled in the art. Such equipment has been used to produce cylindrical or trilobate catalyst shaped bodies with openings passing therethrough. A specific feature of the production of the catalyst shaped bodies of the present invention is the specific shape and design of the tableting tool. The mold for pressing the material shapes the side surfaces of the body. The lower and upper punches represent the specific geometry of the two covers of the catalyst shaped body. As is usually the case with the tableting of a given precursor material, the speed, and in particular the pressure with which the precursor material is compacted, will affect the mechanical properties of the compacted catalyst shaped body, such as its bulk density or mechanical stability. As is usually the case with tableting methods, the specific and advantageous settings of the machine can be easily determined by a person skilled in the art by carrying out some tests.
[0153] Since the preparation of the shaped catalyst bodies according to the invention does not require any specific precursor materials and does not require any specific machines, it is highly flexible. It only requires a pressing tool, which is adapted to the specific shape of the desired shaped catalyst body. Pressing tools of specific geometries can be easily manufactured according to methods known in the prior art and can also be easily replaced on the tablet press.
[0154] After compaction, depending on the properties of the precursor material, the catalyst shaped body can be used directly as a catalyst or require preactivation. Preactivation can also be carried out in the same or at least similar manner as the preactivation of catalyst bodies with the same precursor material and similar geometry and shape. Preactivation methods generally include heating the catalyst shaped body under more or less defined conditions regarding temperature, heating and cooling rates or surrounding gas phase composition (such as the concentration of oxygen, inert gas or water vapor). Typical preactivation methods are described in the prior art and are well known to the technician.
[0155] In another preferred embodiment of the present invention, the shaped catalyst body according to the invention is prepared by a process comprising the following steps:
[0156] (a) preparing a powdery or granular precursor material,
[0157] (b) compacting it into the shape of a shaped catalyst body, and
[0158] (c) depositing a material containing at least one element from Groups 3 to 12 of the Periodic Table of Elements.
[0159] This method mainly refers to the preparation of supported catalysts.
[0160] With regard to steps (a) and (b), the explanations in the preceding paragraphs mainly about the preparation and compaction of a powdered or granular precursor material containing at least one element of Groups 3 to 12 of the Periodic Table of Elements also apply here, but with the difference that the element of Groups 3 to 12 of the Periodic Table of Elements need not necessarily be present in steps (a) and (b), but are not excluded. Typically, the precursor material in step (a) contains primarily a precursor material for forming a shaped support, but may also contain other compounds such as pore formers, lubricants or any other auxiliary agents. After the compaction of step (b), the compact is typically tempered or calcined to convert the support precursor material into the desired support material. This conversion increases the mechanical stability of the shaped body and is also generally important for the preparation of pores. Typical methods and method conditions for preparing support materials known to those skilled in the art can be used.
[0161] In order to finally obtain the catalyst molding, step (c) requires depositing a material containing at least one element of the 3rd to 12th group of the periodic table on the support molding. For this purpose, a typical method for preparing a supported catalyst can be used. Such methods are well known to those skilled in the art, such as impregnation, precipitation and evaporative deposition. After deposition, depending on the properties of the precursor material, the catalyst molding can be used directly as a catalyst or can require preactivation. Also here, a typical method for preparing a supported catalyst can be used.
[0162] In a preferred embodiment, a catalyst shaped body containing vanadium and phosphorus oxide is prepared. Its preparation comprises:
[0163] (a) reacting a pentavalent vanadium compound and a pentavalent or trivalent phosphorus compound with an organic reducing agent, separating the resulting vanadium and phosphorus-containing precursor, drying it, and converting the dried substance into a powdery or granular precursor material, and
[0164] (b) compacting it into a catalyst shaped body.
[0165] Catalysts comprising vanadium and phosphorus oxides (also referred to as VPO catalysts) are complete catalysts and are generally used for the heterogeneously catalyzed selective gas-phase oxidation of n-butenes to maleic anhydride.
[0166] The preparation of the precursor material as described in step (a) above, the main steps of compaction and its treatment after compaction are fully described in the prior art, such as US 7,060,649, US2011 / 0,257,413 and various other patents and applications known to those skilled in the art. The following paragraphs summarize the typical preparation and composition of vanadium and phosphorus oxide catalysts.
[0167] According to the present invention, the main steps for preparing the vanadium and phosphorus oxide catalyst as a preferred shaped catalyst body are as follows.
[0168] (a) Preparing a powdery or granular precursor material.
[0169] (i) reacting a pentavalent vanadium compound with an organic, reducing solvent in the presence of a phosphorus compound under heating. This step may optionally be carried out in the presence of dispersed, powdered auxiliary materials. Preferably, the reaction is carried out without the addition of auxiliary materials.
[0170] (ii) isolating the formed vanadium, phosphorus and oxygen-containing catalyst precursor ("VPO precursor"), for example by filtration or evaporation.
[0171] (iii) drying the VPO precursor, preferably preliminarily pre-activated by heating at a temperature of 250-350° C. Then, powdered auxiliary materials and / or pore formers, such as stearic acid, cellulose or paraffin, may be added to the dried and preferably heat-treated VPO precursor, the substances being thoroughly mixed and optionally ground, pulverized and / or sieved to obtain a powdered precursor material.
[0172] (b) Compaction
[0173] The powdered precursor material obtained is compacted into the shape of the catalyst shaped body of the invention. The compaction is preferably carried out by tableting, preferably with prior mixing with a lubricant such as graphite.
[0174] (c) Preactivation
[0175] The shaped VPO precursor is preactivated by heating in an atmosphere containing oxygen (O2), hydrogen oxide (H2O) and / or an inert gas.
[0176] The mechanical and catalytic properties of the catalyst can be influenced by a suitable combination of temperature, treatment time and gas atmosphere matched to the respective catalyst system.
[0177] As pentavalent vanadium compounds, oxides, acids, inorganic salts and organic salts containing pentavalent vanadium, or mixtures thereof can be used. Preferably, vanadium pentoxide (V2O5), ammonium metavanadate (NH4VO3) and ammonium polyvanadate ((NH4)V6O3) are used. 16 ), in particular vanadium pentoxide (V2O5). The pentavalent vanadium compound present as a solid is used in the form of a powder, preferably a powder with a particle size of 50-500 μm.
[0178] As the phosphorus compound, there can be used a phosphorus compound having a reducing effect, such as phosphorous acid, and a pentavalent phosphorus compound, such as phosphorus pentoxide (P2O5), orthophosphoric acid (H3PO4), pyrophosphoric acid (H4P2O7), n+2 P n O 3n+1(where n≥3) polyphosphoric acid or a mixture thereof. Preferably a pentavalent phosphorus compound is used. The content of the compounds and mixtures is usually reported as a weight percentage based on H3PO4. Preferably, H3PO4 is used in a concentration of 80-110%, particularly preferably H3PO4 in a concentration of 95-110%, and very particularly preferably H3PO4 in a concentration of 100-105%.
[0179] As solvents with reducing action, preference is given to using primary or secondary, acyclic or cyclic, unbranched or branched saturated alcohols or mixtures thereof having 3 to 6 carbon atoms. Preference is given to using primary or secondary, unbranched or branched C3-C6 alkanols or cyclopentanols or cyclohexanols.
[0180] Suitable alcohols which may be mentioned are n-propanol (1-propanol), isopropanol (2-propanol), n-butanol (1-butanol), sec-butanol (2-butanol), isobutanol (2-methyl-1-propanol), 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1-hexanol, 3-methyl-1-pentanol, 4-methyl-1-pentanol, 3-methyl-2-pentanol, 4-methyl-2-pentanol, 2,2-dimethyl-1-butanol, 2,3-dimethyl-1-butanol, 3,3-dimethyl-1-butanol, 3,3-dimethyl-2-butanol, cyclopentanol, cyclohexanol and mixtures thereof. Very particular preference is given to n-propanol (1-propanol), n-butanol (1-butanol), isobutanol (2-methyl-1-propanol), 1-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol and cyclohexanol, in particular isobutanol.
[0181] These components can be combined in various ways, for example in a stirred vessel. The amount of reducing solvent should be above the stoichiometric amount required to reduce vanadium from oxidation state +5 to oxidation state +3.5 to +4.5. The amount of reducing solvent to be added is usually at least sufficient to slurry the pentavalent vanadium compound so that it can be intensively mixed with the added phosphorus compound.
[0182] The slurry is heated to convert the above compounds and form a catalyst precursor. The temperature range to be selected depends on various factors, especially the reduction effect and the boiling point of the components. The temperature is usually set at 50-200°C, preferably 100-200°C. The reaction at high temperature usually takes several hours.
