A coal-based lithium-ion battery negative electrode material and preparation method thereof
By carbonizing coal-based raw materials and organic coating materials under gradient heating and cooling, and graphitizing at high temperatures, the problems of complex and high-cost traditional processes have been solved, and the first-time efficiency and cycle performance of lithium-ion battery anode materials have been significantly improved. Suitable for power and energy storage batteries.
Patent Information
- Application Number
- CN202211442734.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-17
AI Technical Summary
The preparation method of traditional coal-based raw materials for lithium-ion battery anode materials is complex and costly, resulting in poor first-time efficiency and cycle performance of the materials produced.
Coal-based raw materials and organic coating materials are used to perform gradient heating and gradient cooling carbonization in an inert or reducing atmosphere, followed by high-temperature graphitization, combined with screening and demagnetization, to obtain coal-based raw material lithium-ion battery negative electrode materials.
The process is simplified, the production cost is reduced, and the first-time efficiency and cycle performance of the material are significantly improved. The obtained anode material has a high degree of graphitization and a low specific surface area, and is suitable for power and energy storage battery applications.
Smart Images

Figure BDA0003947946380000081 
Figure BDA0003947946380000091 
Figure BDA0003947946380000092
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials, and in particular to a negative electrode material for a lithium-ion battery made of coal and a preparation method thereof. Background Art
[0002] In recent years, lithium-ion batteries have been called green new energy products due to their advantages such as high operating voltage, high energy density, good safety performance, long cycle life, and environmental protection and non-toxicity. At present, lithium-ion batteries are widely used in consumer electronics, power tools, electric vehicles, and energy storage power stations. With the explosive development of electric vehicles and wind and solar energy storage, Gaogong Lithium Battery predicts that the market demand for power and energy storage batteries will have an annual compound growth rate of more than 50% in the next five years, which will be accompanied by a surge in demand for negative electrode materials.
[0003] However, the limited supply and high cost of traditional negative electrode raw materials such as low-sulfur petroleum coke and needle coke have become an important factor restricting the further development of the power and energy storage market. Therefore, it is necessary to develop a new type of negative electrode raw material with large supply and low cost.
[0004] Coal raw materials such as anthracite and bituminous coal are widely distributed, have huge reserves, and are low in cost. They have obvious advantages over traditional artificial graphite raw materials, and coal raw materials, especially anthracite, have the advantages of high carbon content, relatively few impurities, and easy graphitization, and are ideal artificial graphite raw materials. However, coal raw materials have high hardness and large specific surface area after crushing; and the ash content of coal raw materials is high. During the graphitization process, oxides and impurity elements such as nitrogen and sulfur will be gasified and removed, resulting in a large number of defects, resulting in low initial efficiency and poor cycle performance of the prepared negative electrode material. In order to improve the above shortcomings of coal raw materials, invention patent CN101651199A discloses a lithium battery carbon negative electrode material and a preparation method thereof, which coats anthracite and a coating material in liquid phase, and then performs a pressurized polymerization reaction, thereby reducing the internal defects of the particles and improving the initial efficiency and cycle performance; however, the method uses a complex liquid phase coating process, is costly, and is difficult to industrialize and mass produce. Invention patent CN111146417A discloses a fast-charging lithium-ion battery spherical graphite negative electrode material and a preparation method thereof. The method uses graphitized anthracite particles to form secondary particle agglomerates through amorphous carbon coating to improve the fast-charging performance of the material; however, the method has a complicated process and high cost, and the surface of the particles is an amorphous carbon structure, which affects the initial efficiency and cycle performance to a certain extent. Summary of the invention
[0005] The main purpose of the present invention is to provide a coal-based raw material lithium-ion battery negative electrode material and a preparation method thereof, aiming to improve the existing method of using bituminous coal to prepare negative electrode materials, which has complex processes, high costs, and poor initial efficiency and cycle performance of the negative electrode materials obtained.
[0006] To achieve the above object, the present invention provides a method for preparing a negative electrode material for a lithium-ion battery using a coal-based raw material, comprising the following steps: uniformly mixing the coal-based raw material and an organic coating material to obtain a mixed material;
[0007] The mixed material is subjected to gradual temperature increase and gradual temperature decrease in an inert or reducing atmosphere to complete carbonization;
[0008] The carbonized material is graphitized to obtain the coal-based raw material lithium-ion battery negative electrode material.
