Organic binder for back side aluminum paste of bifacial PERC cell and preparation method thereof
By using an organic binder of ethyl cellulose, polyvinyl acetal and modified thixotropic agent, the problem of poor printing and grid breakage of the aluminum paste on the back of double-sided PERC solar cells during high-speed printing was solved, and the aluminum paste was realized The high thixotropy and adhesion ensure the stability of printing performance and production efficiency.
Patent Information
- Application Number
- CN202211344900.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-31
AI Technical Summary
During the high-speed printing process of the existing double-sided PERC solar cell backside aluminum paste, abnormal phenomena such as false printing of grid lines, missing printing of the main grid, thick lines on the frame grid lines, and powder loss of the drying friction grid lines due to fast belt transmission speeds are prone to occur, resulting in Poor printing and broken gate problems.
An organic binder composed of ethyl cellulose, polyvinyl acetal, modified thixotropic agent and organic solvent is used. The organic binder is prepared by stirring, heating and filtering, and is mixed with an inorganic binder and aluminum powder. Aluminum slurry is prepared through three-roll grinding, and the viscosity is controlled within the range of 15-20 Pa.s to improve the thixotropy and adhesion of the aluminum slurry.
It maintains the high thixotropy and adhesion of the aluminum slurry in the low viscosity range, reduces screen breaks and missing printing, ensures stable printing performance, and avoids slurry seepage. It is suitable for high-speed shearing processes of large-size silicon wafers.
Smart Images

Figure CN115565716B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cell back surface paste preparation, and in particular to an organic carrier for a double-sided PERC cell back surface aluminum paste and a preparation method thereof. Background Art
[0002] Currently, bifacial PERC (Passivated Emitter and Rear Cell) solar cell technology is the mainstream technology in the photovoltaic market, accounting for over 90% of the market's production capacity. Furthermore, with the promotion of large-size silicon wafers (182 / 210mm specifications), printing speeds have continued to increase (from 300mm / s to 400mm / s). During the aluminum paste printing process, abnormalities such as false grid lines, missing main grid lines, thick border grid lines, and high belt speeds leading to drying friction and grid line powder loss are prone to occur. Therefore, targeted research on organic binders in the paste is necessary to address these issues.
[0003] To ensure the plasticity of the fine grid lines on the back side, the double-sided PERC aluminum paste currently on the market has a high viscosity and poor thixotropic stability. This makes rapid printing on large-sized cells prone to printing defects. Furthermore, the pastes on the market are prone to powder loss or grid breakage due to friction after drying. This is mainly due to the high surface temperature of the cell after the aluminum paste is printed and removed from the three-stage drying oven. This allows the aluminum grid lines to contact the conveyor belt, causing the grid lines to lose powder or break, which in turn affects the printing of the four main grid lines. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention provides an organic binder for back-field aluminum paste in bifacial PERC cells and its preparation method. The organic binder carrier prepared by the present invention is applied to bifacial PERC aluminum paste, achieving excellent paste printing performance on large-scale silicon wafers and high-speed printing processes, and exhibiting strong adhesion to the aluminum grid lines after drying.
[0005] The technical solutions of the present invention are as follows:
[0006] The invention discloses an organic adhesive for back field aluminum paste of a double-sided PERC solar cell. The organic adhesive comprises the following components by mass percentage: 5-10% ethyl cellulose, 1-5% polyvinyl acetal, 1-2% modified thixotropic agent and 83-93% organic solvent.
[0007] Furthermore, the acetalization degree of the polyvinyl acetal is 75% to 80%.
[0008] Furthermore, the thixotropic agent is polyamide wax.
[0009] Furthermore, the thixotropic agent is modified polyamide wax.
[0010] Furthermore, the model of the modified polyamide wax is 6900-20X.
[0011] Furthermore, the organic solvent is composed of dizinc adipate and other organic solvents, and the other organic solvents are one or more of terpineol, butyl carbitol, diethylene glycol dibutyl ether, lecithin, and triethylene glycol monomethyl ether.
[0012] Furthermore, the mass fraction of the dioctyl adipate in the organic binder is 10-15%, and the mass fraction of the other organic solvent in the organic binder is 68-83%.
[0013] A method for preparing the organic adhesive comprises the following steps, in percentage by mass:
[0014] Ethyl cellulose, polyvinyl acetal, organic solvent and thixotropic agent are added into a reaction kettle, heated to 120-130° C. while stirring, stirred at a constant temperature for 2-3 hours, cooled and filtered to obtain an organic binder.
[0015] Furthermore, the heating rate is 10-15°C / min, and the stirring speed is 45-60r / min.
