A method for testing the expansion rate of silicon-based negative electrode materials
By measuring the thickness change and discharge specific capacity of the silicon-based anode material, the expansion rate is calculated, which solves the problem of cumbersome existing testing methods and achieves fast and accurate expansion rate evaluation.
Patent Information
- Application Number
- CN202211221263.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-08
AI Technical Summary
The existing testing methods for the expansion rate of silicon-based anode materials are cumbersome and costly. They lack rapid testing methods and are difficult to effectively evaluate the expansion rate of silicon-based anode materials.
By cutting, rolling, baking and assembling the battery, the thickness changes of the pole pieces were measured, a standard curve was established based on the discharge specific capacity, and the expansion rate of the silicon-based negative electrode material was calculated using the formula expansion rate = (H2-H1)/(H1-H0 )×100%+(H3-H2)/(H2-H0)×100% for calculation.
It achieves rapid and accurate measurement and prediction of the expansion rate of silicon-based negative electrode materials, provides a basis for studying the expansion rate, and simplifies the testing process.
Smart Images

Figure CN115524377B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a method for testing the expansion rate of a silicon-based negative electrode material. Background Art
[0002] When designing a battery, whether the negative electrode is made of graphite material or silicon-carbon composite material, the negative electrode expansion rate parameter is one of the key parameters in battery design. At the same time, in the development history of negative electrode materials, silicon-based negative electrode materials have entered people's field of vision with their high capacity and low electrode potential, but their discharge process will cause volume expansion, and volume expansion will bring about subsequent cycle capacity attenuation, low coulomb efficiency, poor rate performance and other problems. Therefore, the expansion problem of silicon-based negative electrode materials is a problem that is difficult to solve for silicon-based materials at present, so it is extremely important to analyze the expansion of silicon-based negative electrode materials. And through the test and analysis of the expansion of silicon-based negative electrode materials, the advantages and disadvantages of different silicon-based negative electrode materials can be evaluated through one aspect. Therefore, it is of great significance to establish an analysis method for the expansion of negative electrode materials.
[0003] The existing testing methods are mainly the expansion testing methods of the pole pieces, which are relatively cumbersome and costly. There is no method specifically for the rapid testing of the expansion rate of silicon-based negative electrode materials, nor is there a technology for estimating the expansion rate of silicon-based negative electrode materials based on this method. Therefore, it is urgently needed in the art to provide a testing method that is specific and can quickly analyze the expansion rate of silicon-based negative electrode materials. Summary of the invention
[0004] In view of this, the present invention provides a method for testing the expansion rate of silicon-based negative electrode materials to solve the problem that the existing analysis methods are cumbersome and costly to implement, and there is a gap in the research of proprietary methods for testing the expansion rate of silicon-based negative electrode materials.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The present invention provides a method for testing the expansion rate of a silicon-based negative electrode material, comprising the following steps:
[0007] (1) Cutting, punching and rolling the electrode material made of silicon-based material to obtain the electrode, and measuring the electrode thickness H1 and the current collector thickness H0; baking the electrode, and measuring the thickness H2 of the electrode after baking;
[0008] (2) Assemble the baked electrodes into a battery, activate the battery and test it to a fully charged state, at which the discharge specific capacity is Q;
[0009] (3) Disassemble the fully charged battery to obtain the electrode, clean the electrode, and measure the thickness H3 of the cleaned electrode;
[0010] (4) Calculate the expansion rate of silicon-based negative electrode materials according to formula 1:
[0011] Expansion rate = (H2-H1) / (H1-H0)×100%+(H3-H2) / (H2-H0)×100% Formula 1;
[0012] (5) establishing a standard curve with the discharge specific capacity Q as the horizontal axis and the expansion rate of the silicon-based negative electrode material as the vertical axis; obtaining the expansion rate of the silicon-based negative electrode material of the battery sample to be tested based on the discharge capacity of the battery sample to be tested assembled with electrodes made of silicon-based materials and the standard curve.
[0013] Preferably, the silicon-based material is one or more of a mixed material of graphene and silicon, a mixed material of graphite and silicon oxide, a mixed material of graphite and silicon-carbon, a mixed material of carbon and nanographite, nanosilicon, silicon alloy, carbon-coated silicon, and silicon oxide.