[0009] The coal raw material and the organic coating material in this scheme are mixed evenly at room temperature and pressure, and there is no need to carry out polymerization reaction under high temperature and high pressure, which reduces production costs and makes the process simpler; the coated mixed material is carbonized under an inert gas or a reducing atmosphere, and the carbonization process adopts gradient heating and gradient cooling, so that the carbonized material has better performance, especially the first efficiency and cycle performance are improved; after the carbonization is completed, high-temperature graphitization is carried out, and the graphitized material can also be screened and demagnetized, and finally the coal raw material lithium ion battery negative electrode material is obtained.
[0010] Coal raw materials and organic coating materials can be mixed using the following equipment: VC mixer, horizontal mixer, fusion coating machine, ball mill, granulation kettle. Carbonization can be carried out using a rotary kiln, tunnel kiln, roller kiln, etc. Gradient cooling can be air cooling or water cooling. High-temperature graphitization can be carried out using equipment including Acheson graphitization furnace, box furnace, and continuous graphitization furnace. Inert atmosphere can be used for carbonization under argon atmosphere.
[0011] Preferably, the gradient heating process includes: the first stage: heating from room temperature to 200-300°C, with a heating rate of 4-6°C / min;
[0012] The second stage: heating from 200-300℃ to 300-1000℃, with a heating rate of 3-4℃ / min;
[0013] The third stage: heating from 300-1000℃ to 1000-1400℃, with a heating rate of 1-2℃ / min. The use of a staged gradient heating method for carbonization can make the organic coating material have a better coating effect on the coal raw material, the arrangement of the carbon layer in the mixed material after coating is more orderly, and the performance of the final product negative electrode material is better.
[0014] Preferably, after the temperature is gradually increased to the highest temperature, it is kept warm for 4-10 hours. Similarly, the heat preservation process can completely carbonize the coated mixed material, further improving the performance of the final product negative electrode material.
[0015] Preferably, the gradient cooling process includes: the first stage: cooling from 1000-1400°C to 950-1100°C, with a cooling rate of 2-4°C / min;
[0016] The second stage: cooling from 950-1100℃ to room temperature, with a cooling rate of 4-7℃ / min. In summary, this scheme optimizes the gradient heating and gradient cooling parameters, which can improve the performance of the negative electrode material to a better range.
[0017] Preferably, the graphitization temperature is 3000° C. Graphitization at high temperature changes the carbon atoms from an irregular state to a regularly arranged state, making the graphitized microcrystalline structure more perfect, and the obtained negative electrode material has better performance.
[0018] Preferably, when mixed, the mass ratio of the coal raw material to the organic coating material is 100:(5-20). When the mass ratio is limited to the above, the coating effect of the organic coating material on the coal raw material is better.
[0019] Preferably, the organic coating material is at least one of asphalt, resin or high molecular polymer.
[0020] Preferably, the asphalt comprises at least one of coal asphalt, petroleum asphalt, carbon fiber spinnable asphalt, bonding asphalt or road asphalt;
[0021] The resin includes at least one of epoxy resin or phenolic resin;
[0022] The high molecular polymer includes at least one of polyvinyl alcohol, polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile or polyamide.
[0023] Preferably, the coal raw material is at least one of anthracite, bituminous coal and lignite. Using coal raw materials as the main raw material for preparing negative electrode materials has low cost and also has good performance.
[0024] Preferably, the particle size D50 of the coal raw material is 5-30 μm, and the particle size D50 of the organic coating material is 1-10 μm. When the coal raw material and the organic coating material are controlled within the above particle sizes, a better coating effect is achieved.
[0025] Preferably, the equipment for mixing the coal raw material and the organic coating material can be one of the mixing equipment such as VC mixer, horizontal mixer, fusion coating machine, ball mill, granulation kettle, etc.