[0016] A bifacial PERC solar cell back surface field aluminum paste prepared with the organic binder. The bifacial PERC solar cell back surface field aluminum paste is prepared by stirring and dispersing 20% of the organic binder, 1.5% of the inorganic binder, 78% of aluminum powder, and 0.5% of the dispersant, and then grinding the mixture for 4 hours using a three-roll mill to obtain the solar back surface field aluminum paste.
[0017] The present invention uses polyvinyl acetal to replace part of ethyl cellulose. Since the adhesion strength of polyvinyl acetal after drying is greater than that of ethyl cellulose, the adhesion of aluminum paste can be improved; however, if all polyvinyl acetal is used, the printing thixotropic properties of the paste will be affected.
[0018] The prepared organic adhesive is mixed with an inorganic adhesive, aluminum powder and additives to prepare aluminum paste.
[0019] The beneficial technical effects of the present invention are:
[0020] (1) The organic adhesive prepared by the present invention uses polyvinyl acetal, dizinc adipate, and modified polyamide wax 6900-20X, which can make the aluminum paste have good thixotropy within a relatively low viscosity range (viscosity range 15Pa.s-20Pa.s). After shearing stops, the aluminum paste recovers its viscosity relatively quickly. Temperature changes have little effect on the thixotropy of the aluminum paste, the viscosity stability of the finished aluminum paste is high, and the operating environment window is wide. At the same time, polyvinyl acetal is used in the formula to replace part of the ethyl cellulose. The adhesion strength of polyvinyl acetal after drying is stronger than that of ethyl cellulose. Adding this substance to the formula can enhance the adhesion of the grid lines.
[0021] (2) The present invention uses dizinc adipate to significantly improve the thixotropy of the slurry. This substance has two ester groups with strong polarity, which can form hydrogen bonds with the hydroxyl groups on the ethyl cellulose chain, thereby forming a multi-dimensional network structure, which promotes the slurry to produce a viscose structure. Modified polyamide wax 6900-20X (melting point 145°C) is used as a thixotropic agent. Since the solvent in the organic system is mainly alcohol ethers with strong polarity, ordinary polyamide wax (melting point 120°C) has a thermal re-coarsening phenomenon in polar solvents and an unstable structure, which affects the change of the thixotropy of the slurry during storage, resulting in unstable printing performance of the slurry. Modified polyamide wax improves its alcohol resistance by treating the hydroxyl groups in the molecule.
[0022] (3) The present invention uses an organic solvent, a thixotropic agent, and polyvinyl acetal to prepare an organic binder, which can not only improve the screen printing performance of the slurry, reduce the occurrence of local grid breakage and missing prints, but also maintain the plasticity of the slurry and avoid slurry seepage. The viscosity of the prepared aluminum slurry is controlled within a relatively low range of 15-20 Pa.s, which can ensure the slurry printing performance, without grid breakage and missing prints, while having high thixotropy and good plasticity. In addition, during long-term high-speed shearing, the slurry thinning degree can be controlled to avoid slurry seepage. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the bifacial PERC battery structure. DETAILED DESCRIPTION
[0024] The present invention will be described in detail below with reference to the accompanying drawings and embodiments.
[0025] Example 1 (Examples 1-3 and Comparative Example 1 are about the effect of polyvinyl acetal on the adhesion strength of aluminum grid lines after aluminum paste drying)
[0026] An organic binder for a back-field aluminum paste for bifacial PERC solar cells comprises the following components, by mass percentage: 9% ethyl cellulose, 1% polyvinyl acetal, 15% terpineol (other solvent), 20% butyl carbitol (other solvent), 25% diethylene glycol dibutyl ether (other solvent), 14% triethylene glycol monomethyl ether (other solvent), 15% dizinc adipate (organic solvent), and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0027] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0028] 9% of ethyl cellulose, 1% of polyvinyl acetal, 15% of terpineol, 20% of butyl carbitol, 25% of diethylene glycol dibutyl ether, 14% of triethylene glycol monomethyl ether, 15% of dizinc adipate, and 1% of thixotropic agent modified polyamide wax 6900-20X are added into a reactor, and the temperature is increased by electric heating at a heating rate of 10°C / min; the temperature is stirred at a speed of 45 r / min, and after the temperature is increased to 120°C, the mixture is stirred at a constant temperature for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed. The mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0029] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0030] Example 2
[0031] An organic binder for a back-field aluminum paste for bifacial PERC solar cells comprises the following components, by mass percentage: 7% ethyl cellulose, 3% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0032] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0033] 7% ethyl cellulose, 3% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C at a stirring rate of 45 r / min, and the mixture is stirred at a constant temperature for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed. The mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0034] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0035] Example 3
[0036] The invention discloses an organic binder for back-side aluminum paste of bifacial PERC solar cells. The organic binder comprises the following components by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0037] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0038] 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min. The temperature is raised to 120°C and stirred at a speed of 45 r / min for 3 hours at a constant temperature until the resin and solvent in the reactor are fully dissolved and mixed. The reactor is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0039] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0040] Comparative Example 1 (containing no polyvinyl acetal and containing only ethyl cellulose)