[0014] Preferably, the electrode sheet obtained after cutting and punching is a round sheet with a diameter of 11 to 15 mm; the rolling pressure is 1 to 15 MPa, and the compaction density of the electrode sheet after rolling is 1 to 1.2 g / cm 3 .
[0015] Preferably, the baking temperature is 60-120° C., and the baking time is 2-48 hours.
[0016] Preferably, when the baked pole pieces are assembled into batteries, the number of batteries assembled from pole pieces made of the same silicon-based material is ≥ 2; the discharge specific capacity Q is the average discharge specific capacity.
[0017] Preferably, the cleaning solvent is dimethyl carbonate.
[0018] Preferably, the method for preparing the electrode material made of silicon-based material comprises the following steps:
[0019] a. Mixing a silicon-based material, a conductive agent, a binder, an additive and a solvent to obtain a slurry;
[0020] b. Apply the slurry on the current collector and then dry it to obtain the electrode material.
[0021] Preferably, the conductive agent is one or more of conductive carbon black, conductive graphite, Ketjen black and carbon nanotubes; the binder is an aqueous binder; the additive is carbon nanotubes, chloroprene rubber or N-methylpyrrolidone; and the solvent is water.
[0022] Preferably, the mass ratio of the silicon-based material, the conductive agent, the binder and the additive is 1-3: 0.05-0.4: 1-15: 0-10; the added amount of the solvent is 6-10% of the total mass of the silicon-based material, the conductive agent, the binder and the additive.
[0023] Preferably, the slurry coating thickness is 50 to 200 μm; the drying is vacuum drying, the drying temperature is 80 to 100° C., the drying time is 8 to 24 hours, and the drying vacuum degree is -0.05 to -0.2 MPa.
[0024] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0025] The method for testing the expansion rate of silicon-based negative electrode materials described in the present invention can accurately and quickly measure the expansion rate of silicon-based negative electrode materials, and can also estimate the expansion rate of silicon-based negative electrode materials, laying a foundation for the research on the method for testing the expansion rate of silicon-based negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0027] Figure 1 This is a flow chart of the method for testing the expansion rate of the silicon-based negative electrode material of the present invention;
[0028] Figure 2 A flowchart of the battery assembly described in Examples 1 and 2 of the present invention;
[0029] Figure 3 The figure is a curve diagram of the discharge specific capacity of the battery obtained in Example 1 of the present invention and the expansion rate of the silicon-based negative electrode material;
[0030] Figure 4 The figure is a curve diagram of the discharge specific capacity of the battery obtained in Example 2 of the present invention and the expansion rate of the silicon-based negative electrode material. DETAILED DESCRIPTION
[0031] The present invention provides a method for testing the expansion rate of a silicon-based negative electrode material, comprising the following steps:
[0032] (1) Cutting, punching and rolling the electrode material made of silicon-based material to obtain the electrode, and measuring the electrode thickness H1 and the current collector thickness H0; baking the electrode, and measuring the thickness H2 of the electrode after baking;
[0033] (2) Assemble the baked electrodes into a battery, activate the battery and test it to a fully charged state, at which the discharge specific capacity is Q;
[0034] (3) Disassemble the fully charged battery to obtain the electrode, clean the electrode, and measure the thickness H3 of the cleaned electrode;
[0035] (4) Calculate the expansion rate of silicon-based negative electrode materials according to formula 1:
[0036] Expansion rate = (H2-H1) / (H1-H0)×100%+(H3-H2) / (H2-H0)×100% Formula 1;
[0037] (5) establishing a standard curve with the discharge specific capacity Q as the horizontal axis and the expansion rate of the silicon-based negative electrode material as the vertical axis; obtaining the expansion rate of the silicon-based negative electrode material of the battery sample to be tested based on the discharge capacity of the battery sample to be tested assembled with electrodes made of silicon-based materials and the standard curve.
[0038] In the present invention, the expansion rate calculation method is: total expansion rate = pole piece rebound rate (physical expansion) + full charge expansion rate (chemical expansion). Pole piece rebound rate (physical expansion) = (H2-H1) / (H1-H0)×100%, full charge expansion rate (chemical expansion) = (H3-H2) / (H2-H0)×100%.
