Pre-lithiation method of negative electrode sheet and pre-lithiation device of negative electrode sheet
By replenishing lithium through electrochemical method and combining with heating, microwave or light treatment technology, a stable SEI film is formed, which solves the problems of lithium ion loss and poor high-temperature performance in lithium-ion batteries, and significantly improves the efficiency and durability of the battery.
Patent Information
- Application Number
- CN202110822025.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-07-19
AI Technical Summary
The solid electrolyte membrane (SEI membrane) formed during the first charge and discharge process of lithium-ion batteries causes the loss of lithium ions, reducing battery efficiency and discharge capacity. Moreover, the SEI membrane of existing electrochemical lithium replenishment methods has poor high-temperature resistance, affecting battery performance.
The negative electrode plate is replenished with lithium using an electrochemical method to form a dense and stable SEI film, which is further reformed through heating, microwave or light treatment to improve the stability of the SEI film.
It improves the Coulombic efficiency and rate performance of lithium-ion batteries, enhances the high-temperature resistance of the battery, extends the cycle life and improves safety performance.
Smart Images

Figure CN115642225B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a method for pre-lithiation of a negative electrode plate and a device for pre-lithiation of a negative electrode plate. Background Art
[0002] During the initial charge and discharge process of a lithium-ion battery, part of the electrolyte will react at the negative electrode of the battery and combine with the lithium ions released from the positive electrode to form a solid electrolyte membrane (SEI membrane). The formation of the SEI membrane consumes lithium in the battery and converts lithium into inactive lithium-containing compounds, thereby causing reversible lithium loss and reducing the initial efficiency and discharge capacity of the battery.
[0003] In order to make up for the lithium loss caused by the formation of SEI film during the first charge, the negative electrode plate can be supplemented with lithium by electrochemical methods. However, the SEI film formed on the surface of the negative electrode plate after the existing electrochemical method supplements lithium has poor intrinsic high temperature stability. In the high temperature performance test of the battery, the SEI film is prone to decomposition, resulting in deterioration of the interface performance, aggravation of the battery side reactions, and degradation of the battery performance. Therefore, it is necessary to provide a new pre-lithiation method for the negative electrode plate to improve the stability of the SEI film formed by electrochemical lithium supplementation. Summary of the invention
[0004] In view of this, the present application provides a method for pre-lithiation of a negative electrode plate, which can form a highly stable SEI film on the surface of the negative electrode plate. The application of the pre-lithiation of the negative electrode plate in a battery can effectively improve the coulombic efficiency and rate performance of the battery, and ensure that the battery has good high temperature resistance. The present application also provides a pre-lithiation device for a negative electrode plate, a pre-lithiation of the negative electrode plate, and a lithium secondary battery.
[0005] In a first aspect, the present application provides a method for pre-lithiation of a negative electrode plate, comprising: providing a negative electrode plate, and supplementing the negative electrode plate with lithium by an electrochemical method to obtain a pre-lithiation negative electrode plate precursor, wherein the temperature of the lithium supplementation is 5°C-35°C; performing a reforming treatment on the pre-lithiation negative electrode plate precursor to obtain a pre-lithiation negative electrode plate; the reforming treatment comprises one or more of a heating treatment, a microwave treatment, and a light treatment; and the temperature of the heating treatment is 100°C-200°C.
[0006] In the pre-lithiation method of the negative electrode plate provided in the present application, a SEI film is first formed on the surface of the negative electrode plate through an electrochemical reaction, thereby offsetting the irreversible lithium loss of the battery during the first charge, and is conducive to the formation of a dense and uniform SEI film at a lithium replenishment temperature of 5°C-35°C; then, a reforming treatment is performed to reform the components in the SEI film into substances with higher stability, thereby obtaining a SEI film with good stability, thereby improving the electrochemical performance and thermal stability of the lithium-ion battery.
[0007] Optionally, the environment of the reforming treatment includes a vacuum environment or an inert gas atmosphere.
[0008] Optionally, the vacuum degree of the vacuum environment is less than or equal to -80Kpa.
[0009] Optionally, the inert gas in the inert gas atmosphere includes one or more of nitrogen, helium, neon, argon, krypton and xenon.
[0010] Optionally, the renormalization treatment time is 10s-600min.
[0011] Optionally, the heating treatment comprises electrical heating.
[0012] Optionally, the heating treatment time is 10s-600min. Further, the heating time is 60min-300min.
[0013] Optionally, the power of the microwave treatment is 1KW-50KW. Further, the power of the microwave treatment is 5KW-20KW.
[0014] Optionally, the frequency of the microwave treatment is 10000 Hz-10000 MHz. Further, the frequency of the microwave treatment is 900 MHz-2500 MHz.
[0015] Optionally, the microwave treatment time is 10s-2000s. Further, the microwave treatment time is 180s-1800s.
[0016] Optionally, the wavelength of the light treatment is 10nm-1600nm. Further, the wavelength of the light treatment is 20nm-70nm, or the wavelength of the light treatment is 800nm-1100nm.
[0017] Optionally, the light treatment time is 5 min-300 min.
[0018] Optionally, the electrochemical method includes: immersing the lithium source and the negative electrode plate in an electrolyte, electrically connecting the lithium source and the negative electrode plate to the positive and negative electrodes of a power source respectively, turning on the power supply, replenishing lithium to the negative electrode plate, and forming a SEI film on the surface of the negative electrode plate to obtain a pre-lithiation negative electrode plate precursor.
[0019] Optionally, the negative electrode plate includes one or more of a carbon-based negative electrode plate, a silicon-based negative electrode plate, a tin-based negative electrode plate, a lithium negative electrode plate, a sodium negative electrode plate, a potassium negative electrode plate, a magnesium negative electrode plate, a zinc negative electrode plate and an aluminum negative electrode plate. Further, the negative electrode plate includes a silicon-based negative electrode plate.
[0020] The pre-lithiation method of the negative electrode plate provided in the first aspect of the present application can form a dense and highly stable SEI film on the surface of the negative electrode plate, thereby effectively preventing side reactions caused by direct contact between the electrolyte and the negative electrode material, and improving the cycle performance and safety performance of the battery.
[0021] In the second aspect, the present application provides a pre-lithiation device for a negative electrode plate, comprising: a pre-lithiation component, a reforming treatment component and a transmission mechanism located between the pre-lithiation component and the reforming treatment component; the pre-lithiation component is used to electrochemically replenish lithium on the negative electrode plate to obtain a pre-lithiation negative electrode plate precursor; the transmission mechanism is used to transfer the pre-lithiation negative electrode plate precursor to the reforming treatment component; the reforming treatment component is used to reform the pre-lithiation negative electrode plate precursor to obtain a pre-lithiation negative electrode plate.
[0022] Optionally, the pre-lithiation component includes a power source, an electrolyte, and a lithium source and a negative electrode plate placed in the electrolyte, and the lithium source and the negative electrode plate are electrically connected to the positive electrode and the negative electrode of the power source respectively.
