A nano-phthalocyanine and its preparation method and application
By using volatile organic solvents and acid ultrasonic treatment in phthalocyanine molecules, the problems of phthalocyanine's insolubility and aggregation and precipitation are solved, and nanosized phthalocyanine with high stability and good dispersion is prepared, which significantly improves its phototherapy effect. And avoids toxic side effects and production complexity, providing a safer and more efficient drug form.
Patent Information
- Application Number
- CN202211162329.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-23
AI Technical Summary
The insolubility and aggregation and precipitation problems of phthalocyanine molecules limit their feasibility in pharmaceutical applications. Existing methods such as using surfactants or chemical covalent modifications have toxic side effects or are complicated and cumbersome, affecting efficacy and cost.
By using volatile organic solvents and acids to disperse and ultrasonic treat phthalocyanine, nanometer phthalocyanine is formed, which avoids aggregation, precipitation and complex modification, and prepares nanometer phthalocyanine with high stability and good dispersion.
It achieves good stability and dispersion of phthalocyanine, significantly improves its phototherapy effect, avoids toxic side effects and increases in production costs, and provides a safer and more efficient drug form.
Smart Images

Figure HDA0003860632060000011 
Figure HDA0003860632060000012 
Figure HDA0003860632060000013
Abstract
Description
Technical Field
[0001] The invention relates to the field of medicine, and in particular to nano-phthalocyanine and a preparation method and application thereof. Background Art
[0002] Phthalocyanine is a drug molecule that can be used in phototherapy. It is widely used in photodynamic therapy because of its excellent photodynamic activity, small side effects and long absorption wavelength. Studies in recent years have shown that phthalocyanine molecules also have good photothermal effects and are used in the study of photothermal therapy, showing broad application prospects. At present, many phthalocyanine molecules have been used in clinical practice. For example, Pc4 in the United States and Photosense in Russia have both been clinically tested; my country's "Forskin" is also in phase II clinical trials, showing strong application prospects. However, due to its planar structure and large π conjugated system, phthalocyanine is easy to aggregate and cause precipitation. This insoluble property seriously hinders the efficacy and application of phthalocyanine as a drug. Phthalocyanine molecules themselves have very poor water solubility and very limited solubility in organic solvents, which greatly affects their applicability and seriously hinders their development as therapeutic drugs.
[0003] Many researchers promote the dissolution of phthalocyanine molecules in water by adding surfactants, such as adding surfactants such as Tween, polyoxyethylene castor oil, and sodium dodecyl sulfate, but these surfactants have certain toxic side effects on the human body, which has an adverse effect on the therapeutic effect. Some researchers use carrier materials to load phthalocyanine molecules, which helps the dispersibility of phthalocyanine molecules to a certain extent. However, these carrier materials have no pharmacological activity, and for phthalocyanine molecules that are extremely difficult to dissolve in organic solvents, this method still cannot be effectively carried out. In addition, many studies use hydrophilic groups to modify the structure of phthalocyanine molecules, such as carboxylic acid groups, sulfonic acid groups, quaternary ammonium salt groups, polyethylene glycol groups, etc., which increase the water solubility of phthalocyanine molecules to a certain extent. However, this covalent modification process is complicated and cumbersome, which greatly increases the production cost of phthalocyanine molecules. Moreover, covalent modification changes the structure of the original phthalocyanine molecules, which may have a greater impact on their medicinal activity. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a nano-phthalocyanine and a preparation method and application thereof. The present invention nano-sizes the poorly soluble phthalocyanine molecules, avoids the aggregation and precipitation of the poorly soluble phthalocyanine molecules, avoids the use of surfactants and drug carrier materials, and avoids complex and tedious chemical covalent modification.
[0005] The present invention first provides a method for preparing nano-phthalocyanine, comprising the following steps:
[0006] (1) dispersing phthalocyanine solid powder with a volatile organic solvent, then adding an acid and stirring to obtain a phthalocyanine solution;
[0007] (2) dropping the phthalocyanine solution into water under ultrasonic conditions, and stirring after ultrasonication, and the resulting precipitate is the nano-phthalocyanine.