[0039] In the present invention, the silicon-based material is preferably a mixed material of graphene and silicon, a mixed material of graphite and silicon oxide, a mixed material of graphite and silicon-carbon, a mixed material of carbon and nanographite, nanosilicon, silicon alloy, carbon-coated silicon, silicon oxide, and is further preferably one or more of a mixed material of graphene and silicon, a mixed material of graphite and silicon oxide, a mixed material of graphite and silicon-carbon, and a mixed material of carbon and nanographite.
[0040] In the present invention, the pole piece obtained after cutting and punching is a round piece, and the diameter of the round piece is preferably 11-15 mm, more preferably 13-14 mm; the rolling pressure is preferably 1-15 MPa, more preferably 5-10 MPa; the compaction density of the pole piece after rolling is preferably 1-1.2 g / cm 3 , more preferably 1.12 to 1.18 g / cm 3 ;
[0041] The calculation formula of the compaction density of the electrode sheet after rolling is shown in Formula 2:
[0042] The compaction density of the electrode after rolling = 1000×(m-m0) / [(H1-H0)×πr 2 Formula 2
[0043] Where: m is the weighed mass of the negative electrode after cutting and punching, that is, the mass of the electrode before assembling into a battery; m0 is the mass of the blank copper foil after cutting and punching; r is the radius of the electrode. The electrode used in the present invention is a circular piece, so the active material area of the electrode is calculated as πr2 , H0 is the thickness of the current collector, H1 is the thickness of the pole piece;
[0044] The thickness of the electrode sheet after rolling is preferably 60 to 90 μm, and more preferably 70 to 80 μm, without considering rebound.
[0045] The present invention eliminates the influence of initial thickness on the expansion property of silicon-based negative electrode material by controlling the compaction density and thickness, thereby improving the accuracy of the test method.
[0046] In the present invention, the baking temperature is preferably 60 to 120° C., more preferably 80 to 100° C.; the baking time is preferably 2 to 48 hours, more preferably 24 to 40 hours.
[0047] In the present invention, when the baked pole pieces are assembled into batteries, the number of batteries assembled from pole pieces made of the same silicon-based material is preferably ≥2, and more preferably 3 to 4; the discharge specific capacity Q is preferably the average discharge specific capacity.
[0048] In the present invention, the activation stage is preferably 1 to 5 cycles, more preferably 2 to 3 cycles; the fully charged state is: discharging the battery to a fully charged state at a rate of 0.01 to 5C;
[0049] The magnification is preferably 0.02 to 2C, more preferably 0.05 to 0.5C.
[0050] In the present invention, the cleaning solvent is preferably dimethyl carbonate.
[0051] In the present invention, the method for preparing the electrode material made of the silicon-based material comprises the following steps:
[0052] a. Mixing a silicon-based material, a conductive agent, a binder, an additive and a solvent to obtain a slurry;
[0053] b. Apply the slurry on the current collector and then dry it to obtain the electrode material.
[0054] In the present invention, the conductive agent is preferably one or more of conductive carbon black, conductive graphite, Ketjen black and carbon nanotubes, and is further preferably conductive graphite and / or carbon nanotubes; the binder is preferably an aqueous binder, and is further preferably one or more of aqueous binder LA133, aqueous binder LA132 and aqueous binder LA136D; the additive is preferably carbon nanotubes, chloroprene rubber or N-methylpyrrolidone, and is further preferably carbon nanotubes or N-methylpyrrolidone; the solvent is preferably water.
[0055] In the present invention, the mass ratio of the silicon-based material, the conductive agent, the binder and the additive is preferably 1-3: 0.05-0.4: 1-15: 0-10, and more preferably 1.5-2.5: 0.1-0.3: 2-5: 1-8; the amount of the solvent added is preferably 6-10% of the total mass of the silicon-based material, the conductive agent, the binder and the additive, and more preferably 8-9% of the total mass of the silicon-based material, the conductive agent, the binder and the additive.
[0056] In the present invention, the thickness of the slurry coating is preferably 50 to 200 μm, and more preferably 100 to 150 μm; the drying is vacuum drying, and the drying temperature is preferably 80 to 100° C., and more preferably 90 to 95° C.; the drying time is preferably 8 to 24 h, and more preferably 10 to 20 h; the drying vacuum degree is preferably -0.05 to -0.2 MPa, and more preferably -0.08 to -0.15 MPa.