[0183] The promoter compound can be added at any point in time. Suitable promoter compounds are, for example, acetates, acetylacetonates, oxalates, oxides or alkoxylates of the above-mentioned promoter metals, for example cobalt acetate, cobalt(II) acetylacetonate, cobalt(II) chloride, molybdenum(VI) oxide, molybdenum(III) chloride, iron(III) acetylacetonate, iron(III) chloride, zinc(II) oxide, zinc(II) acetylacetonate, lithium chloride, lithium oxide, bismuth(III) chloride, bismuth(III) ethylhexanoate, nickel(II) ethylhexanoate, nickel(II) oxalate, zirconium(II) oxychloride, zirconium(IV) butoxide, silicon(IV) ethoxide, niobium(V) chloride and niobium(V) oxide.
[0184] After the above-mentioned heat treatment is completed, the catalyst precursor formed is separated, wherein a cooling phase and a storage or aging phase of the cooled reaction mixture can be optionally inserted before the separation. In the separation step, the solid catalyst precursor is separated from the liquid phase. Suitable methods are, for example, filtration, decantation or centrifugation. The catalyst precursor is preferably separated by filtration.
[0185] The separated catalyst precursor can be further processed with or without prior washing. The separated catalyst precursor is preferably washed with a suitable solvent, for example to remove residual agents with a reducing effect (e.g. alcohols) or their degradation products that still adhere to the catalyst precursor. Suitable solvents are, for example, alcohols (e.g. methanol, ethanol, 1-propanol, 2-propanol), aliphatic and / or aromatic hydrocarbons (e.g. pentane, n-hexane, white spirit, benzene, toluene, xylene), ketones (e.g. acetone, 2-butanone, 3-pentanone), ethers (e.g. 1,2-dimethoxyethane, tetrahydrofuran, 1,4-dioxolane) or mixtures thereof. If the catalyst precursor is washed, 2-propanone and / or methanol are preferably used, particularly preferably methanol.
[0186] After separation of the catalyst precursor or after washing, the solid is usually dried. Drying can be carried out under various conditions. Usually it is carried out under reduced pressure or atmospheric pressure. The drying temperature is usually 30-300° C. Drying is preferably carried out under an oxygen-containing or oxygen-free gas atmosphere such as air or nitrogen at a pressure of 1-30 kPa (absolute) and a temperature of 50-200° C.
[0187] In a preferred embodiment, the catalyst precursor powder is thoroughly mixed with about 2 to 4 wt% of graphite and pre-densified. The pre-densified particles can be mixed again with 1-2 wt% of graphite and then tableted to obtain a catalyst shaped body.
[0188] In another embodiment of the compacting operation, the catalyst precursor powder is intimately mixed with about 2 to 4% by weight of graphite and additionally 5 to 40% by weight, in particular 20 to 25% by weight, of a pore former and further processed and compacted as described above to give a shaped catalyst body. As typical pore formers, mention is made of stearic acid, cellulose or alkanes.
[0189] The precursor powder is then compacted into the shape of a shaped catalyst body. Advantageously, it is compressed in a tablet press or similar equipment.
[0190] The shaped VPO precursor is heated at 250-600 °C in an atmosphere containing oxygen (O2), hydrogen peroxide (H2O) and / or an inert gas. ℃ The pre-activation (calcination) is heated at a temperature of 1000 °C. Suitable inert gases are, for example, nitrogen, carbon dioxide and rare gases. The heat treatment can be carried out intermittently, for example in a vertical furnace, a tray furnace, a muffle furnace or an oven, or can be carried out continuously, for example in a rotary tube furnace, a belt calcining furnace or a rotary spherical furnace. It can include continuous different parts in terms of temperature, such as heating, maintaining a constant temperature or cooling, and continuous different parts in terms of atmosphere, such as oxygen-containing, water vapor-containing, oxygen-free gas atmosphere. Suitable pre-activation methods are described in, for example, US 5,137,860, US 4,933,312 or WO 95 / 029,006. It is particularly preferred to continuously calcine in a belt calcining furnace, which has at least two, for example 2-10 calcination zones, which optionally have different gas atmospheres and different temperatures. The mechanical and catalytic properties of the catalyst may be affected and can therefore be set in a targeted manner by a suitable combination of temperature, treatment time and gas atmosphere matched with the corresponding catalyst system.
[0191] Preference is given to calcination in which the catalyst precursor is (i) heated in at least one calcination zone in an oxidizing atmosphere with an oxygen content of 2 to 21% by volume to a temperature of 200 to 350° C. and maintained under these conditions until the desired average oxidation state of the vanadium is reached; and (ii) heated in at least one other calcination zone in a non-oxidizing atmosphere with an oxygen content of ≤1% by volume and a hydrogen peroxide content of 20 to 75% by volume to a temperature of 300 to 500° C. and maintained under these conditions for ≥0.5 h.
[0192] The calcination generally comprises a further step (iii) which is carried out after step (ii) and in which the calcined catalyst precursor is cooled in an inert gas atmosphere to a temperature of ≤300° C., preferably ≤200° C. and in particular ≤150° C.
[0193] In the calcination according to the process of the invention, before, between and / or after steps (i) and (ii) or (i), (ii) and (iii), other steps may be taken. Without constituting a limitation, other steps that may be mentioned are, for example, a change in temperature (heating, cooling), a change in the gas atmosphere (setting a different gas atmosphere), other holding times, transfer of the catalyst intermediate to other devices or interruption of the entire calcination operation.
[0194] For their use in the heterogeneously catalyzed selective gas phase oxidation of n-butenes to maleic anhydride, the shaped catalyst bodies of the VPO catalysts are preferably characterized by a V content of 25 to 40% by weight, a P content of 15 to 25% by weight, a Mo content of 0 to 2% by weight, an Fe content of 0 to 2% by weight, and the following geometry of the shaped catalyst bodies:
[0195] d1 = 1.5 to 2.5 mm,
[0196] d2 = 0.8 to 1.6 mm,
[0197] d3 = 0.8 to 1.6 mm,
[0198] h1=4 to 9 mm,
[0199] h2, h3 = 0.2 to 3 mm,
[0200] and an outwardly shaped arched body.
[0201] In another preferred embodiment, a shaped catalyst body containing a multimetallic oxide of Mo, Fe and Bi is prepared. The preparation thereof comprises:
[0202] (a) preparing an aqueous mixture containing a Mo compound, an Fe compound and a Bi compound, drying the mixture, converting the dried mixture into a powdery or granular precursor material, and
[0203] (b) compacting it into a catalyst shaped body.
[0204] Catalysts containing Mo, Fe and Bi multimetallic oxides are complete catalysts and are suitable for the heterogeneously catalyzed partial gas phase oxidation of propylene to acrolein, isobutylene to methacrolein, propylene to acrylonitrile and isobutylene to methacrylonitrile. They are particularly suitable for the heterogeneously catalyzed partial gas phase oxidation of propylene to acrolein.
[0205] The preparation of the precursor material as described in step (a) above, the main steps of compaction and its treatment after compaction are fully described in the prior art, for example as described in US2013 / 0,023,699 and various other patents and applications known to those skilled in the art. The following paragraphs summarize the typical preparation and composition of catalysts containing Mo, Fe and Bi multimetallic oxides.
[0206] (a) Preparation of powdered or granular precursor materials.
[0207] (i) preparing an aqueous mixture containing a Mo compound, an Fe compound, a Bi compound and optionally one or more promoter compounds.
[0208] (ii) drying the mixture obtained, for example by spray drying or by conventional evaporation.
[0209] (iii) The dried mixture can optionally be processed further before it is compacted into the desired shape, for example by comminuting to the desired fineness, by precalcining or precompacting.
[0210] Instead of steps (i) and (ii), it is in principle also possible to mix the precursor materials in dry form.
[0211] (b) Compaction
[0212] The powdered precursor material obtained is compacted into the shape of the catalyst shaped body of the invention. The compaction is preferably carried out by tableting, preferably with prior mixing with a lubricant such as graphite.
[0213] (c) Heat treatment
[0214] The formed precursor containing Mo, Fe and Bi is heat treated by heating in an inert, oxidizing or reducing atmosphere.
[0215] The mechanical and catalytic properties of the catalyst can be influenced by a suitable combination of temperature, treatment time and gas atmosphere matched to the respective catalyst system.
[0216] As a favorable Mo source for preparing the precursor mixture, ammonium heptamolybdate tetrahydrate is mentioned. Other possible Mo sources are, for example, ammonium orthomolybdate ((NH4)2MoO4), ammonium dimolybdate ((NH4)2Mo2O7), ammonium tetramolybdate dihydrate ((NH4)2Mo40 13 x5H2O) and ammonium molybdate dihydrate ((NH4)4Mo 10 O 32 x2H2O).
[0217] A favorable Fe source is Fe 3+ Salts such as iron (III) nitrate hydrate, in particular iron (III) nitrate nonahydrate. Of course, Fe 2+ Salt was used as the Fe source.