[0026] In addition, the present invention also proposes a coal-based raw material lithium-ion battery negative electrode material, which is prepared by the preparation method of any of the above coal-based raw material lithium-ion battery negative electrode materials, and the coal-based raw material lithium-ion battery negative electrode material is a core-shell structure, including a core body and a shell coated on the core body, and the graphitization degree of the core body is greater than the graphitization degree of the shell. The coal-based raw material lithium-ion battery negative electrode material is prepared by the preparation method of the above coal-based raw material lithium-ion battery negative electrode material. Referring to the above scheme, since the coal-based raw material lithium-ion battery negative electrode material adopts all of the above technical schemes, it at least has all the effects brought by the above technical schemes, which will not be repeated here one by one.
[0027] Compared with the prior art, the preparation method of the coal raw material lithium ion battery negative electrode material of the present invention has the following beneficial effects: the coal raw material particles are coated with organic coating materials for pretreatment, and then high-temperature graphitization is performed to obtain a core-shell structure negative electrode material with a high graphitization core and a low graphitization surface. The method can improve the surface defects of the coal raw material after graphitization, improve the tapping, and reduce the specific surface, thereby improving the material processing performance and the first efficiency and cycle performance; at the same time, the method does not need to use a high temperature and high pressure environment during the coating process, is simple and easy, has a large raw material reserve, and is low in cost, which is conducive to further reducing the cost of power and energy storage batteries, and is of great significance to the application and promotion of coal raw materials in the field of lithium ion battery negative electrodes, especially the further cost reduction of power and energy storage batteries, so that the obtained negative electrode material has the characteristics of low cost, good processing performance, high first efficiency, and good cycle performance. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0030] A method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials comprises the following steps:
[0031] First, a coal raw material is crushed, and then the coal raw material and the organic coating material are uniformly mixed to obtain a mixed material. During the mixing, the mass ratio of the coal raw material to the organic coating material is 100:(5-20), the particle size D50 of the coal raw material is 5-30 μm, and the particle size D50 of the organic coating material is 1-10 μm;
[0032] The coal raw material is at least one of anthracite, bituminous coal and lignite; the organic coating material is at least one of asphalt, resin or high molecular polymer; the asphalt includes at least one of coal asphalt, petroleum asphalt, carbon fiber spinnable asphalt, bonding asphalt or road asphalt; the resin includes at least one of epoxy resin or phenolic resin; the high molecular polymer includes at least one of polyvinyl alcohol, polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile or polyamide;
[0033] Preferably, the volatile matter of the coal raw material is ≤10%, the ash content is ≤8%, the sulfur content is ≤1%, and the calorific value is 6000-8900 kcal / kg; more preferably, anthracite with volatile matter ≤8%, ash content ≤5%, sulfur content ≤0.5%, and calorific value ≥6500 kcal / kg is selected; for example, anthracite raw materials produced in Taixi, Ningxia, Yangquan, Shanxi, Xiangzhong, Hunan, and Jiaozuo, Henan can be selected;
[0034] The equipment for mixing the coal raw material and the organic coating material is one of the mixing equipment such as VC mixer, horizontal mixer, fusion coating machine, ball mill, granulation kettle, etc.;
[0035] The mixed material is subjected to gradual temperature increase and gradual temperature decrease in sequence under an inert or reducing atmosphere to complete carbonization;
[0036] The gradient heating process includes: the first stage: heating from room temperature to 200-300°C, with a heating rate of 4-6°C / min; the second stage: heating from 200-300°C to 300-1000°C, with a heating rate of 3-4°C / min; the third stage: heating from 300-1000°C to 1000-1400°C, with a heating rate of 1-2°C / min; after the gradient heating reaches the highest temperature, keeping the temperature for 4-10h;
[0037] The gradient cooling process includes: the first stage: cooling from 1000-1400°C to 950-1100°C, with a cooling rate of 2-4°C / min; the second stage: cooling from 950-1100°C to room temperature, with a cooling rate of 4-7°C / min;
[0038] The carbonized material is graphitized at high temperature, and the finished product is screened and demagnetized to obtain the coal-based raw material lithium-ion battery negative electrode material, and the graphitization temperature is 3000°C.