[0008] In the above preparation method, the volatile organic solvent is at least one of dichloromethane, ethyl acetate, chloroform, toluene, n-hexane, n-heptane, pentane and benzene;
[0009] The phthalocyanine is at least one of copper phthalocyanine, zinc phthalocyanine and pyridyl-substituted zinc phthalocyanine;
[0010] The volume ratio of the organic solvent to the mass ratio of the phthalocyanine solid powder is 1 mL:0.5-5 mg; specifically, it can be 1 mL:0.5 mg or 1 mL:0.75 mg.
[0011] The acid is at least one of trifluoroacetic acid, trichloroacetic acid, trinitrobenzenesulfonic acid and picric acid;
[0012] The content of the acid in the organic solvent is 50-150 mg / mL; specifically, it may be 75 mg / mL or 87 mg / mL.
[0013] In the above-mentioned preparation method, in step (1), the stirring speed is 1000 to 4000 rpm and the stirring time is 10 to 30 min.
[0014] In the above-mentioned preparation method, in step (2), the volume ratio of the phthalocyanine solution to water is 1:5 to 10, and can be specifically 1:5.
[0015] In step (2), the power of the ultrasound is 10 to 40 kHz, and can be specifically 20 kHz;
[0016] In the step of stirring after ultrasonication, the ultrasonication time is 10 to 30 minutes; the stirring speed is 1000 to 4000 revolutions per minute, and the stirring time is 2 to 4 hours.
[0017] In the above-mentioned preparation method, in step (2), there is also a step of washing the precipitate; specifically, the washing is performed with water for 2 to 5 times.
[0018] After the stirring, the precipitate is separated by centrifugation.
[0019] After the washing, the precipitate is resuspended in water to obtain a nano-phthalocyanine suspension, which is the nano-phthalocyanine.
[0020] In the step of resuspending the precipitate, there is no limit to the amount of water added; the resuspending is performed for storage and transportation.
[0021] The invention also provides nano-phthalocyanine prepared by the above preparation method.
[0022] The application of the above-mentioned nano-phthalocyanine in the preparation of phototherapy drugs also falls within the protection scope of the present invention.
[0023] The present invention has the following beneficial effects:
[0024] (1) The present invention nanosizes the poorly soluble phthalocyanine molecules, thereby avoiding the aggregation and precipitation of the poorly soluble phthalocyanine molecules, avoiding the use of surfactants and drug carrier materials, and avoiding complex and cumbersome chemical covalent modification;
[0025] (2) The nano-phthalocyanine prepared by the method of the present invention has good stability and dispersibility, as well as significant phototherapy effect, which provides theoretical and practical significance for the application and development of phthalocyanine photosensitizers. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The particle size (A) and potential (B) of nano-sized copper phthalocyanine prepared in Example 1.
[0027] Figure 2 The curve of PDI (A) and particle size change (B) of the nano-copper phthalocyanine suspension prepared in Example 1 during four weeks of storage.
[0028] Figure 3 The curve of the change of nano-copper phthalocyanine DCF prepared in Example 1 with the illumination time (with DCFH as the ROS indicator) (A) and the curve of the change of the temperature of the nano-copper phthalocyanine suspension with the illumination time (B).
[0029] Figure 4 The growth inhibition curve of HepG2 cells prepared by nano-phthalocyanine copper in Example 1 under illumination (A) and the apoptosis of HepG2 cells analyzed by flow cytometry using PI and Annexin V-FITC as apoptosis indicators (B).
[0030] Figure 5 Figure 2 shows the changes in body weight (A) and tumor volume (B) of tumor-bearing mice. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0032] The experimental methods in the following examples are all conventional methods unless otherwise specified.
[0033] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0034] The quantitative tests in the following examples were all repeated three times, and the results were averaged.
[0035] The monosubstituted β-4-pyridyl phthalocyanine zinc in the following examples was synthesized by the laboratory. The synthesis method was based on the literature Zheng K, Liu H, Liu X, et al. Tumor targeting chemo-and photodynamic therapy packaged in albumin for enhanced anti-tumor efficacy [J]. International journal of nanomedicine, 2020, 15: 151-167.