[0023] Optionally, the reforming processing component includes a processor and a processing chamber, and the heater is used to heat the processing chamber; the heater includes one or more of a heater, a microwave processor and an illumination processor.
[0024] Optionally, the reforming treatment component further includes a vacuum pump or an inert atmosphere device.
[0025] Optionally, the heater includes one or more of a heater, a microwave processor and a light processor.
[0026] Optionally, the heater includes one or more of an electromagnetic heater and a resistance heater.
[0027] The pre-lithiation equipment for negative electrode plates provided in the second aspect of the present application has high production efficiency and is suitable for large-scale production. The pre-lithiation negative electrode plates obtained by using the pre-lithiation equipment have good structural stability. When applied to lithium secondary batteries, the batteries can have good cycle performance and safety performance.
[0028] In a third aspect, the present application provides a pre-lithiation negative electrode plate, which is prepared by the pre-lithiation method of the negative electrode plate as described in the first aspect of the present application.
[0029] In a fourth aspect, the present application provides a lithium secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode comprises the pre-lithiation negative electrode plate as described in the third aspect of the present application.
[0030] The lithium secondary battery provided in the fourth aspect of the present application can have a higher energy density and cycle life because its negative electrode adopts the pre-lithiation negative electrode plate of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A method for pre-lithiation of a negative electrode plate provided in one embodiment of the present application;
[0032] Figure 2 A schematic diagram of the structure of a pre-lithiation device for a negative electrode plate provided in one embodiment of the present application;
[0033] Figure 3 A schematic diagram of the structure of a pre-lithiation assembly provided in one embodiment of the present application;
[0034] Figure 4 A schematic diagram of the structure of a renormalization processing component provided in one embodiment of the present application;
[0035] Figure 5 A schematic structural diagram of a renormalization processing component provided in another embodiment of the present application;
[0036] Figure 6 This is a scanning electron microscope image of the pre-lithiation negative electrode sheet prepared in Example 1 of the present application;
[0037] Figure 7 This is a scanning electron microscope image of the lithium-supplemented negative electrode sheet prepared in Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0039] The core components of lithium secondary batteries include positive electrodes, negative electrodes, electrolytes, diaphragms, and corresponding connecting accessories and circuits. During charging, lithium ions are released from the lattice of the positive electrode, and are embedded in the negative electrode or react with the negative electrode after being transmitted by the electrolyte; during discharge, lithium ions are released from the negative electrode, and are inserted into the lattice of the positive electrode after passing through the electrolyte. However, during the first charging process of a lithium secondary battery, part of the electrolyte will undergo a reduction reaction on the surface of the negative electrode, and at the same time combine with the lithium ions released from the positive electrode to form a solid electrolyte interface film (SEI film). The formation of the SEI film will consume the active lithium in the battery, converting the active lithium into inactive lithium-containing compounds, thereby causing a loss of reversible lithium and reducing the initial efficiency and discharge capacity of the battery. Lithium supplementation of the negative electrode can make up for the loss of active lithium in the battery during the first charging. The embodiment of the present application provides a pre-lithiation method for a negative electrode plate. The method can be used to treat the negative electrode plate to form a stable SEI film on the surface of the negative electrode plate, thereby isolating the electrolyte from the negative electrode plate, reducing the loss of active lithium in the battery, and improving the overall performance of the battery.
[0040] See also Figure 1 , Figure 1 A method for pre-lithiation of a negative electrode plate provided in one embodiment of the present application includes:
[0041] Step 100: providing a negative electrode plate, and using an electrochemical method to supplement lithium on the negative electrode plate to obtain a pre-lithiated negative electrode plate precursor, wherein the temperature of the supplementation is 5° C.-35° C.;
[0042] Step 200: reforming the pre-lithiated negative electrode precursor to obtain a pre-lithiated negative electrode; the reforming treatment includes one or more of heating treatment, microwave treatment and light treatment; the temperature of the heating treatment is 100°C-200°C.
[0043] In step 100 of the present application, the electrochemical method of lithium replenishment includes: immersing the lithium source and the negative electrode plate in an electrolyte, then electrically connecting the lithium source and the negative electrode plate to the positive and negative electrodes of a power source respectively, turning on the power supply, and replenishing the negative electrode plate with lithium. This electrochemical method simulates the environment of the first charge of the battery, so that lithium ions are released from the lithium source and reduced by electrons on the negative electrode plate, thereby replenishing the negative electrode plate with lithium. The use of the electrochemical method to replenish lithium is conducive to the formation of a dense and uniform SEI film on the surface of the negative electrode plate, and the electrochemical lithium replenishment can achieve precise control of the amount of lithium replenishment by adjusting the concentration of the lithium salt in the electrolyte and the magnitude of the voltage and current. This method is simple in process and is conducive to industrial production.
[0044] In the embodiment of the present application, the temperature of electrochemical lithium replenishment is 5°C-35°C. Controlling the temperature of the electrochemical lithium replenishment process can ensure that the formed SEI film is dense and uniform on the one hand, and can reduce side reactions on the other hand. If the temperature of the electrochemical lithium replenishment process is too high, the SEI film will be continuously generated, and the thickness of the SEI film will be too large, causing a large interface impedance, hindering the transmission of lithium ions, and being detrimental to the cycle performance of the battery; and too high a temperature will also cause the electrolyte lithium salt in the electrolyte to decompose, triggering a series of side reactions. Taking the electrolyte lithium salt LiPF6 as an example, LiPF6 is easily decomposed into LiF and PF5 when heated. PF5, as a strong Lewis acid, will cause many side reactions, such as the generation of HF to corrode the SEI film interface, and form deposits on the surface of the negative electrode, increasing the interface impedance and reducing the safety performance of the battery.
[0045] In the embodiment of the present application, the lithium source for electrochemical lithium supplementation can be a self-supporting lithium plate or a lithium foil attached to other thin film materials. The thin film material can be a metal thin film material, such as copper foil, aluminum foil, nickel foil, iron foil, tin foil and their alloys or composites. The thin film material can also be a plastic or polymer thin film material, such as polyethylene film, polypropylene film, polypropylene film, polyvinylidene fluoride film, polyethylene terephthalate (PET) film, polyimide (PI) film and their modified materials or composites.
[0046] In the embodiments of the present application, when a lithium plate is used as a lithium source, the lithium plate can be prepared by a die-casting method. In some embodiments of the present application, the preparation of the lithium plate includes: selecting a mold of a specific size, die-casting a lithium ingot in the mold by a cold rolling process, and after the die-casting is completed, a demolding operation is performed to obtain a lithium plate that can be used for electrochemical lithium supplementation. In the present application, the length and width of the lithium plate can be adjusted according to the size of the lithium supplementation device and the negative electrode plate that needs to be supplemented with lithium. In some embodiments of the present application, the thickness of the lithium plate is 1mm-5cm, and further, the thickness of the lithium plate is 3mm-4cm. In the embodiments of the present application, when lithium foil attached to other thin film materials is used as a lithium source, the preparation method of the lithium source can be: dispersing metallic lithium powder in an organic solvent such as hexane, and then applying the dispersion on one side of the thin film material; the preparation method of the lithium source can also be: heating the metallic lithium to melt, and directly applying the melt on one side of the thin film material; the lithium source can also be evaporated by evaporating lithium on one side of the thin film material; or the lithium is deposited on one side of the thin film material by rolling.