[0218] As a Bi source, Bi 3+ Salts are advantageous. Possible such salts are, for example, bismuth(III) oxide, bismuth(III) oxynitrate (bismuth oxynitrate), bismuth halides (eg fluoride, chloride, bromide, iodide), in particular bismuth(III) nitrate pentahydrate.
[0219] As regards the optional promoter compounds, these are also preferably added in the form of their suitable salts as described in the prior art. Possible promoter compounds are, for example, Ni, Co, Cu, alkali metals, alkaline earth metals, Th, Sm, Zn, Cd, P, As, B, Sb, Sn, Pb, Ce, V, Cr, Nb, Ta, Re, Rh, W, Ag, Au, Ga, Si, Al, Ti.
[0220] The precursor compounds are preferably mixed together in the form of their aqueous solutions and dried to obtain a solid material which can be further processed. As mentioned before, spray drying or conventional evaporation are possible methods.
[0221] In the case of spray drying, typical gas inlet temperatures are from 250 to 450° C., preferably from 270 to 370° C. Typical gas outlet temperatures are from 100 to 160° C., preferably from 120 to 150° C. The average particle diameter of the resulting spray powder is generally from 10 to 100 μm, preferably from 15 to 60 μm, more preferably from 25 to 50 μm, the diameters mentioned being determined by light scattering of the spray powder dispersed in water at 25° C. in accordance with ISO 13320. The tapped bulk density (25 ℃ , 0.1 MPa (absolute)) is generally 500 to 1300 g / L, preferably 700 to 1100 g / L. The ignition loss of the spray powder (calcined at a powder temperature of 600° C. for 3 hours under fixed air (excessive presence)) is generally 20 to 40% by weight, preferably 25 to 35% by weight, based on its starting weight.
[0222] Before the dried precursor material is compacted into the desired shape, it can be further processed, for example by comminution, precalcination or precompacting. In addition, auxiliary agents such as graphite or stearic acid can also be added as lubricants and other auxiliary agents. Appropriately for the purpose of application, the particle diameter of the precursor composition to be compacted (particle diameter of the finely divided homogeneous dry mixture), optionally as a result of previous coarsening by compaction, is 100 to 2000 μm, preferably 150 to 1500 μm, more preferably 400 to 1250 μm, or 400 to 1000 μm, or 400 to 800 μm.
[0223] The precursor powder is then compacted into the shape of a catalyst shaped body. Advantageously, it is pressed in a tablet press or similar equipment. Advantageously, the compacting pressure used in compacting the finely divided precursor composition as a finely divided homogeneous dry mixture is 50 to 50,000 kg / cm 2 , preferably 200 to 10000 kg / cm 2 , more preferably 400 to 5000 kg / cm 2 , most preferably 600 to 3000 kg / cm 2 The catalyst precursor shaped body generally has a carbon content of 1 to 5 g / cm 3 , preferably 1.5 to 3.5 g / cm 3 , most preferably 2 to 3 g / cm 3 The body density.
[0224] The shaped Mo-, Fe- and Bi-containing precursors are preactivated (calcined) by heating in an inert, oxidizing or reducing atmosphere, preferably in an oxidizing atmosphere containing oxygen (O2), such as in air, at a temperature of 350 to 650°C. The heat treatment can in principle be carried out in various types of furnaces, such as heatable convection chambers (convection furnaces, such as convection shaft furnaces), disk furnaces, rotary tube furnaces, belt calcining furnaces or shaft furnaces. The shaped catalyst bodies generally have a mass fraction of 1 to 5 g / cm 3 , preferably 1.2 to 2.5 g / cm 3 , most preferably 1.4 to 2.2 g / cm 3 The body density.
[0225] In an alternative but also preferred embodiment, the catalyst shaped body containing the Mo, Fe and Bi multimetallic oxide is prepared as a coated catalyst. For this purpose, a mixture containing the Mo compound, the Fe compound and the Bi compound is applied to a prefabricated support shaped body, which predetermines the shape of the final Mo, Fe and Bi-containing catalyst shaped body. The support shaped body can contain support materials such as Al2O3 and SiO2, etc., which are usually used for support shaped bodies. The support shaped body can be produced as known in the prior art, but in particular it is formed in the shape of the catalyst shaped body. Its coating with the precursor mixture containing the Mo, Fe and Bi multimetallic oxide can also be carried out as generally known in the prior art, for example by using a rotatable container. Finally, the coated catalyst shaped body is usually preactivated (heat treated) as described above for the finished catalyst.
[0226] For their use in the heterogeneously catalyzed selective gas-phase oxidation of propene to acrolein or acrylonitrile, of isobutene to methacrolein or methacrylonitrile, the shaped catalyst bodies comprising Mo, Fe and Bi multimetallic oxides are preferably characterized by the stoichiometry of the general formula (I):
[0227] Mo 12 Bi a Fe b X1 c X2 d X3 e X4 f O n (I)
[0228] in
[0229] X1=Ni and / or Co,
[0230] X2 = Tl, Sm, alkali metal and / or alkaline earth metal,
[0231] X3=Zn, P, As, B, Sb, Sn, Ce, Pb, V, Cr, Nb and / or W, X4=Si, Al, Ti and / or Zr,
[0232] a=0.2 to 5,
[0233] b = 0.01 to 5,
[0234] c = 0 to 10,
[0235] d = 0 to 2,
[0236] e = 0 to 8,
[0237] f = 0 to 10, and
[0238] n = a value determined by the valence and abundance of the elements in formula (I) other than oxygen,
[0239] Or characterized by the stoichiometry of general formula (II):
[0240] [Y1 a′ Y2 b′ O x′ ] p [Y3 c′ Y4 d′ Y5 e′ Y6 f′ Y7 g′ Y8 h′ O y′ ] q (II)
[0241] in
[0242] Y1 = Bi alone, or Bi and at least one of the elements Te, Sb, Sn and Cu,
[0243] Y2=Mo and / or W,
[0244] Y3 = alkali metal, Tl and / or Sm,
[0245] Y4 = alkaline earth metal, Ni, Co, Cu, Mg, Zn, Sn and / or Ca
[0246] Y5 = Fe alone, or Fe and at least one of the elements V, Cr and Ce,
[0247] Y6=P, As, B and / or Sb,
[0248] Y7 = rare earth metals, Ti, Zr, Nb, Ta, Re, Ru, Rh, Ag, Au, Al, Ga, In, Si, Ge and / or Pb,
[0249] Y8 = Mo alone, or Mo and W,
[0250] a′=0.01 to 8,
[0251] b′=0.1 to 30,
[0252] c′=0 to 4,
[0253] d′=0 to 20,
[0254] e′=>0 to 20,
[0255] f = 0 to 6,
[0256] g′=0 to 15,
[0257] h′=8 to 16,
[0258] x', y' = values determined by the valence and abundance of the elements in formula (II) other than oxygen, and p, q = values whose p / q ratio is 0.1 to 10,
[0259] and having a molybdenum content of 10 to 85% by weight,
[0260] and the geometry of the shaped catalyst body, wherein
[0261] d1 = 1 to 5 mm, more preferably 1 to 3 mm, particularly preferably 1 to 2 mm,
[0262] d2 = 1 to 2 mm,
[0263] d3 = 1 to 2 mm,
[0264] h1=4 to 9 mm,
[0265] h2, h3 = 0.2 to 1 mm,
[0266] and an outwardly shaped arched body.
[0267] The catalyst shaped bodies of the present invention can be easily prepared by known methods. Only the compaction requires a specific mold and a pressing punch or a suitable substitute to form the outwardly curved arched body. However, the manufacture of a specific pressing punch or a suitable substitute is part of the expertise and is therefore within common practice.
[0268] The catalyst shaped body of the present invention can be advantageously used for the catalytic conversion of organic compounds in the gas phase in a fixed bed reactor. The geometry of the fixed bed reactor, including its length and its inner diameter, and the presence of specific internals such as thermocouples, can be adapted according to the specific requirements and catalytic performance of the reaction. In addition, the mode and nature of the filler of the fixed bed reactor can also be adapted according to the specific requirements and catalytic performance of the reaction. For example, the reactor can contain a continuous filler of a type of catalyst shaped body, it can contain a mixture of different catalyst shaped bodies, and there can also be catalyst bodies other than the catalyst shaped body of the present invention, it can also contain structured fillers of different catalyst shaped bodies, and there can also be catalyst bodies other than the catalyst shaped body of the present invention, and it can also contain inert substances as diluents.
[0269] Although the catalyst molded body of the present invention can be widely used in various catalytic conversions of various organic compounds in the gas phase in a fixed bed reactor, it is preferably used for catalytic conversions such as oxidation or oxychlorination in the presence of oxygen. Since oxidation reactions are usually exothermic, the heat generated during oxidation must be removed. For undesirable exothermic reactions, heat can be removed together with the gaseous effluent stream. For other exothermic reactions, particularly for high exothermic reactions, the cooling of a fixed bed reactor may be required. This cooling can be carried out, for example, by a cooling plate in the reactor or a cooling outer wall of the reactor. The cooling type mentioned last is usually more effective for a reactor with a higher outer surface to internal volume ratio and therefore has a tubular shape. Such reactors are called fixed bed tubular reactors and are usually more preferably used for gas phase oxidation reactions.