[0041] An organic binder for a back-field aluminum paste for bifacial PERC solar cells comprises the following components, by mass percentage: 10% ethyl cellulose, 0% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0042] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0043] 10% ethyl cellulose, 0% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent modified polyamide wax 6900-20X are placed into a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C and stirred at a stirring rate of 45 r / min for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed. The mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0044] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0045] Example 4 (Comparison of the effect of dizinc adipate on the thixotropic index of aluminum paste on Examples 4-5 and Comparative Example 2) An organic binder for the back field aluminum paste of a bifacial PERC solar cell comprises the following components, by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 20% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 10% dizinc adipate, and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0046] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0047] 5% ethyl cellulose, 5% polyvinyl acetal, 20% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 10% dizinc adipate, and 1% thixotropic agent modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C and stirred at a speed of 45 r / min for 3 hours at a constant temperature until the resin and solvent in the reactor are fully dissolved and mixed, and the mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0048] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0049] Example 5
[0050] An organic binder for a back-field aluminum paste for bifacial PERC solar cells comprises the following components, by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0051] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0052] 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% thixotropic agent modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C and stirred at a stirring rate of 45 r / min for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed. The mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0053] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0054] Example 6
[0055] The invention discloses an organic binder for back-side aluminum paste of bifacial PERC solar cells. The organic binder comprises the following components by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 13.5% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1.5% thixotropic agent-modified polyamide wax 6900-20X.
[0056] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0057] 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 13.5% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1.5% thixotropic agent-modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C and stirred at a stirring rate of 45 r / min for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed, and the mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0058] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0059] Example 7
[0060] The invention discloses an organic binder for back-side aluminum paste of bifacial PERC solar cells. The organic binder comprises the following components by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 13% triethylene glycol monomethyl ether, 15% dizinc adipate, and 2% thixotropic agent-modified polyamide wax 6900-20X.
[0061] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0062] 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 13% triethylene glycol monomethyl ether, 15% dizinc adipate, and 2% thixotropic agent modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C and stirred at a stirring rate of 45 r / min for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed. The mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0063] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0064] Comparative Example 2 (does not contain dizinc adipate in the formula)
[0065] An organic binder for a back-field aluminum paste for bifacial PERC solar cells comprises the following components, by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 30% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 0% dizinc adipate, and 1% thixotropic agent-modified polyamide wax 6900-20X.
[0066] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0067] 5% ethyl cellulose, 5% polyvinyl acetal, 30% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 0% dizinc adipate, and 1% thixotropic agent modified polyamide wax 6900-20X are placed in a reactor and heated with electric heating at a heating rate of 10°C / min; the temperature is raised to 120°C and stirred at a stirring rate of 45 r / min for 3 hours until the resin and solvent in the reactor are fully dissolved and mixed. The mixture is cooled and filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0068] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0069] Comparative Example 3 (Compared with Example 5, comparing the effect of modified polyamide wax on the thixotropic stability of aluminum paste)
[0070] The invention discloses an organic binder for back-field aluminum paste of bifacial PERC solar cells, wherein the organic binder comprises the following components by mass percentage: 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% unmodified polyamide wax.
[0071] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0072] 5% ethyl cellulose, 5% polyvinyl acetal, 15% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 15% dizinc adipate, and 1% unmodified polyamide wax are added into a reactor and heated with electric heating at a heating rate of 10°C / min; the stirring speed is 45 r / min, the temperature is raised to 120°C and stirred at a constant temperature for 3 hours, and the resin and solvent in the reactor are fully dissolved and mixed. After cooling, the reaction is filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0073] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0074] Comparative Example 4 (the formula does not contain polyvinyl acetal, dizinc adipate, and modified polyamide wax) is an organic binder for the back field aluminum paste of a double-sided PERC solar cell. The organic binder comprises the following components, by mass percentage: 10% ethyl cellulose, 0% polyvinyl acetal, 30% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 0% dizinc adipate, and 1% thixotropic agent unmodified polyamide wax.
[0075] The preparation method of the organic binder comprises the following steps, in percentage by mass:
[0076] 10% ethyl cellulose, 0% polyvinyl acetal, 30% terpineol, 20% butyl carbitol, 25% diethylene glycol dibutyl ether, 14% triethylene glycol monomethyl ether, 0% dizinc adipate, and 1% thixotropic agent unmodified polyamide wax are put into a reactor and heated with electric heating at a heating rate of 10°C / min; the stirring speed is 45r / min, the temperature is raised to 120°C and stirred at a constant temperature for 3 hours, and the resin and solvent in the reactor are fully dissolved and mixed. After cooling, the reaction is filtered through a 280-mesh screen to obtain a finished organic adhesive.