[0036] Example 1
[0037] (1) Copper phthalocyanine was selected as the insoluble phthalocyanine, 1 mg of which was ultrasonically dispersed in 2 mL of dichloromethane at 20 kHz. 150 mg of trifluoroacetic acid was added under rapid stirring (1000 rpm), and stirring was continued for 20 min until the copper phthalocyanine was completely dissolved in the dichloromethane solution.
[0038] (2) Using an ultrasonic instrument, 2 mL of a dichloromethane solution containing copper phthalocyanine was gradually dropped into 10 mL of water under 20 kHz ultrasonic conditions. At the same time, the dichloromethane solution was emulsified into an emulsion in the water.
[0039] (3) The emulsion was subjected to ultrasound for 20 minutes (20 kHz), and then stirred (1000 rpm). After 4 hours, the resulting solution was centrifuged at 14000 rpm to obtain a precipitate of nano-sized copper phthalocyanine.
[0040] (4) resuspending the obtained precipitate with water and centrifuging again to wash the copper phthalocyanine nanoparticle precipitate. After washing three times, suspending with 2 mL of water to obtain a final nano-sized copper phthalocyanine suspension product. The concentration of the obtained nano-sized copper phthalocyanine suspension is 500 μM.
[0041] After the copper phthalocyanine was nano-processed by the method of Example 1 of the present invention, the particle size and potential of the obtained nano-copper phthalocyanine suspension were measured by dynamic light scattering (Malvern Instruments, Malvern, UK). Figure 1 ; Figure 1The results show that its particle size is small, averaging 197nm, and its zeta potential is -11mV, proving that it has good colloidal dispersion properties.
[0042] The nano-copper phthalocyanine suspension obtained in Example 1 was placed at room temperature for 28 days, and the dispersion coefficient PDI and particle size of the nano-copper phthalocyanine were regularly tested by dynamic light scattering. The results are shown in FIG. Figure 2 The results show that it can exist stably in water, and its PDI and particle size basically do not change much, proving that it can still be well dispersed in aqueous solution within one month, and the nanoparticles will not agglomerate and precipitate.
[0043] The ROS generation of the nano-copper phthalocyanine suspension prepared in Example 1 was studied using the ROS probe DCFH. The nano-copper phthalocyanine suspension in which the DCFH probe was dissolved was irradiated with light (680 nm, 100 mW). As the illumination time increased, the fluorescence of DCF gradually increased, proving that the nano-copper phthalocyanine suspension had good ROS generation activity (see Figure 3 A in the figure). The stability of the suspension was tested with a thermometer, and a pure aqueous solution without any reagent was used as a control. The results are shown in Figure 3 B in the figure; The results show that with the extension of illumination time, the temperature of the nano-copper phthalocyanine suspension gradually increases. After 20 minutes of illumination, the temperature of the aqueous solution increased by nearly 30°C, which fully demonstrates its good photothermal performance.
[0044] The phototoxicity of the nano-copper phthalocyanine in Example 1 was detected by MTT method. HepG2 cells were added to a 96-well plate (6000 cells per well), and 20 μL of nano-copper phthalocyanine suspensions of different concentrations were added (final concentrations were 0.01 μM, 0.05 μM, 0.1 μM, 0.5 μM, 1 μM, 5 μM, 10 μM, 50 μM, and 20 μL of deionized water were added to the control group) and 1640 culture medium (containing 10% fetal bovine serum, v / v). After incubation (37° C., 5% carbon dioxide, volume percentage) for 24 hours, fresh culture medium was replaced, and the cells were irradiated with light (680 nm, 1.5 J / cm 2 ), after 24 hours, the survival rate of cells was detected by MTT. Figure 4 . The results showed that it has excellent phototherapy cell killing activity, and its average IC50 value is 4.9μM. In addition, after the HepG2 cells incubated with 2μM nano-copper phthalocyanine suspension were treated with light, the cells were digested and prepared into a cell suspension. PI / Annexin V-FITC probe was added to the suspension. After incubation for 5 minutes, the cell apoptosis was analyzed by flow cytometry. Compared with the control group, the nano-copper phthalocyanine moved significantly to the lower right quadrant, indicating that it can significantly induce cell apoptosis under light conditions.