[0270] Therefore, another aspect of the present invention is a reactor tube filled with a plurality of catalyst shaped bodies of the present invention. The inner diameter of the reactor tube generally depends on the size of the catalyst shaped body filled and the exothermicity of the oxidation reaction. Usually the inner diameter corresponds at least to the highest value of the outer dimension of the catalyst shaped body, i.e. the total height h0 or the outer diameter d0 (whichever is higher). More preferably, the inner diameter of the reactor tube is ≥1.5 times, particularly preferably ≥2 times, and very particularly preferably ≥2.5 times the highest value of the outer dimension of the catalyst shaped body. The maximum inner diameter of the recommended reactor tube depends mainly on the ability to properly remove the generated heat. It can be determined by a person skilled in the art in the same manner as determining other shaped catalysts for such reactions. However, the inner diameter of the reactor tube is preferably ≤10 cm, more preferably ≤8 cm, and particularly preferably ≤5 cm. The length of such reactor tubes depends mainly on the nature of the oxidation reaction. It is generally 1 to 20 m, preferably ≥2 m, more preferably ≥3 m, and preferably ≤15 m, more preferably ≤10 m.
[0271] The above reactor tube is filled with a plurality of shaped catalyst bodies according to the invention. The term plurality means that the reactor tube is filled with a relatively large number of such shaped catalyst bodies, depending on the size of the shaped catalyst bodies, the type of filler, whether it is filled with only such shaped catalyst bodies or diluted, for example, with inert substances or other catalyst bodies, and on the geometry of the reactor tube, mainly its inner diameter and length. More specifically, a plurality preferably means at least 100 or more such shaped catalyst bodies. There are not many restrictions on the maximum number.
[0272] Therefore, a more preferred aspect of the present invention is a reactor tube filled with ≥100 particles of the inventive shaped catalyst bodies. Particularly preferably, the reactor tube has an inner diameter ≥1.5 times the highest value of the outer dimensions of the shaped catalyst bodies and a length ≥1 m.
[0273] Since the tubes show only a very limited internal volume per unit length, it is preferred to combine a plurality of such tubes side by side into a large reactor unit. Such reactor units are well known in the prior art as shell-and-tube reactors, in which a cooling medium such as a salt bath circulates around the tubes. The use of such shell-and-tube reactors is particularly preferred for gas phase oxidation in the presence of the catalyst shaped bodies of the present invention. The number of reactor tubes in a shell-and-tube reactor depends primarily on the expected production capacity of the device. It is generally 10,000 to 60,000 tubes, preferably ≥20,000 tubes and preferably ≤50,000 tubes.
[0274] Finally, a further aspect of the present invention is a process for producing oxidized organic compounds by heterogeneously catalyzed gas-phase oxidation of organic compounds in the presence of an oxygen-containing gas and the shaped catalyst bodies according to the invention.
[0275] The oxidation is usually carried out using an oxygen-containing gas as the oxidant, such as air, synthetic air, oxygen-enriched gas or even highly concentrated or pure oxygen, as long as the heat generation allows for a higher oxygen concentration.
[0276] As preferred processes according to the invention there is mentioned the oxidation of n-butane or benzene to maleic anhydride, the oxidation of propylene to acrolein, the oxidation of isobutylene to methacrolein, the oxidation of acrolein to acrylic acid, the oxidation of methacrolein to methacrylic acid and the oxidation of methanol to formaldehyde.
[0277] Particular preference is given to a process for producing maleic anhydride by heterogeneously catalyzed gas-phase oxidation of n-butane in the presence of an oxygen-containing gas and a shaped catalyst body according to the invention which contains an oxidic material comprising vanadium and phosphorus.
[0278] In addition to the abovementioned use of n-butane as starting material for the production of maleic anhydride, it is also possible in principle to use other aliphatic or aromatic, saturated or unsaturated hydrocarbons, preferably having 4 to 6 carbon atoms, more preferably having 4 carbon atoms, such as 1-butene, 2-butene or 1,3-butadiene.
[0279] A particularly preferred process for producing maleic anhydride by oxidation of n-butane in the presence of the catalyst shaped body of the invention is preferably carried out under the process conditions well described in the prior art, for example as described in US 7,060,649, US2011 / 0,257,413 and various other patents and applications known to the person skilled in the art. The process is generally preferably carried out at a temperature of 250 to 500° C., preferably 380 to 460° C., particularly preferably 380 to 440° C. It is advantageously carried out in an isothermal manner (which has a temperature profile that increases over the length of the reactor) or by using a combination of a temperature that increases over the length of the reactor and an isothermal operating mode. It is advantageously carried out at an oxygen partial pressure of 0.001 to 0.1 MPa (absolute), preferably 0.01 to 0.1 MPa (absolute), particularly preferably 0.03 to 0.1 MPa (absolute), especially 0.04 to 0.09 MPa (absolute). The hydrocarbon concentration of the feed stream fed to the reactor unit is 0.5 to 10% by volume, preferably 0.5 to 5% by volume, particularly preferably 1 to 3% by volume, very particularly preferably 1 to 2.5% by volume. The hydrocarbon conversion per pass through the reactor is 40-100%, preferably 50-95%, particularly preferably 70-95%, in particular 85-95% of the hydrocarbons in the feed stream. The GHSV (gas hourly space velocity) is preferably set via the amount of the feed stream introduced into the reactor unit, based on the volume of the feed stream standardized to 0° C. and 0.1013 MPa (absolute) and based on the reaction volume filled with catalyst, to 1000 to 5000 h -1 , particularly preferably 1000 to 3000h -1 . Preferably, in the process of the invention, a volatile phosphorus compound is advantageously introduced into the gas in order to ensure a long catalyst operating life and to further increase the conversion, selectivity, yield, space velocity and space-time yield of the catalyst. Its concentration at the beginning, i.e. at the reactor inlet, is 0.2 to 20 ppm by volume of volatile phosphorus compounds, based on the total volume of the gas at the reactor inlet. A content of 0.5 to 5% by volume is preferred. Volatile phosphorus compounds are all phosphorus-containing compounds which are present in gaseous form at the desired concentration under the conditions of use. Preference is given to using triethyl phosphate or trimethyl phosphate as volatile phosphorus compound.
[0280] Particular preference is also given to processes for producing acrolein, acrylic acid, acrylonitrile, methacrolein or methacrylonitrile by heterogeneously catalyzed gas phase oxidation of propene or isobutene in the presence of an oxygen-containing gas and a shaped catalyst body according to the invention containing an oxidizing material comprising Mo, Fe and Bi. In the case of the preparation of acrolein or acrylonitrile as the oxidized organic compound, propene is used as the organic compound, and in the case of the preparation of methacrolein or methacrylonitrile as the oxidized organic compound, isobutene is used as the organic compound.
[0281] The particularly preferred process for producing acrolein, acrylonitrile, methacrolein or methacrylonitrile by oxidation of propylene or isobutene in the presence of the shaped catalyst bodies of the invention is preferably carried out under the process conditions which are well described in the prior art, for example as described in US 2005 / 0,101,803 and in various other patents and applications known to the person skilled in the art.
[0282] A shell and tube reactor cooled by a salt bath is usually used. The inner diameter of each reactor tube is usually 20 to 30 mm, preferably 21 to 28 mm, and most preferably 25 to 27 mm. The length of each reaction tube is usually 2 to 5 m, preferably 3 to 4.5 m, and most preferably 3.2 to 4 m. The method is usually preferably carried out at a temperature of 300 to 450° C. and a reaction pressure of 0.05 to 0.4 MPa (absolute). The hydrocarbon concentration of the feed stream supplied to the reactor unit is usually 4 to 20% by volume, preferably 5 to 15% by volume, and particularly preferably 5 to 8% by volume. The hydrocarbon conversion rate of each passage through the reactor is 50-100%, preferably 80-99%, and particularly preferably 90-99% of the hydrocarbons in the feed stream. The GHSV (gas hourly space velocity) is preferably 1000 to 10000 h -1 , particularly preferably 1500 to 5000h -1 , based on the volume of the feed stream normalized to 0° C. and 0.1013 MPa (absolute) and based on the reaction volume filled with catalyst.
[0283] Due to its geometry, the catalyst shaped body of the invention combines high mechanical stability, high packing density per reactor volume, efficient diffusion paths within the bulk volume, high packing density within a typical reactor tube and high catalyst shaped body heat exchange efficiency with a low bulk volume to surface area ratio, low pressure drop over the reactor cross section during gas phase reactions, low fragmentation and low wear during handling of the catalyst and filling it into the reactor. Its performance is overall completely positive compared to the known shapes described in the prior art. It is very flexible with regard to its active substances, making it possible to use the same precursor oxidic materials as the shaped catalysts known for conversions of organic compounds such as oxidation, oxychlorination, hydrogenation and other conversions.