[0047] In the embodiment of the present application, the electrolyte for electrochemical lithium supplementation is a non-aqueous electrolyte, and the non-aqueous electrolyte refers to a solution formed by an electrolyte lithium salt in a non-aqueous solvent. Among them, the electrolyte can adopt a conventional non-aqueous electrolyte known to those skilled in the art. For example, the electrolyte lithium salt can be selected from lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluorosilicate (LiSiF6), lithium tetraphenylborate (LiB(C6H5)4), lithium chloride (LiCl), lithium bromide (LiBr), lithium chloroaluminate (LiAlCl4) and lithium fluorocarbon sulfonate (LiC(SO2CF3)3), LiCH3SO3, LiN(SO2CF3)2, LiN(SO2C2F5)2 One or more. The non-aqueous organic solvent can be selected from one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, butyl propionate, and ethyl butyrate. The non-aqueous organic solvent can also be selected from one or more of organic esters containing fluorine, sulfur, or unsaturated bonds. In some embodiments of the present application, the non-aqueous solvent is selected from a chain ether and a cyclic ether solution or a mixed solution, wherein the chain ether includes dimethoxymethane (DMM), 1,2-dimethoxyethane (DME), 1,2-dimethoxypropane (DMP) and diethylene glycol dimethyl ether (DG), and one or more of other fluorine-containing, sulfur-containing or unsaturated bond-containing chain organic esters; the cyclic ether can be tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-MeTHF), 1,3-dioxolane (DOL) and 4-methyl-1,3-dioxolane (4-MeDOL), and one or more of other fluorine-containing, sulfur-containing or unsaturated bond-containing chain organic esters. In some embodiments of the present application, the electrolyte further includes a film-forming additive, which may be one or more of fluoroethylene carbonate, lithium difluorophosphate, tris(trimethylsilane) borate, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, ethylene sulfate, ethylene carbonate, and propylene carbonate. In some embodiments of the present application, the concentration of the electrolyte lithium salt in the electrolyte is 0.1 mol / L-15 mol / L. In some embodiments of the present application, the concentration of the electrolyte lithium salt in the electrolyte is 1 mol / L-10 mol / L.
[0048] The present application uses an electrochemical method to supplement lithium on the negative electrode plate to obtain a pre-lithiated negative electrode plate precursor, and the pre-lithiated negative electrode plate precursor includes a negative electrode plate body and a SEI film formed on the surface of the negative electrode plate body. In the present application, the SEI film of the pre-lithiated negative electrode plate precursor contains a large amount of inorganic lithium salts and organic lithium salts, and the inorganic lithium salts include but are not limited to LiF, Li2CO3, Li2O, and LiOH, and the organic lithium salts include but are not limited to (CH2OCO2Li)2, LiOCO2CH3, LiOCO2C2H5, LiOCH3, and (LiCO2)2. Further research in the present application found that in the SEI film formed after the negative electrode plate is electrochemically supplemented with lithium, the nucleation and growth of some inorganic lithium salts are not complete, resulting in large internal stress in the SEI film and poor stability of the SEI film; and the organic lithium salt in the SEI film has poor thermal stability, and is prone to decomposition during the use of the battery, resulting in damage to the SEI film, which in turn triggers a series of side reactions between the electrolyte and the negative electrode material, and more seriously, causes thermal runaway of the battery. Therefore, the negative electrode plate directly obtained by electrochemical lithium supplementation has poor high temperature resistance, and its use in the battery is not conducive to the battery's cycle performance and safety performance.
[0049] In order to solve the above problems, the present application performs a reforming treatment on the pre-lithiated negative electrode plate obtained by electrochemical lithium supplementation, and the reforming treatment includes one or more of heating treatment, microwave treatment and light treatment. During the reforming treatment, the organic lithium salt in the SEI film of the pre-lithiated negative electrode plate precursor will be dissolved and transformed, and the inorganic lithium salt in the SEI film will be aged and regenerated, thereby reforming the components of the SEI film and greatly improving the stability of the SEI film. Specifically, the pre-lithiated negative electrode plate precursor obtained after the negative electrode plate is electrochemically supplemented with lithium contains a portion of electrolyte. During the reforming treatment, the electrolyte has a certain dissolving effect on the organic lithium salt and inorganic lithium salt in the SEI film, thereby causing the organic lithium salt and inorganic lithium salt to be dissolved or aged under the action of the electrolyte. Taking the electrolyte solvents DMC and EC as examples, the solubility of DMC and EC for organic lithium salts and inorganic lithium salts in the SEI film is as follows:
[0050] (CH2OCO2Li)2>LiOCO2CH3>LiOH>LiOCO2C2H5>LiOCH3>LiF>(LiCO2)2
[0051] For organic lithium salts in the SEI film, the dissolution of organic lithium salts means that during the reforming process, the molecular motion is accelerated and the organic lithium salts can be dissolved in the electrolyte. The conversion of organic lithium salts means that during the reforming process, the organic lithium salts are decomposed and converted into inorganic lithium salts. Taking (CH2OCO2Li)2 as an example, the reactions that occur during the reforming process of (CH2OCO2Li)2 are as follows:
[0052] (CH2OCO2Li)2→Li2CO3+CH2CH2+CO2+1 / 2O2
[0053] It can be seen from the reaction equation that the reforming treatment can reduce the unstable organic lithium salts in the SEI film and convert them into stable inorganic components, thereby improving the structural stability of the negative electrode sheet.
[0054] For inorganic lithium salts in SEI membrane, the regeneration of inorganic lithium salts refers to: during the reforming process, unstable organic lithium salts in SEI membrane are dissolved and transformed to generate new inorganic lithium salts, thereby increasing the content of inorganic lithium salts in SEI membrane and greatly improving the thermal stability of SEI membrane. The aging of inorganic lithium salts refers to: under the combined action of reforming treatment and electrolyte, inorganic lithium salts fully nucleate and grow to form stable substances. The aging of inorganic lithium salts is conducive to promoting the growth of inorganic components and releasing the internal stress of SEI membrane, thereby improving the structural stability of SEI membrane.
[0055] In the present application, in addition to promoting the dissolution and conversion of organic lithium salts and the aging reaction of inorganic lithium salts, the reforming treatment can also promote the remaining reactions of the electrochemical lithium replenishment process. Taking the electrolyte solvent EC as an example, during the reforming treatment process, the electrolyte lithium salt in the electrolyte and the electrolyte can react as follows:
[0056] 2EC+2Li + C n 2- →Li2CO3+CH2CH2+C n
[0057] Taking the electrolyte solvent as PC as an example, during the reforming process, the electrolyte lithium salt in the electrolyte and the electrolyte can react as follows:
[0058] 2PC+2Li + C n 2- →Li2CO3+CH3CHCH2+C n
[0059] It can be seen from the above reaction formula that the reforming treatment can promote the intermediate reaction of electrochemical lithium replenishment, thereby ensuring that each component in the SEI film is fully converted into a stable substance to obtain a structurally stable SEI film.