[0057] The present invention assembles button-type batteries by using pole pieces made of different silicon-based negative electrode materials, disassembles the batteries before assembly and in a fully charged state (or in any step of the cycle) and uses a micrometer to measure the required thickness of the components. This method can be used to directly measure the thickness to measure the expansion rate of the silicon-based negative electrode materials during the charging and discharging or cycling of the silicon-based negative electrode, providing a method for quickly testing the expansion rate. At the same time, the expansion rate of the silicon-based negative electrode materials can be obtained by subsequently assembling the materials into button batteries to test the discharge specific capacity.
[0058] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0059] Example 1
[0060] Step 1, preparing silicon-based negative electrode materials: pure silicon carbon (not mixed with graphite), pure silicon carbon mixed with 10% graphite, pure silicon carbon mixed with 20% graphite, pure silicon carbon mixed with 30% graphite, pure silicon carbon mixed with 40% graphite, pure silicon carbon mixed with 50% graphite, pure silicon carbon mixed with 60% graphite, pure silicon carbon mixed with 70% graphite, pure silicon carbon mixed with 80% graphite, pure silicon carbon mixed with 90% graphite;
[0061] Step 2, weigh 2.275 g of the silicon-based material obtained by mixing graphite and silicon-carbon in different proportions in step 1, respectively, and stir and mix with 0.075 g of conductive carbon black SP, 3 g of water-based binder LA132 (concentration of 5%), and 0.5 g of pure water to obtain 10 slurries;
[0062] Step 3, the obtained slurry is evenly coated on the copper foil, dried in a blast oven at 80°C for 8h, rolled after drying, and then cut and punched, and a pole piece with a diameter of 13mm is selected, and the thickness of the pole piece at this time is measured and recorded as H1 and the thickness of the blank copper foil is recorded as H0; wherein H0 and H1 are both average values;
[0063] Among them, the requirements for rolling are: the requirements for the compaction density of the pole piece after rolling: the compaction density of the pole piece after rolling is required to be controlled to 1g / cm 3 ; Requirements for the thickness of the pole piece after rolling: The thickness of the pole piece after rolling is required to be controlled at 60μm (without considering rebound);
[0064] Step 4, placing the electrode into an oven and baking at 80°C for 8 hours. After baking, the electrode is placed into a glove box to measure the thickness of the electrode after baking and record it as H2; wherein H2 is the average value;
[0065] Step 5, repeat the above steps 3 and 4 4 times to obtain 11 groups (4 parallel sample pole pieces in each group) of pole pieces;
[0066] Step 6: Assemble each pole piece into a lithium battery. The assembly steps are as follows:
[0067] Step S01: moving the prepared electrode sheet, ceramic diaphragm, lithium sheet, negative electrode shell, positive electrode shell, spring sheet and gasket into a glove box;
[0068] Step S02: placing the negative electrode shell at the bottom layer, and placing the spring sheet, gasket, and lithium sheet on top in sequence;
[0069] Step S03: adding 0.1 g of lithium hexafluorophosphate electrolyte to the lithium sheet prepared in step S02, placing a ceramic diaphragm, and then adding 0.2 g of lithium hexafluorophosphate electrolyte again, and then placing an electrode sheet and covering the positive electrode shell to complete the assembly of the battery;
[0070] Step S04: placing the battery assembled in step S03 on the card slot of the sealing machine, and obtaining the lithium battery after sealing.
[0071] Step 7, take the lithium battery out of the glove box, activate the battery in the test cabinet, test it to a fully charged state, record the discharge specific capacity Q at this time, and take out the battery and put it into the glove box for disassembly;
[0072] The activation stage is the first two cycles, and then the battery is discharged at a rate of 0.1C until it is fully charged and then removed;
[0073] Step 8, in a glove box, the silicon-based negative electrode obtained after disassembling the battery is cleaned with DMC, and then the electrode is naturally dried and the thickness of the electrode is measured and recorded as H3; wherein H3 is an average value;
[0074] Step 9, the data obtained in the above steps are calculated according to the expansion rate formula (H2-H1) / (H1-H0)×100%+(H3-H2) / (H2-H0)×100% to obtain the result;
[0075] The data obtained in this example are shown in Table 1:
[0076] Table 1 Data of 7 silicon-based materials described in Example 1
[0077]
[0078]
[0079] According to the data in Table 1, with the discharge specific capacity Q as the horizontal coordinate and the corresponding silicon-based negative electrode material expansion rate Y as the vertical coordinate, the curve Q and Y are approximately linearly related. Figure 3 As shown, the relationship between Q and Y is Y = 0.1148Q-22.444; where the linear correlation coefficient R 2 =0.9916, the slope K is 0.1148, that is, Y∝0.1148Q. In the future, using this relationship, we only need to assemble the silicon-based negative electrode material into a button battery to test the discharge specific capacity to quickly estimate the expansion rate of the silicon-based negative electrode material.