[0284] Furthermore, the catalyst shaped bodies according to the invention can be easily produced by methods known to the person skilled in the art. Although the shaping requires special pressing punches or suitable substitutes, their production is part of the expertise and can be easily performed.
[0285] The shaped catalyst bodies of the present invention can produce various types of organic compounds by heterogeneously catalyzed gas phase conversion of the corresponding organic isolated compounds, including the production of oxidized organic compounds such as acrolein or acrylic acid from propylene or maleic anhydride from n-butane in high yield and high selectivity by utilizing the specific advantages of the shaped catalyst bodies. Example
[0286] Since the advantageous characteristics of the shapes of the catalyst shaped bodies of the present invention with respect to their physical properties, such as their surface area to bulk volume ratio, their mechanical stability, their packing density in a typical reactor tube, their total surface area / bulk volume in a typical reactor tube and their pressure drop in a typical reactor tube can be better and more easily compared with the corresponding characteristics of typical catalyst shaped bodies of the prior art by numerical simulation rather than by laborious experiments, numerical simulations were performed. The general procedure of the numerical simulations is explained below.
[0287] Simulation Program
[0288] The starting point for Examples 1 to 5 was a simulated prior art annular body of 6.5 x 5.0 x 3.5, with an outer diameter of 6.5 mm, an inner bore of 3.5 mm in diameter and a height of 5.0 mm, which is a typical dimension of a vanadyl pyrophosphate (VO) 2 P2 O7 catalyst (VPO catalyst) for the oxidation of n-butane to maleic anhydride. This catalyst shaped body was formed by CAD (computer-aided design) as a comparative shaped body. Based on the annular body described, catalyst shaped bodies according to the invention and other comparative catalyst shaped bodies were formed by CAD and compared with each other.
[0289] For Examples 6-10, the starting point was to simulate another prior art annular body with dimensions of 5.0 x 5.0 x 2.0, which involves an outer diameter of 5.0 mm, an inner hole of 2.0 mm diameter and a height of 5.0 mm. This dimension is typical for Mo, Fe and Bi multimetal oxide catalysts for the oxidation of propylene to acrolein and acrylic acid.
[0290] Although the dimensions d0, d1, d2, d3, h0, h1, h2 and h3 are defined for the shaped catalyst bodies according to the invention, they also apply in an analogous manner to the shaped catalyst bodies as follows:
[0291] d0 is the outer diameter as the diameter of the smallest circle which surrounds the shaped catalyst body in a horizontal section. In the case of an annular body as the shaped catalyst body, d0 refers to the outer diameter of the annular body.
[0292] d1: Inner diameter of the continuous hole.
[0293] d2 is the wall thickness between two consecutive holes. Since there is only one hole in the annular body, d2 does not exist in the annular body.
[0294] d3 Wall thickness between continuous pore and side surface. In the case of annular bodies as shaped catalyst bodies, d3 is the wall thickness around a single pore.
[0295] h0 Total height in the vertical direction.
[0296] h1 Height between the (imaginary) planar bottom cover region and the (imaginary) planar top cover. In the case of shaped catalyst bodies with two planar covers, h1 is equal to d0.
[0297] h2, h3 are the heights of the outwardly curved arch. In the case of a flat cover, h2 and h3 are 0.
[0298] In addition to the geometry, two other physical properties must be defined for comparison purposes. One of these physical properties is the bulk density of the catalyst body. For simplicity, this is set to 1 g / cm for all examples. 3 , which is equal to 1000kg / m 3 . Although this value deviates from the typical bulk density of VPO and other metal oxides such as Mo, Fe and Bi multimetallic oxides (which are higher), this does not prejudice the direct comparison between different catalyst shaped bodies according to the invention and comparative catalyst shaped bodies. A further physical property is the mechanical hardness of the bulk material. Here too, fixed values were selected and used for all simulations. The mechanical hardness determines the lateral crushing strength of the respective catalyst shaped body together with the shape and the absolute dimensions. With respect to the properties resulting from the bulk density, the properties resulting from the mechanical hardness can also be directly compared, since the same initial values were used in all simulations.
[0299] Based on the geometry, bulk density and mechanical stiffness, a specific geometric value, referred to as the "characteristic length", the side crushing strength, the packing density in the model reactor tube and the pressure drop in the model reactor tube at a certain flow rate were calculated by simulation. The mentioned values are described below.
[0300] Characteristic length
[0301] Characteristic length is defined as the volume of the body (denoted by "V" and expressed in mm 3 measurement) and surface area (expressed as "SA" and in mm 2 The characteristic length is the ratio between the length of the catalyst and the surface area. It is expressed in mm. The bulk volume and surface area can be easily calculated by the geometric shape of the catalyst molding. Under a given bulk volume, the characteristic length decreases with the increase of the surface area. Since a large surface area is conducive to the mass transfer of the separated compound of the reaction mixture to the catalyst molding and the mass transfer of the product compound back to the reaction mixture, a low characteristic length is desirable for effective catalysis.
[0302] Side crushing strength
[0303] The side crushing strength (expressed as "SCS") indicates the mechanical strength of the catalyst shaped body. In practice, it is measured by directly compressing an annular, cylindrical or trilobate catalyst shaped body with two uniform plates parallel to the axis and determining the force of the catalyst shaped body crushing. The side crushing strength is expressed in N. For the present numerical simulation, a numerical method is used to simulate the side crushing strength test taking into account the shape of the catalyst shaped body, its absolute size and the mechanical hardness of the bulk material. A high side crushing strength is generally advantageous because it indicates that the mechanical stability of the catalyst shaped body is high. However, the side crushing strength of the catalyst shaped body must be viewed in conjunction with its mass, or if the bulk density is the same, in conjunction with its bulk volume. The greater the mass of the catalyst shaped body, the higher the side crushing strength should be to avoid cracks during the filling of the reactor tube. In other words, a large catalyst shaped body with a specific side crushing strength is mechanically weaker than a small catalyst shaped body with the same side crushing strength. Therefore, a more meaningful value is the side crushing strength SCS / bulk volume V (in N / mm 3 Measurement).
[0304] Filling density
[0305] The packing density indicates how densely the shaped catalyst bodies are located in a vertical reactor tube (if the shaped catalyst bodies are loosely packed from the top of the tube). For the present numerical simulations, an internal diameter ID of the reaction tube of 21 mm (Examples 1-5) and 26 mm (Examples 6-10) was assumed, since these are typical values for shell-and-tube reactors, e.g. with respect to 21 mm for the oxidation of n-butane to maleic anhydride or 26 mm for the oxidation of propylene to acrolein. The arrangement of the shaped catalyst bodies in the reactor tube during its filling was calculated by using Newton's equations of motion and the spatial geometry of the filled tube was visualized by CAD. The packing density is expressed in kg / m 3 A high packing density of shaped catalyst bodies is generally preferred, since it involves a high amount of catalytically active material per volume of reaction zone, which enables, inter alia, a more compact reactor design at a given conversion rate.
[0306] Surface area / filling volume
[0307] The surface area / filling volume represents the available surface area of the catalyst shaped bodies in the vertical reactor tube (if they were filled loosely from the top of the tube). For the present numerical simulations, the same inner diameter ID of the reactor tube as the packing density was assumed, namely 21 mm (Examples 1-5) and 26 mm (Examples 6-10). The arrangement of the catalyst shaped bodies in the reactor tube during its filling was calculated by using Newton's equations of motion and the spatial geometry of the filled tube was visualized by CAD. The surface area / filling volume is expressed in m 2 / m 3 High surface area / packing volume is generally preferred because it involves a large surface area of catalyst bulk per reaction zone volume.
[0308] Pressure Drop
[0309] Based on the geometry and packing of the reactor tube as described under the packing density above, the pressure drop in the reactor tube at 20°C and a pressure at the end of the reactor tube of 0.1 MPa (absolute) at an air flow rate of 1.0 m / s was calculated. The flow rate is based on an empty reactor tube so that for each example, the same amount of air was passed. The numerical calculations were performed using the thermodynamic and transport properties of air as specified in the recognized scientific literature. The pressure drop is expressed in Pa / m. A low pressure drop is advantageous because it has a lower gas pressure at the top of the reactor tube and therefore also a lower energy requirement for pressing the gas through the reactor tube.
[0310] Examples 1-5 relate to comparative and inventive dimensions for the oxidation of n-butane to maleic anhydride and Examples 6-10 relate to comparative and inventive dimensions for the oxidation of propylene to acrolein and acrylic acid.