[0077] 20% of an organic binder, 1.5% of an inorganic binder, 78% of aluminum powder, and 0.5% of a dispersant were stirred and dispersed and mixed uniformly, and then ground with a three-roll grinder for 4 hours to obtain the solar back surface field aluminum paste.
[0078] Test example:
[0079] The adhesion properties of the aluminum pastes prepared in Examples 1-3 and Comparative Example 1 when used in the production of aluminum grid lines were measured, and the results are shown in Table 1.
[0080] Table 1: Effect of polyvinyl acetal on the adhesion of aluminum paste grid lines
[0081] Example Powder removal of aluminum grid after tape tearing and drying Example 1 Aluminum grid tape can be torn without losing powder Example 2 Aluminum grid tape can be torn without losing powder Example 3 Aluminum grid tape can be torn without losing powder Comparative Example 1 The aluminum grid tape is severely peeled off due to tearing
[0082] As shown in Table 1, by comparing Examples 1-3 with Comparative Example 1, polyvinyl acetal has a significant effect on the adhesion strength of the aluminum grid lines after the aluminum paste is dried.
[0083] The thixotropic index of the aluminum pastes prepared in Examples 4-5 and Comparative Example 2 was measured. The thixotropic index was measured using a Brookfield rotational viscometer. Viscosity values at speeds of 6 r / min and 60 r / min were used for calculation. Thixotropic index = η6 / η60. The test results are shown in Table 2.
[0084] Table 2: Effect of dizinc adipate on the thixotropic index of aluminum paste
[0085] Example Thixotropic index of aluminum paste Example 4 2.69 Example 5 2.86 Comparative Example 2 2.43
[0086] As can be seen from the table, by comparing Examples 4-5 with Comparative Example 2, the use of dizinc adipate can increase the thixotropic index of the aluminum paste.
[0087] The thixotropic index of the aluminum pastes prepared in Example 5 and Comparative Example 3 was measured immediately after preparation and after 30 days of storage to assess their stability. The thixotropic index was determined using a Brookfield rotational viscometer. Viscosity values at speeds of 6 and 60 rpm were used for calculation: thixotropic index = η6 / η60. The results are shown in Table 3.
[0088] Table 3: Effect of modified polyamide wax on thixotropic stability of aluminum paste
[0089] Example Thixotropic index of aluminum paste Thixotropic index of aluminum paste after 30 days of storage Example 5 2.86 2.89 Comparative Example 3 2.81 2.53
[0090] As can be seen from the table, the comparison between Example 5 and Comparative Example 3 shows that the modified polyamide wax has better thixotropic stability to the aluminum paste.
[0091] The printing performance of the slurries of Example 5 and Comparative Example 4 was tested using a screen designed with a grid line width of 100 μm, 182 mm single crystal printing, and a printing speed of 400 mm / s. The results are shown in Table 4.
[0092] Table 4: Printing performance test of slurry of Example 5 and Comparative Example 4
[0093]
[0094]
[0095] As shown in Table 4, the optimization of the organic binder can effectively improve the printability of the aluminum paste and increase the production yield.
[0096] The above embodiments are only preferred embodiments of the present invention. The present invention is not limited to the above embodiments. Various changes may be made by those skilled in the art. Any modifications, equivalent replacements, improvements, etc. made within the design principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. Organic adhesive for back-side aluminum paste of bifacial PERC solar cells, characterized in that: The organic binder comprises the following components by mass percentage: 5-10% ethyl cellulose, 1-5% polyvinyl acetal, 1-2% thixotropic agent, and 83-93% organic solvent; The acetal degree of the polyvinyl acetal is 75% to 80%; The thixotropic agent is modified polyamide wax; The model of the modified polyamide wax is 6900-20X; The organic solvent is composed of dioctyl adipate and other organic solvents, and the other organic solvents are one or more of terpineol, butyl carbitol, diethylene glycol dibutyl ether, lecithin, and triethylene glycol monomethyl ether; The mass fraction of the dioctyl adipate in the organic binder is 10-15%, and the mass fraction of the other organic solvents in the organic binder is 68-83%.
2. A method for preparing the organic adhesive according to claim 1, characterized in that: The preparation method of the organic binder comprises the following steps, in terms of mass percentage: Ethyl cellulose, polyvinyl acetal, organic solvent and thixotropic agent are added into a reaction kettle, heated to 120-130° C. while stirring, stirred at a constant temperature for 2-3 hours, cooled and filtered to obtain an organic binder.
3. The preparation method according to claim 2, characterized in that: The heating temperature rise rate is 10-15°C / min, and the stirring speed is 45-60r / min.
4. A double-sided PERC solar cell back field aluminum paste prepared using the organic adhesive according to claim 1.