[0045] 200 μL of 5 million H22 cells were injected into the abdominal cavity of Kunming mice (four weeks old, male, 18-22g, Shanghai Slake Experimental Animal Co., Ltd.). After 7 days, the ascites in the abdominal cavity of the mice was removed, and the ascites was diluted with normal saline. 200 μL of 5 million cells were injected into the subcutaneous part of the back of the mice. After about 5 days, the H22 tumor-bearing mouse model was successfully constructed. After 200 μL of the nano-copper phthalocyanine suspension obtained in Example 1 (concentration of 25 μM) was injected into the H22 tumor-bearing mice through the tail vein, the tumor site was illuminated with 680nm light (500mW, 5min) every day, and the weight and tumor size of the mice were tested every day. The tumor-bearing mice injected with 200 μL of normal saline were used as the control group. The results are shown in Table 1. Figure 5 The results showed that the weight of mice did not change compared with the control group, indicating that nano-copper phthalocyanine did not cause obvious toxic side effects. Monitoring of tumor volume in tumor-bearing mice showed that nano-copper phthalocyanine had a certain activity in inhibiting tumor growth.
[0046] Example 2
[0047] (1) Copper phthalocyanine was selected as the insoluble phthalocyanine, 1 mg of which was ultrasonically dispersed in 2 mL of ethyl acetate at 20 kHz, and 150 mg of trifluoroacetic acid was added thereto under rapid stirring (1000 rpm), and stirring was continued for 20 min until the copper phthalocyanine was completely dissolved in the ethyl acetate solution.
[0048] (2) Using an ultrasonic instrument, under 20 kHz ultrasonic conditions, 2 mL of ethyl acetate solution containing copper phthalocyanine was gradually dropped into 10 mL of water. At the same time, the ethyl acetate solution was emulsified into an emulsion in the water.
[0049] (3) The emulsion was subjected to ultrasound for 20 minutes (20 kHz), and then stirred (1000 rpm). After 4 hours, the resulting solution was centrifuged at 14000 rpm to obtain a precipitate of nano-sized copper phthalocyanine.
[0050] (4) The obtained precipitate is resuspended with water and centrifuged again to wash the copper phthalocyanine nanoparticle precipitate. After washing three times, it is suspended with 2 mL of water to obtain the final nano-sized copper phthalocyanine suspension product.
[0051] Example 3
[0052] (1) Copper phthalocyanine was selected as the insoluble phthalocyanine, 1 mg of which was ultrasonically dispersed in 2 mL of chloroform at 20 kHz, and 174 mg of trichloroacetic acid was added thereto under rapid stirring (1000 rpm), and stirring was continued for 20 min until the copper phthalocyanine was completely dissolved in the chloroform solution.
[0053] (2) Using an ultrasonic instrument, under 20 kHz ultrasonic conditions, 2 mL of chloroform solution containing copper phthalocyanine was gradually dropped into 10 mL of water. At the same time, chloroform was emulsified into an emulsion in the water.
[0054] (3) The emulsion was subjected to ultrasound for 20 minutes (20 kHz), and then stirred (1000 rpm). After 4 hours, the resulting solution was centrifuged at 14000 rpm to obtain a precipitate of nano-sized copper phthalocyanine.
[0055] (4) The obtained precipitate is resuspended with water and centrifuged again to wash the copper phthalocyanine nanoparticle precipitate. After washing three times, it is suspended with 2 mL of water to obtain the final nano-sized copper phthalocyanine suspension product.
[0056] Example 4
[0057] (1) Zinc phthalocyanine was selected as the insoluble phthalocyanine, 1 mg of which was ultrasonically dispersed in 2 mL of chloroform at 20 kHz, and 150 mg of trifluoroacetic acid was added thereto under rapid stirring (1000 rpm), and stirring was continued for 20 min until the zinc phthalocyanine was completely dissolved in the chloroform solution.
[0058] (2) Using an ultrasonic instrument, under 20 kHz ultrasonic conditions, 2 mL of chloroform solution containing zinc phthalocyanine was gradually dropped into 10 mL of water. At the same time, the chloroform solution was emulsified into an emulsion in the water.