[0311] Example 1 (comparative)
[0312] Example 1 relates to a 6.5×5.0×3.5 annular body having an outer diameter of 6.5 mm, an inner hole of 3.5 mm diameter and a height of 5.0 mm, which is a typical shape and size for a VPO catalyst. It has been mentioned above as a starting point for the simulations of Examples 1-5. The performance of this type of annular body was simulated as described above and summarized in Figure 6 middle.
[0313] The catalyst body of the prior art has a characteristic length V / SA of 0.57 mm, which is a rather high value and indicates that the volume V is rather high compared to the surface area SA. The simulation of the side crushing strength SCS shows a value of 22.3 N and 0.191 N / mm 3 Side crushing strength / body volume SCS / V. <0.2N / mm 3 An SCS / V value of 1.5 indicates a higher risk of breakage during filling of the reaction tube and is therefore not a preferred value. Figure 7 The visualized catalyst bed in a 21 mm reactor tube is shown in Figure 1. The simulated geometry resulted in a 354 kg / m 3 The packing density is a good value. The surface area SA / filling volume is 616m 2 / m 3 , which is a feasible value. In the case of this simulated catalyst bed, the pressure drop at an air flow rate of 1.0 m / s at 20°C and a pressure at the end of the reactor tube of 0.1 MPa (absolute) was calculated. It is 1080 Pa / m. Although this is a feasible value, a pressure drop of <1000 Pa / m would be more advantageous.
[0314] Example 2 (Comparative)
[0315] Example 2 relates to a 5.5x3.0x3.0 annular body with an outer diameter of 5.5 mm, an inner hole with a diameter of 3.0 mm and a height of 3.0 mm. It is obtained from the 6.5x5.0x3.5 annular body of Example 1 by reducing the outer diameter from 6.5 mm to 5.5 mm while keeping the ratio of the outer diameter d0 to the inner diameter d1 of the hole constant. By this reduction, the overall height h0 is also reduced from 5.0 mm to 3.0 mm, which is a common height for a 5.5 mm annular body. Due to its classic annular shape, this catalyst shaped body is also prior art. The performance of these annular bodies is simulated as described above and summarized in Figure 6 middle.
[0316] The shaped catalyst body has a characteristic length V / SA of 0.44 mm, which is significantly lower than the annular body of Example 1 and is an advantageously low value in absolute terms. This indicates that the surface area SA is quite high compared to the volume V. The simulation of the side crushing strength SCS shows values of 12.3 N and 0.247 N / mm 3 Side crushing strength / bulk volume SCS / V. This indicates a fairly stable shaped body with a low risk of crushing during filling of the reaction tube. Figure 7 The visualized catalyst bed in a 21 mm reaction tube is shown in Figure 1. Compared to the visualized catalyst bed of the shaped body of Example 1, it is much denser. The simulated geometric arrangement results in 381 kg / m 3 The packing density is a good value. The surface area SA / filling volume is 865m 2 / m 3 , which is a high value. In the case of this simulated catalyst bed, the pressure drop at an air flow rate of 1.0 m / s at 20°C and a pressure at the end of the reactor tube of 0.1 MPa (absolute) was calculated. It is a very high value of 2174 Pa / m.
[0317] Although the characteristic length, side crush strength / bulk volume and packing density are favorable, this high pressure drop is technically and energetically very disadvantageous. The target pressure drop is <1000 Pa / m.
[0318] Example 3 (Comparative)
[0319] Example 3 relates to a trilobate with three continuous holes and two flat cover sides. Due to the flat cover, the trilobate relates to the prior art. It is designed so that the characteristic length V / SA is about 0.5 mm, which is well between the characteristic lengths V / SA of the catalyst shaped bodies of Examples 1 and 2. The wall thicknesses d2 and d3 are set to 1.00 mm and the diameter d1 of the inner hole is set to 2.00 mm. Both of these values are significantly lower than the values of the annular bodies of Examples 1 and 2. This reduction is required to keep the outer diameter d0 at a value that is still suitable for filling a 21 mm tube. At the above values of d1, d2 and d3, the outer diameter d0 is 7.5 mm. Compared with the annular bodies of Examples 1 and 2, the significantly lower values of d2 and d3 lead to significantly lower mechanical stability and compared with the annular bodies of Examples 1 and 2, the significantly lower inner hole diameter d1 negatively affects the mass transfer behavior. Therefore, the significantly lower values of d1, d2 and d3 will negatively affect the comparability of the annular bodies of Examples 1 and 2 with the trilobate of this Example 3. Based on the fixed values of d1, d2, d3 and a characteristic length V / SA of about 0.5 mm, the total height h0 is 9.2 mm.
[0320] The shaped catalyst body had a characteristic length V / SA of 0.51 mm, which lies well between the characteristic lengths V / SA of the shaped catalyst bodies of Examples 1 and 2. The simulation of the side crushing strength SCS showed high values of 57.1 N and 0.264 N / mm 3 This indicates a stable shaped body with a low risk of crushing during filling of the reaction tube. Figure 7 The visualized catalyst bed in a 21 mm reactor tube is shown in Figure 1. It is significantly less dense than the catalyst bed of the small annulus of Example 2 and is also visibly less dense than the catalyst bed of the annulus of Example 1. Due to the relatively high total length of 9.2 mm, the visualized catalyst bed shows some areas of free space. This free space area is disadvantageous because it represents unused volume in the reactor tube. In addition, this free space area may contribute to the escape of unreacted educts from the reactor outlet. The simulated geometric arrangement results in only 304 kg / m 3 This is a relatively low value and underscores the unfavorable conclusion of the visualized catalyst bed. The surface area SA / packing volume is only 596 m 2 / m 3 , which is very low. In the case of this simulated catalyst bed, the pressure drop at an air flow rate of 1.0 m / s at 20°C and a pressure at the end of the reactor tube of 0.1 MPa (absolute) was calculated. It is 612.1 Pa / m, which is a very low value and which is completely consistent with a loosely packed catalyst bed.
[0321] Although the characteristic length, side crush strength / bulk volume and very low pressure drop are advantageous, the low packing density clearly indicates that the total amount of catalytically active material is only low and the volume of the reactor tube is not optimally utilized. In practice, this requires larger reactors with larger reaction volumes.
[0322] Embodiment 4 (present invention)
[0323] Example 4 relates to a trilobate according to the invention with three continuous holes and an outwardly curved arch on both cover sides. The purpose of Example 4 is to take the comparative trilobate of Example 3 as a basis and implement an outwardly curved arch, which is necessary for the catalyst body of the invention, in order to confirm the advantages of the invention. After the trilobate of comparative Example 3, the design of the trilobate according to the invention of Example 4 also makes the characteristic length V / SA about 0.5 mm. The wall thickness d2 and d3 and the inner hole diameter d1 are also the same as in Example 3, i.e., the two wall thicknesses d2 and d3 are 1.00 mm and the inner hole diameter is 2.00. Therefore, the outer diameter d0 is also 7.5 mm. For Example 4, two hemispheres with a diameter of 7.5 mm have been used as two outwardly curved arches, and their height has been tamped from 3.75 mm of the overall hemisphere to 0.45 mm. Therefore, h2 and h3 are both 0.45 mm. Then h1 is calculated so that the characteristic length V / SA obtained is 0.50 mm. The corresponding value for d1 is 6.60 mm, which results in an overall height d0 of only 7.5 mm.
[0324] The catalyst shaped body of Example 4 according to the invention has a characteristic length V / SA of 0.50 mm, which is approximately the same as the comparative trilobate of Example 3. The simulation of the side crushing strength SCS shows a value of 46.7 N and 0.273 N / mm 3 This indicates a stable shaped body with a low risk of crushing during filling of the reaction tube. Figure 7 The visualized catalyst bed in a 21 mm reaction tube is shown in Figure 3. Compared to the visualized catalyst bed of the comparative trilobate of Example 3, the packing is more regular and there are fewer areas of open space. This is due in particular to the lower overall height. The simulated geometric arrangement results in a packing density of only 322 kg / m 3 , which is about 6% higher than the density of the comparative trilobes of Example 3. The surface area SA / filling volume is 648 m 2 / m 3 , which is a very suitable value. In the case of this simulated catalyst bed, the pressure drop at an air flow rate of 1.0 m / s at 20° C. and a pressure at the end of the reactor tube of 0.1 MPa (absolute) was calculated. It is 779.9 Pa / m, which is higher than the comparative trilobate of Example 3, but still significantly lower than 1000 Pa / m.
[0325] Looking at the overall and evaluation of the characteristic length, side crushing strength / body volume, packing density and pressure drop of the inventive trilobes of Example 4, the values are overall superior to those of the comparative annular bodies of Examples 1 and 2 and the comparative trilobes of Example 3. This is related to the fact that the comparative annular bodies of Examples 1 and 2 are disadvantageous mainly due to their high pressure drop of >1000 Pa / m, and the comparative trilobes of Example 3 are disadvantageous mainly due to their low packing density and their unfavorable geometric arrangement in the reaction tube, although their pressure drop is even lower than that of the inventive trilobes of Example 4. Compared with Examples 1, 2 and 3, the inventive trilobes of Example 4 avoid all these disadvantages and show well-balanced overall characteristics.