[0060] In the present application, the reforming treatment of the pre-lithiated negative electrode sheet precursor can also fully remove the electrolyte solvent remaining in the pre-lithiated negative electrode sheet precursor after electrochemical lithium supplementation, and promote the complete volatilization of the electrolyte solvent, which is beneficial to the subsequent production of the battery, such as winding, hot pressing, and tab welding. Since the components and proportions of the solvent and additives in the battery electrolyte need to be prepared in advance during battery assembly, if there is electrolyte solvent remaining in the negative electrode sheet, the components and content of the electrolyte will change when the sheet is assembled into a battery, and some electrolyte solvents used for electrochemical lithium supplementation are not suitable for the solvent system required for battery performance, which will cause uncontrollable effects on the battery.
[0061] In the embodiment of the present application, the method of reforming treatment includes one or more of heating treatment, microwave treatment and light treatment. In the embodiment of the present application, the time of reforming treatment is 10s-600min. In some embodiments of the present application, the time of reforming treatment is 60min-300min. The time of reforming treatment can be specifically but not limited to 10s, 1min, 10min, 30min, 60min, 90min, 120min, 150min, 300min, 500min or 600min. Controlling the reforming treatment within a certain time can ensure that the SEI film is fully reformed and rectified, thereby improving the stability of the SEI film. The pre-lithiation negative electrode plate obtained after the reforming treatment can be used to assemble into a battery or electrochemical device, so that the battery or electrochemical device has excellent high temperature cycle and high temperature storage performance.
[0062] In some embodiments of the present application, the pre-lithiation negative electrode precursor is reformed by heating treatment, wherein the heating treatment includes electric heating, and the electric heating includes one or more of electromagnetic heating and resistance heating. In the embodiment of the present application, the temperature of the heating treatment is 100°C-200°C. The temperature of the heating treatment may be, but is not limited to, 100°C, 120°C, 150°C, 170°C or 200°C. When the temperature of the heating treatment is too high, most of the components in the SEI film will undergo thermal decomposition, and the side reactions between the electrolyte and the negative electrode will not be suppressed. If the heating treatment temperature is too low, the unstable organic lithium salts in the SEI film cannot be effectively decomposed, and the effect of reforming the SEI components of the electrode cannot be achieved. In the embodiment of the present application, when heating is used for reforming treatment, the time of the reforming treatment is 60min-300min.
[0063] In some embodiments of the present application, microwave treatment is used to reform the pre-lithiated negative electrode sheet precursor. When microwave treatment is used, microwave energy can be converted into the internal energy of the negative electrode sheet. Compared with the heating treatment from the outside to the inside, the heating rate of microwave treatment is faster, and the effect of microwave treatment on the reformation treatment of the pre-lithiated negative electrode sheet precursor is more uniform. In some embodiments of the present application, the power of microwave treatment is 1KW-50KW, the frequency of microwave treatment is 10000Hz-10000MHz, and the time of microwave treatment is 10s-2000s. In some embodiments of the present application, the power of microwave treatment is 5KW-20KW, the frequency of microwave treatment is 900MHz-2500MHz, and the time of microwave treatment is 180s-1800s. In the embodiment of the present application, the power of microwave treatment can be specifically but not limited to 1KW, 2KW, 5KW, 10KW, 20KW, 30KW, 40KW or 50KW. Controlling the power of the microwave treatment can ensure that the microwaves fully dissolve the unstable organic lithium salts in the SEI film and remove the electrolyte in the pre-lithiated negative electrode plate.
[0064] In some embodiments of the present application, the pre-lithiated negative electrode plate precursor is reformed by light treatment. When light treatment is used, in addition to increasing the temperature of the pre-lithiated negative electrode plate precursor through photothermal conversion, the light treatment can also excite electrons, catalyze the remaining reduction reaction in the electrolyte, and promote the complete growth of the SEI film. In the embodiment of the present application, when light treatment is used for renormalization treatment, the wavelength of the light treatment is 10nm-1600nm, and the time of the light treatment is 5min-300min. In some embodiments of the present application, the wavelength of the light treatment is 20nm-70nm, and the time of the light treatment is 5min-120min. When the wavelength of light is 20nm-70nm, the high-energy particles in the light wave have a strong impact, which can accelerate molecular motion and provide energy, thereby promoting the conversion of organic lithium salts in the SEI film and the generation of inorganic components, thereby improving the high temperature resistance of the SEI film. In some embodiments of the present application, the wavelength of the light treatment is 800nm-1100nm, and the time of the light treatment is 30min-240min. When the wavelength of the light is 800nm-1100nm, the light wave is easily converted into heat, thereby promoting the dissolution of organic lithium salts in the SEI film and the aging of inorganic lithium salts.
[0065] In an embodiment of the present application, the environment for the reforming treatment includes a vacuum environment or an inert gas atmosphere. Carrying out the reforming treatment in a vacuum environment or an inert gas atmosphere can avoid the reaction of the SEI film in the pre-lithiated negative electrode sheet precursor with the air. In some embodiments of the present application, the pre-lithiated negative electrode sheet precursor is placed in a vacuum environment for reforming treatment, and the vacuum degree of the vacuum environment is less than or equal to -80Kpa. The vacuum degree of the vacuum environment can be, but is not limited to, -80Kpa, -90Kpa, -100Kpa, -150Kpa or -200Kpa. In some embodiments of the present application, the pre-lithiated negative electrode sheet precursor is placed in an inert gas atmosphere for reforming treatment, and the inert gas in the inert gas atmosphere includes, but is not limited to, one or more of nitrogen, helium, neon, argon, krypton and xenon.
[0066] In the embodiment of the present application, after the pre-lithiation negative electrode sheet precursor is subjected to a reforming treatment, the components of the SEI film in the pre-lithiation negative electrode sheet precursor are reformed, and the unstable organic lithium salts in the SEI film are converted into stable inorganic substances, and the inorganic substances can be further aged to form a stable phase structure, thereby improving the stability of the SEI and ensuring that the surface of the pre-lithiation negative electrode sheet precursor has a uniform SEI film, thereby inhibiting the reaction of the electrolyte with the active lithium on the negative electrode surface, reducing the loss of active lithium, and ensuring that the battery has a high energy density and cycle life.
[0067] In the present application, after the pre-lithiation negative electrode plate precursor is subjected to a reforming treatment, the SEI film becomes more compact and uniform. In the embodiment of the present application, the thickness of the SEI film in the pre-lithiation negative electrode plate is 50nm-1000nm. The thickness of the protective layer may be, but is not limited to, 50nm, 100nm, 200nm, 300nm, 500nm or 1000nm. When the thickness of the SEI film is within the above range, it can ensure that the battery has a higher discharge capacity and a longer cycle life without causing a larger interface impedance, and can ensure the effective transmission of lithium ions.