[0080] Example 2
[0081] Step 1, preparing silicon-based negative electrode materials: silicon oxide (not mixed with graphite), silicon oxide mixed with 10% graphite, silicon oxide mixed with 20% graphite, silicon oxide mixed with 30% graphite, silicon oxide mixed with 40% graphite, silicon oxide mixed with 50% graphite, silicon oxide mixed with 60% graphite, silicon oxide mixed with 70% graphite, silicon oxide mixed with 80% graphite, silicon oxide mixed with 90% graphite;
[0082] Step 2, weigh 1.875 g of the silicon-based material obtained by mixing graphite and silicon-carbon in different proportions in step 1, respectively, and stir and mix with 0.125 g of conductive carbon black SP, 5 g of water-based binder LA132 (concentration of 5%), 0.25 g of conductive carbon black SFG-6, and 0.5 g of pure water to obtain 11 slurries;
[0083] Step 3, the obtained slurry is evenly coated on the copper foil, dried in a blast oven at 80°C for 8h, rolled after drying, and then cut and punched, and a pole piece with a diameter of 13mm is selected, and the thickness of the pole piece at this time is measured and recorded as H1 and the thickness of the blank copper foil is recorded as H0; wherein H0 and H1 are both average values;
[0084] Among them, the requirements for rolling are: the requirements for the compaction density of the pole piece after rolling: the compaction density of the pole piece after rolling is required to be controlled to 1g / cm 3; Requirements for the thickness of the pole piece after rolling: The thickness of the pole piece after rolling is required to be controlled at 60μm (without considering rebound);
[0085] Step 4, placing the electrode into an oven and baking at 80°C for 8 hours. After baking, the electrode is placed into a glove box to measure the thickness of the electrode after baking and record it as H2; wherein H2 is the average value;
[0086] Step 5, repeat the above steps 3 and 4 4 times to obtain 11 groups (4 parallel sample pole pieces in each group) of pole pieces;
[0087] Step 6: Assemble each pole piece into a lithium battery. The assembly steps are as follows:
[0088] Step S01: moving the prepared electrode sheet, ceramic diaphragm, lithium sheet, negative electrode shell, positive electrode shell, spring sheet and gasket into a glove box;
[0089] Step S02: placing the negative electrode shell at the bottom layer, and placing the spring sheet, gasket, and lithium sheet on top in sequence;
[0090] Step S03: adding 0.1 g of lithium hexafluorophosphate electrolyte to the lithium sheet prepared in step S02, placing a ceramic diaphragm, and then adding 0.2 g of lithium hexafluorophosphate electrolyte again, and then placing an electrode sheet and covering the positive electrode shell to complete the assembly of the battery;
[0091] Step S04: placing the battery assembled in step S03 on the card slot of the sealing machine, and obtaining the lithium battery after sealing.
[0092] Step 7, take the lithium battery out of the glove box, activate the battery in the test cabinet, test it to a fully charged state, record the discharge specific capacity Q at this time, and take out the battery and put it into the glove box for disassembly;
[0093] The activation stage is the first two cycles, and then the battery is discharged at a rate of 0.1C until it is fully charged and then removed;
[0094] Step 8, in a glove box, the silicon-based negative electrode obtained after disassembling the battery is cleaned with DMC, and then the electrode is naturally dried and the thickness of the electrode is measured and recorded as H3; wherein H3 is an average value;
[0095] Step 9, the data obtained in the above steps are calculated according to the expansion rate formula (H2-H1) / (H1-H0)×100%+(H3-H2) / (H2-H0)×100% to obtain the result;
[0096] The data obtained in this example are shown in Table 2:
[0097] Table 2 Data of 7 silicon-based materials described in Example 2
[0098]
[0099]
[0100] According to the data in Table 2, with the discharge specific capacity Q as the horizontal coordinate and the corresponding silicon-based negative electrode material expansion rate Y as the vertical coordinate, the curve Q and Y are approximately linearly related. Figure 4 As shown, the relationship between Q and Y is Y = 0.065Q-8.4085; where the linear correlation coefficient R 2 =0.9972, the slope K is 0.065, that is, Y∝0.065Q. In the future, using this relationship, we only need to assemble the silicon-based negative electrode material into a button battery to test the discharge specific capacity to quickly estimate the expansion rate of the silicon-based negative electrode material.