[0326] Embodiment 5 (present invention)
[0327] Example 5 relates to another trilobate according to the invention with three continuous holes and outwardly curved arches on both cover sides. Like the trilobate according to the invention of Example 4, it is also based on a characteristic length V / SA of 0.50 mm, a wall thickness d2 and d3 of 1.00 mm and an inner hole diameter d1 of 2.00 mm. Therefore, the outer diameter d0 is also 7.5 mm. The trilobate of Example 5 differs from Example 4 in the shape and size of its outwardly curved arches. For Example 5, two circular parts with a height of 1.00 mm are used as two outwardly curved arches. Therefore, h2 and h3 are both 1.00 mm. h1 is then calculated so that a characteristic length V / SA of 0.50 mm is obtained. The corresponding value for d1 is 5.50 mm, which finally involves a total height d0 of only 7.5 mm.
[0328] The catalyst shaped body of Example 5 according to the invention has a characteristic length V / SA of 0.50 mm, which is approximately the same as the comparative trilobate of Example 3 and completely identical to the trilobate according to the invention of Example 4. The simulation of the side crushing strength SCS shows a value of 48.1 N and 0.292 N / mm 3 This indicates a stable shaped body with a low risk of crushing during filling of the reaction tube. Figure 7 The visualized catalyst bed in a 21 mm reaction tube is shown in Figure 1. The visualized catalyst bed looks similar to Example 4 according to the invention and is more regularly packed with fewer areas of open space than Comparative Example 3. This is due in particular to the lower overall height. The simulated geometric arrangement results in a packing density of only 330 kg / m 3 , which is about 9% higher than the comparative trilobate of Example 3. The surface area SA / filling volume is 653 m 2 / m 3, which is a very suitable value. In the case of this simulated catalyst bed, the pressure drop at an air flow rate of 1.0 m / s at 20° C. and a pressure at the end of the reactor tube of 0.1 MPa (absolute) was calculated. It is 870.5 Pa / m, which is higher than the comparative trilobate of Example 3 and the trilobate of the invention of Example 4, but still significantly lower than 1000 Pa / m.
[0329] The overall view and evaluation of the characteristic length, side crush strength / body volume, packing density and pressure drop of the inventive trilobes of Example 5 lead to the same conclusions as those of Example 4. The corresponding values of the inventive trilobes of Example 5 are also generally better than those of the comparative annular bodies of Examples 1 and 2 and the comparative trilobes of Example 3.
[0330] Figure 8 The results of Examples 1-5 are summarized in an illustrative overview, where each result for the four criteria characteristic length, side crush strength / body volume, packing density and pressure drop is rated by "-" (unfavorable), "o" (neutral) and "+" (favorable). This shows that the inventive trilobes of Examples 4 and 5 with three continuous holes and outwardly curved arches on both cover sides are favorable in all four criteria, while the comparative shapes of Examples 1, 2 and 3 have at least one unfavorable criterion.
[0331] Example 6 (Comparative)
[0332] Example 6 relates to a 5.0 x 5.0 x 2.0 annular body with an outer diameter of 5.0 mm, an inner hole with a diameter of 2.0 mm and a height of 5.0 mm, which is a typical shape and size of a Mo, Fe and Bi multimetallic oxide catalyst. It has been mentioned above as a starting point for the simulations of Examples 6-10. The performance of such annular bodies has been simulated as described above and is summarized in Fig. 9 Like Examples 1-5, Examples 6-10 also show a visualized catalyst bed and an illustrative overview: Fig.10 Visualizing the catalyst bed in the 26 mm reactor tube Fig.11 An illustrative overview of .
[0333] Although the characteristic length V / SA, the packing density and the surface area SA / packing volume show good values, the side crushing strength / tablet volume SCS / V is not excellent but at least acceptable. However, the pressure drop at an air flow rate of 1.0 m / s at 20° C. and a pressure at the end of the reactor tube of 0.1 MPa (absolute) is very high. Overall, the comparative annular body is very disadvantageous due to its very high pressure drop.
[0334] Example 7 (Comparative)
[0335] Example 7 involves a 8.0x7.5x1.5 trilobate with three continuous holes, d2 and d3 values of 1.5 mm and two flat cover sides. It is based on a typical prior art catalyst size design for a 26 mm reactor tube for oxidation of propylene to acrolein or acrylic acid.
[0336] Compared with the annular body of Example 6, the pressure drop at an air flow rate of 1.0 m / s at 20° C. and a pressure at the end of the reactor tube of 0.1 MPa (absolute) is only about one third of that of the annular body and is very low. The characteristic length V / SA also shows good values, and the side crushing strength / tablet volume SCS / V and the surface area SA / filling volume are also acceptable. However, the packing density is very low. Overall, the comparative trilobal body is very disadvantageous due to its very low packing density.
[0337] Embodiment 8 (present invention)
[0338] Example 8 shows the very advantageous effect of the outwardly curved arches at the two cover sides of the trilobate with three continuous holes. Its outer dimensions d0 and h0 are the same as those of the comparative trilobate of Example 7, i.e. d0 is 8.0 mm and h0 is 7.5 mm, and the diameter d1 of the three inner holes and the wall thicknesses d2 and d3 are also the same, i.e. d1, d2 and d3 are 1.5 mm. The inventive trilobate of Example 8 differs from the comparative trilobate of Example 7 only in having two outwardly curved arches with heights h2 and h3 of 0.6 mm on the two cover sides.
[0339] The simulations clearly show that the characteristic length V / SA, the packing density, the surface area SA / packing volume and the pressure drop at an air flow rate of 1.0 m / s at 20° C. and a pressure at the end of the reactor tube of 0.1 MPa (absolute) are all very favorable, and even the side crushing strength / tablet volume SCS / V is still acceptable. Overall, the trilobate of the invention is very advantageous, since most of all five important values are very favorable, but at least acceptable, and none of the five values are unfavorable.
[0340] Example 9 (Comparative)
[0341] Example 9 is a variation of Comparative Example 7, wherein the outer diameter d0 is increased from 8.0 mm to 8.3 mm, the overall height h0 is increased from 7.5 mm to 7.8 mm and the values of d2 and d3 are increased from 1.50 mm to 1.83 mm.
[0342] The increase in wall thickness d2 and d3 leads to an increase in the side crushing strength / tablet volume SCS / V. The pressure drop at an air flow rate of 1.0 m / s at 20°C and a pressure at the end of the reactor tube of 0.1 MPa (absolute) is still a very low value and is actually lower than that in Example 7, and the characteristic length V / SA increases from 0.71 mm to 0.86 mm, which is still an acceptable value for this trilobate size. However, the packing density is still very low and the surface area SA / packing volume increases from 580 m 2 / m 3 Significantly reduced to only 505m 2 / m 3 , which is very low. Overall, the comparison with the trilobite is very unfavorable due to its very low packing density and very low surface area SA / packing volume.
[0343] Embodiment 10 (present invention)
[0344] Example 10 shows the very advantageous effect of the outwardly curved arches at the two cover sides of the trilobate with three continuous holes. Its outer dimensions d0 and h0 are the same as those of the comparative trilobate of Example 9, i.e. d0 is 8.3 mm and h0 is 7.8 mm, and its wall thicknesses d2 and d3 are also the same as those of the comparative trilobate of Example 9, i.e. 1.83. The trilobate of the invention of Example 10 differs from the comparative trilobate of Example 9 in having a smaller inner hole with a diameter of only 1.2 mm instead of 1.5 mm and in having two outwardly curved arches with a height h2 and h3 of 0.35 mm on both cover sides.
[0345] The simulations clearly show that the side crushing strength / tablet volume SCS / V, the packing density and the pressure drop at an air flow rate of 1.0 m / s at 20° C. and a pressure at the end of the reactor tube of 0.1 MPa (absolute) are all very favorable, and even the characteristic length V / SA and the surface area SA / packing volume are still acceptable. Overall, the trilobate of the invention is very advantageous, because most of all five important values are very favorable, but at least acceptable, and none of the five values are unfavorable. BRIEF DESCRIPTION OF THE DRAWINGS
[0346] Figure 1 shows a general cross section of a shaped catalyst body (according to the invention);
[0347] Figure 2 The shape of the arch curving outwards is shown (the present invention);
[0348] Figure 3 The shape of the arch curving outwards is shown (the present invention);
[0349] Figure 4 The shape of the notch of the trilobal structure is shown (present invention);
[0350] Figure 5 A shaped catalyst body (according to the invention) is shown;
[0351] Figure 6 The properties of the catalyst shaped bodies are shown (Examples 1-5);
[0352] Figure 7 Simulated packed beds in 21 mm tubes are shown (Examples 1-5);
[0353] Figure 8 An evaluation of the results of Examples 1-5 is shown;
[0354] Fig. 9 The properties of the catalyst shaped bodies are shown (Examples 6-10);
[0355] Fig.10 Simulated packed beds in 26 mm tubes are shown (Examples 6-10);
[0356] Fig.11 An evaluation of the results of Examples 6-10 is shown.