[0068] In the embodiment of the present application, the negative electrode plate for pre-lithiation can be any negative electrode plate known in the prior art. In some embodiments of the present application, the negative electrode plate includes one or more of a carbon-based negative electrode plate, a silicon-based negative electrode plate, a tin-based negative electrode plate, a lithium negative electrode plate, a sodium negative electrode plate, a potassium negative electrode plate, a magnesium negative electrode plate, a zinc negative electrode plate and an aluminum negative electrode plate. In the present application, the negative electrode active material used in the negative electrode plate can be but is not limited to graphite, hard carbon, soft carbon, graphene, silicon, silicon oxygen, silicon metal compound, tin, tin carbon, tin oxygen, tin metal compound, lithium silicon alloy, lithium sodium alloy, lithium potassium alloy, lithium aluminum alloy, lithium tin alloy, lithium indium alloy, lithium titanate, iron oxide, lithium titanium phosphate and titanium, aluminum, zinc, germanium, antimony and other elements and their oxides, nitrides, sulfides, phosphides one or more. In some embodiments of the present application, the negative electrode plate to be pre-lithiated is a silicon-based negative electrode plate. Considering that the silicon-based negative electrode plate will consume more active lithium during the first charge, resulting in a decrease in the initial efficiency and discharge capacity of the battery, the pre-lithiation method of the negative electrode plate provided in the present application can effectively supplement the lithium loss caused by the first charging of the silicon-based negative electrode plate, thereby greatly improving the initial charge and discharge efficiency of the silicon-based negative electrode plate.
[0069] In the embodiment of the present application, the current collector used in the negative electrode plate includes copper foil, which may be a porous structure or an ordinary copper foil, and the thickness of the copper foil is 5μm-100μm, and further, the thickness of the copper foil is 10μm-20μm. In the embodiment of the present application, the binder used in the negative electrode plate includes one or more of polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and styrene butadiene latex (SBR). In the embodiment of the present application, the conductive agent used in the negative electrode plate may be any conductive agent known in the art, for example, the conductive agent may be one or more of acetylene black, Ketjen black, Super-P, carbon nanotubes, carbon nanofibers, activated carbon and graphene. In the embodiment of the present application, the mass of the conductive agent accounts for 0.1%-20% of the mass of the negative electrode active material, and further the mass of the conductive agent accounts for 1%-10% of the mass of the negative electrode active material.
[0070] In the present application, the preparation method of the negative electrode sheet can adopt any method known in the art. In some embodiments of the present application, the preparation method of the negative electrode sheet includes: preparing the negative electrode active material, the binder, the conductive agent and the solvent into a negative electrode material slurry, slurrying the negative electrode material slurry and coating it on the collector to dry and press the sheet, and then cutting the sheet to obtain the negative electrode sheet, the drying temperature is 100℃-150℃, and the drying time is 2h-10h. The solvent used to prepare the negative electrode material slurry can be various solvents in the prior art, for example, the solvent can be selected from one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), diethylformamide (DEF), dimethyl sulfoxide (DMSO), tetrahydrofuran (THF), water and alcohols. The amount of solvent can be adjusted according to the viscosity of the slurry and the operating requirements. In some embodiments of the present application, the mass percentage of the negative electrode active material in the negative electrode material slurry is 20%-90%, and further, the mass percentage of the negative electrode active material in the negative electrode material slurry is 40%-85%.
[0071] The present application also provides a pre-lithiation negative electrode plate, which is prepared by the pre-lithiation method of the negative electrode plate of the present application, and the pre-lithiation negative electrode plate has good thermal stability.
[0072] This application also provides a pre-lithiation device for a negative electrode plate, see Figure 2 , Figure 2 A schematic diagram of the structure of a pre-lithiation device for a negative electrode plate provided in one embodiment of the present application. The pre-lithiation device for a negative electrode plate includes a pre-lithiation component 10, a transmission mechanism 20, and a reforming treatment component 30. Among them, the pre-lithiation component 10 is used to electrochemically replenish lithium for the negative electrode plate, and the negative electrode plate is replenished with lithium to obtain a pre-lithiation negative electrode plate precursor; the transmission mechanism 20 is used to transfer the pre-lithiation negative electrode plate precursor to the reforming treatment component 30; the reforming treatment component 30 is used to reform the pre-lithiation negative electrode plate precursor, and the pre-lithiation negative electrode plate precursor is reformed to obtain a pre-lithiation negative electrode plate.
[0073] See also Figure 3 , Figure 3 A schematic diagram of the structure of a pre-lithiation component provided for one embodiment of the present application. The pre-lithiation component includes a lithium source 101, an electrolyte 102, a negative electrode plate 103 and a power source 104. Among them, the lithium source 101 and the negative electrode plate 103 are immersed in the electrolyte 102, and the lithium source 101 and the negative electrode plate 103 are electrically connected to the positive and negative electrodes of the power source 104, respectively. In the embodiment of the present application, the lithium source can be a lithium plate or a lithium foil attached to other thin film materials. In the embodiment of the present application, the electrolyte is a non-aqueous electrolyte, and the electrolyte can use a conventional non-aqueous electrolyte known to those skilled in the art.
[0074] See also Figure 4 , Figure 4 A schematic diagram of the structure of a pre-lithiation component provided for one embodiment of the present application. The reformation processing component includes a processor 301 and a processing chamber 302, and the processor 301 is used to perform a reformation process on the pre-lithiation negative electrode plate precursor. In the embodiment of the present application, the processor includes one or more of a heater, a microwave processor, and a light processor. When the processor is a heater, the heater can directly heat the processing chamber, and the heater can be, but is not limited to, one or more of an electromagnetic heater and a resistance heater; when the processor is a microwave processor, the microwave processor can irradiate the processing chamber with microwaves; when the processor is an light processor, the light processor can irradiate the processing chamber with light waves. In some embodiments of the present application, the processor is a microwave processor, and the microwave processor includes a waveguide and an oscillator.
[0075] In some embodiments of the present application, the reforming treatment component further includes a vacuum pump or an inert atmosphere device. The vacuum pump can evacuate the interior of the processing chamber to provide a vacuum environment, and the inert atmosphere device can form an inert gas atmosphere in the processing chamber. Figure 5 , Figure 5 This is a schematic diagram of the structure of a reforming treatment component provided in another embodiment of the present application. The reforming treatment component includes a processor 301, a processing chamber 302 and a vacuum pump 303. The vacuum pump 303 is connected to the processing chamber 302 and is used to evacuate the interior of the processing chamber 302 to a vacuum.
[0076] In the present application, the transmission mechanism 20 is used to transfer the pre-lithiation negative electrode plate precursor to the processing chamber of the reforming processing assembly. The structure of the transmission mechanism is not limited. For example, the transmission mechanism may include a motor and a conveyor belt.