[0059] (3) The emulsion was subjected to ultrasound for 20 minutes (20 kHz), and then stirred (1000 rpm). After 4 hours, the resulting solution was centrifuged at 14000 rpm to obtain a precipitate of nano-sized zinc phthalocyanine.
[0060] (4) resuspending the obtained precipitate with water and centrifuging again to wash the zinc phthalocyanine nanoparticle precipitate. After washing three times, suspending with water to obtain the final nano-sized zinc phthalocyanine suspension product.
[0061] Example 5
[0062] (1) Monosubstituted β-4-pyridyl phthalocyanine zinc was selected as the insoluble phthalocyanine, 1.5 mg of which was ultrasonically dispersed in 2 mL of chloroform under 20 kHz conditions, and 150 mg of trifluoroacetic acid was added thereto under rapid stirring conditions (1000 rpm), and stirring was continued for 20 min, so that the monosubstituted β-4-pyridyl phthalocyanine zinc was completely dissolved in the chloroform solution.
[0063] (2) Using an ultrasonic instrument, under 20 kHz ultrasonic conditions, 2 mL of a chloroform solution containing monosubstituted β-4-pyridylphthalocyanine zinc was gradually dropped into 10 mL of water. At the same time, the chloroform solution was emulsified into an emulsion in the water.
[0064] (3) The emulsion was subjected to ultrasound for 20 minutes (20 kHz), and then stirred (1000 rpm). After 4 hours, the resulting solution was centrifuged at 14000 rpm to obtain a precipitate of nano-sized mono-substituted β-4-pyridylphthalocyanine zinc.
[0065] (4) The obtained precipitate is resuspended with water and centrifuged again to wash the mono-substituted β-4-pyridylphthalocyanine zinc nanoparticle precipitate. After washing three times, it is suspended with 2 mL of water to obtain the final nano-sized mono-substituted β-4-pyridylphthalocyanine zinc suspension product.
Claims
1. A method for preparing nano-phthalocyanine, comprising the following steps: (1) dispersing phthalocyanine solid powder with a volatile organic solvent, then adding an acid and stirring to obtain a phthalocyanine solution; The volatile organic solvent is at least one of dichloromethane, ethyl acetate, chloroform, toluene, n-hexane, n-heptane, pentane and benzene; The phthalocyanine is at least one of copper phthalocyanine, zinc phthalocyanine and pyridyl-substituted zinc phthalocyanine; The acid is at least one of trifluoroacetic acid, trichloroacetic acid, trinitrobenzenesulfonic acid and picric acid; The volume ratio of the organic solvent to the mass ratio of the phthalocyanine solid powder is 1 mL: 0.5-5 mg; The content of the acid in the organic solvent is 50-150 mg / mL; (2) dropping the phthalocyanine solution into water under ultrasonic conditions, stirring after ultrasonication, and the resulting precipitate is the nano-phthalocyanine; In step (2), the volume ratio of the phthalocyanine solution to water is 1:5-10.
2. The preparation method according to claim 1, characterized in that: In step (1), the stirring speed is 1000-4000 rpm and the stirring time is 10-30 min.
3. The preparation method according to claim 1 or 2, characterized in that: In step (2), the power of the ultrasound is 10-40 kHz; In the step of stirring after ultrasound, the ultrasound time is 10 to 30 min; the stirring speed is 1000 to 4000 rpm, and the stirring time is 2 to 4 h.
4. The preparation method according to claim 1 or 2, characterized in that: In step (2), there is also a step of washing the precipitate.
5. The preparation method according to claim 4, characterized in that: The washing is performed with water for 2 to 5 times.
6. The preparation method according to claim 4, characterized in that: After the washing, the precipitate is resuspended in water to obtain a nano-phthalocyanine suspension, which is the nano-phthalocyanine.
7. Nano-phthalocyanine prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the nano-phthalocyanine according to claim 7 in the preparation of phototherapy drugs.
Citation Information
Patent Citations
Method for preparing phthalocyanine micro-nano structure
CN103664965A
Phthalocyanine copper dispersion system and preparation method thereof
CN103992328A
Preparation method of nano-microspheres based on zinc phthalocyanine
CN114099700A