Claims
1. A shaped catalyst body for heterogeneous catalytic reactions of organic compounds in the gas phase in a fixed bed reactor, wherein the shaped catalyst body is characterized by: (a) contains at least one element from Groups 3 to 12 of the Periodic Table of the Elements, wherein the total amount of elements from Groups 3 to 12 of the Periodic Table of the Elements is 0.01 to 85% by weight; (b) a cylindrical structure having a top cover (A), a bottom cover (B) and a side surface (C), wherein the side surface (C) has three notches extending in the periphery of the cylinder along the height of the cylinder, forming a trilobal structure; (c) Three continuous substantially circular holes extending from one cover side to the other cover side as void spaces with a diameter d 1 And the d of each hole 1 a tolerance of 15% based on the shortest diameter of the corresponding holes, wherein each hole is assigned to a blade and wherein the center points of the three holes are arranged substantially equidistantly in a horizontal section of the cylindrical structure with a tolerance of 15% based on the shortest distance between two center points of two holes; in (d) The wall thickness d between two consecutive holes at the imaginary connecting line between the center points of the two consecutive holes on the horizontal cross section of the cylindrical structure 2 For all three the wall between two consecutive holes is essentially the same, where d 2 The tolerance is based on a minimum wall thickness of 15%; (e) For each of the three blades, the wall thickness d between the continuous hole and the side surface 3 is substantially constant within the corresponding section within the 180° section and is substantially the same for all three sections of the three blades, where d 3 The tolerance is based on a minimum wall thickness of 15%, and the 180° portion is defined as the portion on the horizontal cross section of the cylindrical structure, whose chord is parallel to the imaginary connecting line between the two center points of two adjacent consecutive holes; (f) Three wall thicknesses d 2 Each of the three wall thicknesses d 3x The ratio of each of them is 0.9-1.1, where d 3x is the wall thickness on a horizontal section of the cylindrical structure located at the extension of an imaginary connecting line between the center point of the cylinder and the center points of the consecutive holes of the corresponding blade; (g) The top cover (A) and the bottom cover (B) have an outwardly curved arched body with a maximum height h relative to the top cover (A). 2 and the maximum height h for the bottom cover (B) 3 ,in h 2 is the distance between: - an imaginary flat top region of an imaginary circular cylinder (D) comprising a circular side surface, said circular side surface just surrounding three blades of the shaped catalyst body, whereby the imaginary flat top region contacts the circular side surface at a right angle at the highest level at which the circular side surface of the imaginary circular cylinder (D) just contacts at least one blade; and - the highest height of the tectum (A) above the imaginary plane tectum area, measured perpendicular to the imaginary plane tectum area; h 3 is the distance between: - an imaginary flat bottom cover region of an imaginary circular cylinder (D) comprising a circular side surface, said circular side surface just surrounding the three vanes of the shaped catalyst body, whereby the imaginary flat bottom cover region contacts the circular side surface at a right angle at the lowest horizontal position where the circular side surface of the imaginary circular cylinder (D) just contacts at least one vane; and - the maximum height of the base cap (B) above the imaginary plane base cap area, measured perpendicular to the imaginary plane base cap area; and The imaginary circular cylinder (D) has a height h measured as the distance between the imaginary planar top cover area and the imaginary planar bottom cover area. 1 ;and (h) diameter d 1 Independently of each other, 1-5 mm, wall thickness d 2 and d 3 Independently of each other, 0.5-3 mm, height h 2 and h 3 Independently of each other, the height h is 0.2-3 mm. 1 2-10mm.
2. The shaped catalyst body according to claim 1, wherein it contains at least one element selected from the group consisting of V, Nb, Mo, Fe, Co, Ni, Pd, Pt, Cu, Ag and Zn.
3. The shaped catalyst body according to claim 1, wherein it contains an oxidic material comprising vanadium and phosphorus.
4. The shaped catalyst body according to claim 2, wherein it contains an oxidic material comprising vanadium and phosphorus.
5. The shaped catalyst body according to claim 1, wherein at least one of the two outwardly curved domes has a convex shape on the corresponding cover.
6. The shaped catalyst body according to claim 2, wherein at least one of the two outwardly curved domes has a convex shape on the corresponding cover.
7. The shaped catalyst body according to claim 3, wherein at least one of the two outwardly curved domes has a convex shape on the corresponding cover.
8. The shaped catalyst body according to claim 4, wherein at least one of the two outwardly curved domes has a convex shape on the corresponding cover.
9. The shaped catalyst body according to claim 1, wherein at least one of the two outwardly curved domes has a compressed semicircular shape on the corresponding cover.
10. The shaped catalyst body according to claim 2, wherein at least one of the two outwardly curved domes has a compressed semicircular shape on the corresponding cover.
11. The shaped catalyst body according to claim 3, wherein at least one of the two outwardly curved domes has a compressed semicircular shape on the corresponding cover.
12. The shaped catalyst body according to claim 4, wherein at least one of the two outwardly curved domes has a compressed semicircular shape on the corresponding cover.
13. The catalyst shaped body according to any one of claims 1 to 12, wherein the inner angles α at the edges where the side surfaces of the imaginary circular cylinder (D) contact the outwardly curved arched bodies of the top cover (A) and the outwardly curved arched bodies of the bottom cover (B) are independently 120 to 160°.
14. The shaped catalyst body according to any one of claims 1 to 12, wherein the outer diameter d 0 The outer diameter is 5 to 15 mm, the outer diameter is the diameter of the smallest circle, the circle just surrounds the catalyst body in a horizontal section, and the total height h 0 is 4 to 12 mm, the total height is h 1 、h 2 and h 3 sum.
15. The shaped catalyst body according to claim 13, wherein the outer diameter d 0 The outer diameter is 5 to 15 mm, the outer diameter is the diameter of the smallest circle, the circle just surrounds the catalyst body in a horizontal section, and the total height h 0 is 4 to 12 mm, the total height is h 1 、h 2 and h 3 sum.
16. The shaped catalyst body according to any one of claims 1 to 12, wherein an inner area of a recess of a side surface between two adjacent blades is at least partially filled with an oxidic material of at least one element from Groups 3 to 12 of the Periodic Table of Elements, the inner area being defined as an area between imaginary vertical lines in which a chord of an imaginary 180° section intersects the side surface of the blade, wherein the 180° section is defined as a portion on a horizontal cross section of a cylindrical structure whose chord is parallel to an imaginary connecting line between two center points of two adjacent continuous holes.
17. The catalyst shaped body according to claim 15, wherein an inner area of the recess of the side surface between two adjacent blades is at least partially filled with an oxidic material of at least one element from Groups 3 to 12 of the Periodic Table of Elements, the inner area being defined as an area between imaginary vertical lines in which a chord line of an imaginary 180° section intersects the side surface of the blade, wherein the 180° section is defined as a portion on a horizontal cross section of a cylindrical structure whose chord is parallel to an imaginary connecting line between two center points of two adjacent continuous holes.
18. The catalyst shaped body according to claim 16, wherein the filling of the recess at the side surface has a concave shape.
19. The catalyst shaped body according to claim 17, wherein the filling of the recess at the side surface has a concave shape.
20. A method for preparing a shaped catalyst body according to any one of claims 1 to 19, comprising (a) preparing a powdery or granular precursor material containing at least one element from Groups 3 to 12 of the Periodic Table of the Elements, and (b) compacting it into a catalyst shaped body.
21. The process according to claim 20, wherein the shaped catalyst body containing vanadium and phosphorus oxides is prepared by: (a) reacting a pentavalent vanadium compound and a pentavalent or trivalent phosphorus compound with an organic reducing agent, separating the resulting vanadium and phosphorus-containing precursor, drying it, and converting the dried substance into a powdery or granular precursor material, and (b) compacting it into a catalyst shaped body.
22. A reactor tube filled with ≥ 100 particles of the shaped catalyst body according to any one of claims 1 to 19.
23. A process for producing oxidized organic compounds by heterogeneously catalyzed gas-phase oxidation of organic compounds in the presence of an oxygen-containing gas and a shaped catalyst body as claimed in any one of claims 1 to 19.
24. A process according to claim 23, wherein the oxidic organic compound is maleic anhydride, the organic compound is n-butane and the shaped catalyst body comprises an oxidic material comprising vanadium and phosphorus.
25. The process according to claim 23, wherein the oxidized organic compound is acrolein, acrylic acid, acrylonitrile, methacrolein or methacrylonitrile, the organic compound is propylene or isobutylene, and the shaped catalyst body contains an oxidized material comprising Mo, Fe and Bi.