[0077] The method for using the pre-lithiation equipment of the negative electrode plate of the present application includes: immersing a lithium source and a negative electrode plate in an electrolyte, connecting the lithium source and the negative electrode plate to a power source, and electrochemically replenishing lithium to the negative electrode plate to obtain a pre-lithiation negative electrode plate precursor; transferring the pre-lithiation negative electrode plate precursor to a processing chamber of a reforming processing component through a transmission mechanism for reforming processing to obtain a pre-lithiation negative electrode plate.
[0078] The present application also provides a lithium secondary battery, including a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode includes a pre-lithiated negative electrode plate provided in the present application. In the present application, the positive electrode of the lithium secondary battery includes a positive electrode active material that can reversibly embed / de-embed lithium ions. In some embodiments of the present application, the positive electrode active material can be, but is not limited to, lithium cobalt oxide (LiCoO2), lithium iron phosphate (LiFePO4), LiNi 0.33 Co 0.33 Mn 0.33 O2(NCM111),LiNi 0.4 Co 0.2 Mn 0.4O2(NCM424),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) or more.
[0079] In the present application, the electrolyte of the lithium secondary battery includes a solution of an electrolyte lithium salt in a non-aqueous solvent. In an embodiment of the present application, the electrolyte lithium salt includes lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluorosilicate (LiSiF6), lithium tetraphenylborate (LiB(C6H5)4), lithium chloride (LiCl), lithium bromide (LiBr), lithium chloroaluminate (LiAlCl4), lithium fluoroalkylsulfonate (LiC(SO2CF3)3), LiCH3SO3, LiN(SO2CF3)2 and LiN(SO2C2F5)2. In some embodiments of the present application, the non-aqueous solvent includes one or more of a chain acid ester and a cyclic acid ester. In some embodiments of the present application, the chain acid ester includes one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC) and dipropyl carbonate (DPC). In some embodiments of the present application, the chain acid ester includes chain organic esters containing fluorine, sulfur or unsaturated bonds. In some embodiments of the present application, the cyclic acid ester includes one or more of ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), γ-butyrolactone (γ-BL) and sultone. In some embodiments of the present application, the cyclic acid ester includes cyclic organic esters containing fluorine, sulfur or unsaturated bonds. In some embodiments of the present application, the non-aqueous solvent includes one or more of chain ethers and cyclic ether solutions. In some embodiments of the present application, the cyclic ether includes one or more of tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-MeTHF), 1,3-dioxolane (DOL) and 4-methyl-1,3-dioxolane (4-MeDOL). In some embodiments of the present application, the cyclic ether includes a cyclic organic ether containing fluorine, sulfur or unsaturated bonds. In some embodiments of the present application, the chain ether includes one or more of dimethoxymethane (DMM), 1,2-dimethoxyethane (DME), 1,2-dimethoxypropane (DMP) and diethylene glycol dimethyl ether (DG). In some embodiments of the present application, the chain ether includes a chain organic ether containing fluorine, sulfur or unsaturated bonds. In an embodiment of the present application, the concentration of the electrolyte lithium salt in the electrolyte is 0.1mol / L-15mol / L. In some embodiments of the present application, the concentration of the electrolyte lithium salt is 1mol / L-10mol / L.
[0080] In the present application, the separator of the lithium secondary battery can be any separator known to those skilled in the art, for example, the separator can be one or more of polyolefin microporous membrane, polyethylene terephthalate, polyethylene felt, glass fiber felt or ultrafine glass fiber paper.
[0081] In the embodiments of the present application, the battery can be prepared by using either a lamination process or a winding process. In some embodiments of the present application, the battery is prepared by using a lamination process.
[0082] The lithium secondary battery provided in the present application has high cycle performance and high safety because it adopts the pre-lithiation negative electrode plate provided in the present application.
[0083] The technical solution of the present application is further described below with reference to a number of embodiments.
[0084] Example 1
[0085] A method for preparing a lithium secondary battery, comprising:
[0086] 1) Preparation of pre-lithiation negative electrode
[0087] The negative electrode active materials silicon dioxide, graphite, conductive agent Super P, binder and N-methylpyrrolidone (NMP) are mixed into a slurry in a mass ratio of 35:60:2:3:150, wherein the binder includes CMC and SBR, and the mass ratio of CMC to SBR is 1.5:1.5; the slurry is then coated on a wide conductive substrate copper foil and dried, rolled and cut to obtain a negative electrode sheet.
[0088] The negative electrode plate and the lithium plate are assembled into two electrodes, which are immersed in an electrolyte, wherein the solvent of the electrolyte includes 30% by mass of ethylene carbonate (EC) and 70% by mass of ethyl methyl carbonate (EMC), the concentration of the electrolyte lithium salt LiPF6 in the electrolyte is 1.0M, and the electrolyte additives include fluoroethylene carbonate (FEC) and methyl vinyl carbonate (VC), wherein the mass percentage of fluoroethylene carbonate (FEC) in the electrolyte is 10%, and the mass percentage of methyl vinyl carbonate (VC) in the electrolyte is 1%. The negative electrode plate is electrochemically supplemented with lithium by applying an external circuit to obtain a pre-lithiated negative electrode plate precursor, and the temperature of the electrochemical lithium supplement process is 25°C.
[0089] The pre-lithiation negative electrode sheet precursor is transferred to the reforming treatment component, which is heated by an electric heater. The vacuum degree in the treatment chamber is -90Kpa. The temperature of the treatment chamber is raised to 150°C by the electric heater, and the pre-lithiation negative electrode sheet precursor is heated for 2 hours to obtain a pre-lithiation negative electrode sheet.
[0090] 2) Preparation of positive electrode
[0091] The positive electrode active material LiCoO2, the conductive agent conductive carbon, and the binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 96:2:2, and stirred under the action of a vacuum mixer until the system is uniform to obtain a positive electrode slurry with a certain viscosity; the positive electrode slurry is evenly coated on the surface of the positive electrode collector aluminum foil, dried at 85°C and cold pressed, and then trimmed, cut, and striped, and then dried under vacuum conditions at a temperature of 85°C for 4 hours, and the pole ears are welded to obtain a positive electrode sheet.
[0092] 3) Preparation of electrolyte
[0093] 1M lithium hexafluorophosphate was dissolved in a mixed solvent of ethylene carbonate and ethyl methyl carbonate, wherein the volume ratio of ethylene carbonate to ethyl methyl carbonate was 3:7, and then 9wt% FEC (fluoroethylene carbonate) and 2wt% VC (ethylene carbonate) were added to obtain an electrolyte.
[0094] 4) Preparation of lithium secondary batteries
[0095] The pre-lithiation negative electrode sheet, positive electrode sheet, electrolyte and polyethylene porous separator prepared above are assembled into a soft pack battery.
[0096] Example 2
[0097] The negative electrode sheet was prepared by the same method as in Example 1, and the negative electrode sheet was electrochemically supplemented with lithium. The difference between Example 2 and Example 1 is that the temperature of the electrochemical lithium supplementation process is 10° C. The pre-lithiated negative electrode sheet precursor was reformed and a soft-pack battery was prepared by the same method as in Example 1 to obtain a soft-pack battery.