[0101] It can be seen from Examples 1 and 2 that the testing method of the present invention is simple and quick, and can also quickly estimate the expansion rate of silicon-based negative electrode materials.
[0102] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for testing the expansion rate of a silicon-based negative electrode material, characterized in that: The steps include: (1) Rolling the electrode material made of silicon-based material, cutting and punching the electrode, measuring the electrode thickness H1 and the current collector thickness H0; baking the electrode, and measuring the electrode thickness H2 after baking; (2) Assemble the baked electrodes into a battery, activate the battery and test it to a fully charged state, at which the discharge specific capacity is Q; (3) Disassemble the fully charged battery to obtain the electrode, clean the electrode, and measure the thickness H3 of the cleaned electrode; (4) Calculate the expansion rate of silicon-based negative electrode materials according to formula 1: Expansion rate = (H2-H1) / (H1-H0)×100%+(H3-H2) / (H2-H0)×100% Formula 1; (5) establishing a standard curve with the discharge specific capacity Q as the horizontal axis and the expansion rate of the silicon-based negative electrode material as the vertical axis; obtaining the expansion rate of the silicon-based negative electrode material of the battery sample to be tested according to the discharge capacity of the battery sample to be tested assembled with the electrode pieces made of the silicon-based material and the standard curve; The baking temperature is 60-120°C and the baking time is 2-48h; The rolling pressure is 1-15 MPa, and the compaction density of the electrode after rolling is 1-1.2 g / cm 3 ; The method for preparing the electrode material made of silicon-based material comprises the following steps: a. Mixing a silicon-based material, a conductive agent, a binder, an additive and a solvent to obtain a slurry; b. Applying the slurry on the current collector and drying it to obtain the electrode material; The conductive agent is one or more of conductive carbon black, conductive graphite and carbon nanotubes; the binder is a water-based binder; the additive is carbon nanotubes, chloroprene rubber or N-methylpyrrolidone; and the solvent is water; The mass ratio of the silicon-based material, the conductive agent, the binder and the additive is 1-3: 0.05-0.4: 1-15: 0-10; the added amount of the solvent is 6-10% of the total mass of the silicon-based material, the conductive agent, the binder and the additive.
2. The method for testing the expansion rate of silicon-based negative electrode materials according to claim 1, characterized in that: The silicon-based material is one or more of a mixed material of graphene and silicon, a mixed material of graphite and silicon oxide, a mixed material of graphite and silicon-carbon, nano-silicon, silicon alloy, carbon-coated silicon, and silicon oxide.
3. The method for testing the expansion rate of silicon-based negative electrode materials according to claim 2, characterized in that: The pole piece obtained after cutting and punching is a disc with a diameter of 11~15mm.
4. The method for testing the expansion rate of silicon-based negative electrode materials according to claim 1, characterized in that: When the baked pole pieces are assembled into batteries, the number of batteries assembled from pole pieces made of the same silicon-based material is ≥ 2; the discharge specific capacity Q is the average discharge specific capacity.
5. The method for testing the expansion rate of silicon-based negative electrode materials according to claim 4, characterized in that: The cleaning solvent is dimethyl carbonate.
6. The method for testing the expansion rate of silicon-based negative electrode materials according to claim 1, characterized in that: The slurry coating thickness is 50-200 μm; the drying is vacuum drying, the drying temperature is 80-100° C., the drying time is 8-24 hours, and the drying vacuum degree is -0.05--0.2 MPa.
Citation Information
Patent Citations
Method for monitoring and analyzing rebound of positive pole piece of lithium ion battery and lithium ion battery
CN110346727A
Method for monitoring and analyzing rebound of negative pole piece of lithium ion battery and lithium ion battery
CN110346728A
Method for testing and analyzing expansion rate of silicon-based negative electrode material
CN111928805A
Battery fuel gauges, battery management systems, and methods of managing battery life cycle
US20190178944A1
Rechargeable battery electrode testing device
US6177799B1