[0098] Example 3
[0099] The difference between Example 3 and Example 1 is that the temperature of the heating treatment is 100° C., and the pre-lithiated negative electrode plate is heated for 2 hours to obtain a pre-lithiated negative electrode plate. The pre-lithiated negative electrode plate, the positive electrode plate, the electrolyte and the separator are then assembled into a soft pack battery.
[0100] Example 4
[0101] The difference between Example 4 and Example 1 is that the temperature of the heating treatment is 200° C., and the pre-lithiated negative electrode sheet precursor is heated for 2 hours to obtain a pre-lithiated negative electrode sheet. The pre-lithiated negative electrode sheet, the positive electrode sheet, the electrolyte and the separator are then assembled into a soft pack battery.
[0102] Example 5
[0103] The difference between Example 5 and Example 1 is that the pre-lithiated negative electrode sheet precursor is transferred to the reforming treatment component, and the reforming treatment component uses a microwave processor to irradiate the pre-lithiated negative electrode sheet precursor with microwaves. The power of the microwave processor is 15KW, the frequency of the microwave processor is 2450MHz, and the microwave treatment time is 15min. During the microwave treatment process, the temperature of the pre-lithiated negative electrode sheet precursor is 200°C, and a pre-lithiated negative electrode sheet is obtained. Then, the pre-lithiated negative electrode sheet, the positive electrode sheet, the electrolyte and the separator are assembled into a soft pack battery.
[0104] Example 6
[0105] The difference between Example 6 and Example 1 is that the pre-lithiated negative electrode sheet precursor is transferred to the reforming treatment component, and the reforming treatment component uses a light processor to irradiate the pre-lithiated negative electrode sheet precursor with light waves. The wavelength of the light processor is 50nm, and the light treatment time is 30min. During the light treatment process, the temperature of the pre-lithiated negative electrode sheet precursor is 150°C, and a pre-lithiated negative electrode sheet is obtained. Then, the pre-lithiated negative electrode sheet, the positive electrode sheet, the electrolyte and the separator are assembled into a soft pack battery.
[0106] Example 7
[0107] The difference between Example 7 and Example 6 is that the light treatment time is 20 minutes. During the light treatment process, the temperature of the pre-lithiated negative electrode precursor is 150° C. to obtain a pre-lithiated negative electrode. The pre-lithiated negative electrode, positive electrode, electrolyte and separator are then assembled into a soft pack battery.
[0108] Example 8
[0109] The difference between Example 8 and Example 6 is that the wavelength of the light irradiation processor is 980nm, and the light irradiation time is 60min. During the light irradiation process, the temperature of the pre-lithiated negative electrode precursor is 150°C, and a pre-lithiated negative electrode is obtained. Then, the pre-lithiated negative electrode, the positive electrode, the electrolyte and the separator are assembled into a soft pack battery.
[0110] In order to highlight the beneficial effects of the present application, the following comparative examples are set.
[0111] Comparative Example 1
[0112] A method for preparing a lithium secondary battery, comprising:
[0113] A negative electrode sheet was prepared by the same method as in Example 1, and the negative electrode sheet and the lithium sheet were assembled into two electrodes, and immersed in an electrolyte, wherein the solvent of the electrolyte included 30% by mass of ethylene carbonate (EC) and 70% by mass of ethyl methyl carbonate (EMC), the concentration of the electrolyte lithium salt LiPF6 in the electrolyte was 1.0M, and the electrolyte additives included fluoroethylene carbonate (FEC) and methyl vinyl carbonate (VC), the mass percentage of fluoroethylene carbonate (FEC) in the electrolyte was 10%, and the mass percentage of methyl vinyl carbonate in the electrolyte was 1%. An external circuit was applied to the negative electrode sheet for electrochemical lithium supplementation, and the temperature of the electrochemical lithium supplementation process was 100°C, to obtain a lithium supplemented negative electrode sheet precursor.
[0114] The lithium-replenished negative electrode precursor is transferred to the reforming treatment component, which is heated by an electric heater. The vacuum degree in the treatment chamber is -90Kpa, and the temperature is raised to 150°C for 2 hours of reforming treatment to obtain a lithium-replenished negative electrode.
[0115] The positive electrode sheet and the electrolyte were prepared in the same manner as in Example 1, and the lithium-supplemented negative electrode sheet, the positive electrode sheet, the electrolyte and the polyethylene porous diaphragm were assembled into a soft-pack battery.
[0116] Comparative Example 2
[0117] The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, the negative electrode plate is electrochemically supplemented with lithium without undergoing a reforming treatment, so as to obtain a lithium-supplemented negative electrode plate. Then, the lithium-supplemented negative electrode plate, the positive electrode plate, the electrolyte and the separator are assembled into a soft-pack battery.
[0118] Comparative Example 3
[0119] The difference between Comparative Example 3 and Example 1 is that the heating temperature is 60°C, and the pre-lithiated negative electrode precursor is heated for 2 hours to obtain a lithium-supplemented negative electrode. The lithium-supplemented negative electrode, positive electrode, electrolyte and separator are then assembled into a soft-pack battery.
[0120] Comparative Example 4
[0121] The difference between Comparative Example 4 and Example 1 is that the temperature of the heating treatment is 300°C, and the pre-lithiated negative electrode precursor is heat treated for 2 hours to obtain a lithium-supplemented negative electrode. The lithium-supplemented negative electrode, positive electrode, electrolyte and separator are then assembled into a soft-pack battery.
[0122] Effect Example
[0123] In order to strongly support the beneficial effects brought by the technical solutions of the embodiments of this application, the following tests are provided:
[0124] 1) The morphology of the pre-lithiated negative electrode sheets of Example 1 and Comparative Example 2 was characterized by scanning electron microscopy. Figure 6 and Figure 7 ,in, Figure 6 This is a scanning electron microscope image of the pre-lithiation negative electrode sheet prepared in Example 1 of the present application. Figure 7 This is a scanning electron microscope image of the lithium-supplemented negative electrode sheet prepared in Comparative Example 2 of the present application. Figure 6 and Figure 7 In the process, the film layer wrapped around the outside of the particles is the SEI film. Figure 6 and Figure 7 By comparison, it can be seen that compared with the lithium-supplemented negative electrode plate of comparative example 2 which has not been reformed, the SEI film structure of the pre-lithiation negative electrode plate of embodiment 1 of the present application which has been reformed is denser, has fewer pores on the surface, and has a thinner SEI film.
[0125] 2) The soft-pack batteries of Examples 1-8 and Comparative Examples 1-4 were tested for high temperature cycle performance. The specific test conditions were as follows: the soft-pack batteries were placed in an oven at 45°C for 1 hour, charged at 1C (1C = 3000mAh) to 4.45V, and the constant voltage was cut off at 0.025C. The soft-pack batteries were taken out and placed at 25°C for 1 hour, and the thickness (PPG 400g) and internal resistance after full charge were recorded. The above are the initial thickness and internal resistance; the soft-pack batteries were put back into the oven at 45°C, placed for 1 hour, and discharged at 0.2C to 3.0V. The capacity obtained at this time is the initial capacity.
[0126] During the cycle, the battery was charged to 4.45V at 1C and then cut off at 0.025C at constant voltage, which was considered as the charging process; then the battery was discharged to 3.0V at 0.5C, which was considered as the discharging process; one charge and one discharge were counted as one cycle, and the soft-pack battery was cycled 500 times in a 45°C oven and then the battery was taken out. For the 501st charge, the battery was charged to 4.45V at 1C and cut off at 0.025C at constant voltage. The soft-pack battery was taken out and left to stand at 25°C for 1h. The thickness (PPG 400g) and internal resistance after full charge were recorded. The above are the thickness and internal resistance after the cycle; the soft-pack battery was put back into the 45°C oven and left to stand for 1h; the battery was discharged to 3.0V at 0.2C, and the capacity obtained at this time was the capacity after the cycle. The capacity, internal resistance and thickness after the cycle were compared with the initial capacity, internal resistance and thickness, and the cycle retention rate, thickness growth rate and internal resistance growth rate were obtained. The high temperature cycle performance tests of the soft-pack batteries of Examples 1-8 and Comparative Examples 1-4 are shown in Table 1.
[0127] Table 1 High temperature resistant cycle performance parameters of soft pack batteries of Examples 1-8 and Comparative Examples 1-4
[0128]
[0129] 1) The soft-pack batteries of Examples 1-8 and Comparative Examples 1-4 were tested for their high temperature storage performance. The specific conditions of the test were as follows: the soft-pack batteries were placed in an oven at 25°C for 1 hour, charged to 4.45V at 1C (1C = 3000mAh), and the constant voltage was cut off at 0.025C. The soft-pack batteries were taken out and placed at 25°C for 1 hour, and the thickness (PPG 400g) and internal resistance after full charge were recorded. The above are the initial thickness and internal resistance; the soft-pack batteries were placed back in an oven at 85°C, placed for 1 hour, and discharged to 3.0V at 0.2C. The capacity obtained at this time was the initial capacity.
[0130] Place the soft-pack battery in a 25°C oven for 1 hour, charge at 1C to 4.45V, and keep constant voltage until 0.025C is reached. Place the fully charged battery at 85°C and leave it in an open circuit for 8 hours; take out the battery and place it at 25°C for 3 hours, then test the cooling thickness, voltage, and internal resistance (stand for 3 hours → 50g PPG → 400g PPG → voltage → internal resistance) to obtain the thickness, voltage, and internal resistance after storage. At 25°C, discharge at 0.2C to 3.0V, and record the discharge capacity as the remaining capacity after storage. Then charge at 1C to 4.45V, keep constant voltage until 0.025C is reached, and then discharge at 0.2C to 3.0V. Repeat this charge and discharge step twice to obtain the larger value of the discharge capacity, which is the recovery capacity after storage.
[0131] Compare the remaining capacity and the recovered capacity after storage with the initial capacity to obtain the capacity retention rate and capacity recovery rate; compare the internal resistance and thickness after storage with the initial internal resistance and thickness to obtain the internal resistance growth rate and thickness growth rate (Note: 50g and 400g refer to the mass of the iron block applied to the battery when testing the thickness, representing the thickness of the battery tested under different pressures); subtract the voltage after storage from the initial voltage to obtain the voltage drop. The high temperature storage performance test of the soft-pack batteries of Examples 1-8 and Comparative Examples 1-4 is shown in Table 2.
[0132] Table 2 High temperature storage performance test table of soft pack batteries of Examples 1-8 and Comparative Examples 1-4
[0133]
[0134] It can be seen from the test results in Tables 1 and 2 that, compared with the lithium-supplemented negative electrode plate of the comparative example, the pre-lithiation method of the negative electrode plate of the present application can form a SEI film with higher thermal stability on the surface of the negative electrode plate, thereby significantly improving the battery performance. The use of the pre-lithiation negative electrode plate of the present application can improve the battery energy density, and enhance the battery's cycle performance and high temperature resistance.
[0135] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A method for pre-lithiation of a negative electrode plate, characterized in that: include: Providing a negative electrode plate, and supplementing the negative electrode plate with lithium by an electrochemical method to obtain a pre-lithiated negative electrode plate precursor, wherein the temperature of the lithium supplementation is 5° C.-35° C.; The pre-lithiation negative electrode plate precursor is subjected to a reforming treatment to obtain a pre-lithiation negative electrode plate; the reforming treatment includes one or more of a heating treatment, a microwave treatment and a light treatment; the temperature of the heating treatment is 100°C-200°C; the power of the microwave treatment is 1KW-50KW; the wavelength of the light treatment is 10nm-1600nm; and the time of the reforming treatment is 10s-600min.
2. The pre-lithiation method according to claim 1, characterized in that The environment of the reforming treatment includes a vacuum environment or an inert gas atmosphere; the vacuum degree of the vacuum environment is less than or equal to -80Kpa.
3. The pre-lithiation method according to claim 1, characterized in that The electrochemical method includes: immersing the lithium source and the negative electrode plate in an electrolyte, electrically connecting the lithium source and the negative electrode plate to the positive and negative electrodes of a power source respectively, turning on the power supply, replenishing lithium for the negative electrode plate, and forming a SEI film on the surface of the negative electrode plate to obtain a pre-lithiated negative electrode plate precursor.
4. A pre-lithiation device for the pre-lithiation method of the negative electrode sheet according to any one of claims 1 to 3, characterized in that: include: A pre-lithiation component, a reforming component, and a transmission mechanism located between the pre-lithiation component and the reforming component; The pre-lithiation component is used to electrochemically supplement lithium to the negative electrode plate to obtain a pre-lithiation negative electrode plate precursor; the transmission mechanism is used to transfer the pre-lithiation negative electrode plate precursor to the reforming treatment component; the reforming treatment component is used to reform the pre-lithiation negative electrode plate precursor to obtain a pre-lithiation negative electrode plate.
5. The pre-lithiation device according to claim 4, characterized in that: The pre-lithiation component includes a power source, an electrolyte, and a lithium source and a negative electrode plate placed in the electrolyte. The lithium source and the negative electrode plate are electrically connected to the positive electrode and the negative electrode of the power source respectively.
6. The pre-lithiation device according to claim 4 or 5, characterized in that: The reforming treatment component includes a processor and a processing chamber, and the processor is used to perform reforming treatment on the pre-lithiated negative electrode plate precursor; the processor includes one or more of a heater, a microwave processor and a light processor.
7. The pre-lithiation device according to claim 6, characterized in that: The reforming treatment component also includes a vacuum pump or an inert atmosphere device.
8. A pre-lithiation negative electrode plate, characterized in that: The negative electrode is prepared by the pre-lithiation method of the negative electrode sheet as described in any one of claims 1 to 3.
9. A lithium secondary battery, characterized in that: It comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode comprises the pre-lithiation negative electrode plate as claimed in claim 8.