[0039] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0040] Example 1
[0041] A method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials comprises the following steps:
[0042] Firstly, the anthracite raw material is placed in a pulverizer and crushed to a D50 of 10 to 20 μm, and then the coal raw material and the organic coating material-polyvinyl alcohol are uniformly mixed to obtain a mixed material. During the mixing, the mass ratio of the coal raw material to the organic coating material is 100:5, and the particle size D50 of the organic coating material is 3 to 9 μm;
[0043] The mixed material is subjected to gradient heating and gradient cooling in sequence under an inert atmosphere to complete carbonization: the gradient heating process includes the first stage: heating from room temperature to 280°C, with a heating rate of 4°C / min; the second stage: heating from 280°C to 900°C, with a heating rate of 3°C / min; the third stage: heating from 900°C to 1400°C, with a heating rate of 2°C / min; after the gradient heating reaches the highest temperature, the temperature is kept for 5 hours; the gradient cooling process includes the first stage: cooling from 1400°C to 1100°C, with a cooling rate of 4°C / min; the second stage: cooling from 1100°C to room temperature, with a cooling rate of 5°C / min;
[0044] The carbonized material is graphitized at high temperature, and the finished product is screened and demagnetized to obtain the coal-based raw material lithium-ion battery negative electrode material, and the graphitization temperature is 3000°C.
[0045] Example 2
[0046] A method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials comprises the following steps:
[0047] Firstly, the anthracite raw material is placed in a pulverizer and crushed to a D50 of 15 to 30 μm, and then the coal raw material and the organic coating material-epoxy resin are uniformly mixed to obtain a mixed material. During the mixing, the mass ratio of the coal raw material to the organic coating material is 100:3, and the particle size D50 of the organic coating material is 1 to 10 μm;
[0048] The mixed material is subjected to gradient heating and gradient cooling in a reducing atmosphere to complete carbonization: the gradient heating process includes the first stage: heating from room temperature to 200°C, with a heating rate of 5°C / min; the second stage: heating from 200°C to 800°C, with a heating rate of 4°C / min; the third stage: heating from 800°C to 1200°C, with a heating rate of 2°C / min; after the gradient heating reaches the highest temperature, the temperature is kept for 6 hours; the gradient cooling process includes the first stage: cooling from 1200°C to 1050°C, with a cooling rate of 2°C / min; the second stage: cooling from 1050°C to room temperature, with a cooling rate of 4°C / min;
[0049] The carbonized material is graphitized at high temperature, and the finished product is screened and demagnetized to obtain the coal-based raw material lithium-ion battery negative electrode material, and the graphitization temperature is 3000°C.
[0050] Example 3
[0051] A method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials comprises the following steps:
[0052] Firstly, the anthracite raw material is placed in a pulverizer and crushed to a D50 of 10 to 20 μm, and then the coal raw material and the organic coating material - carbon fiber spinnable asphalt are uniformly mixed to obtain a mixed material. During the mixing, the mass ratio of the coal raw material to the organic coating material is 100:5, and the particle size D50 of the organic coating material is 3 to 9 μm;
[0053] The mixed material is subjected to gradient heating and gradient cooling in a reducing atmosphere to complete carbonization: the gradient heating process includes the first stage: heating from room temperature to 300°C, with a heating rate of 4.5°C / min; the second stage: heating from 300°C to 1000°C, with a heating rate of 4°C / min; the third stage: heating from 1000°C to 1250°C, with a heating rate of 1°C / min; after the gradient heating reaches the highest temperature, the temperature is kept for 8 hours; the gradient cooling process includes the first stage: cooling from 1250°C to 1100°C, with a cooling rate of 3°C / min; the second stage: cooling from 1100°C to room temperature, with a cooling rate of 6°C / min;
[0054] The carbonized material is graphitized at high temperature, and the finished product is screened and demagnetized to obtain the coal-based raw material lithium-ion battery negative electrode material, and the graphitization temperature is 3200°C.
[0055] Example 4
[0056] A method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials comprises the following steps:
[0057] Firstly, the anthracite raw material is placed in a pulverizer and crushed to a D50 of 5 to 15 μm, and then the coal raw material and the organic coating material (carbon fiber spinnable asphalt + polystyrene) are uniformly mixed to obtain a mixed material. During the mixing, the mass ratio of the coal raw material to the organic coating material is 100:20, and the particle size D50 of the organic coating material is 1 to 10 μm;
[0058] The mixed material is subjected to gradient heating and gradient cooling in a reducing atmosphere to complete carbonization: the gradient heating process includes the first stage: heating from room temperature to 250°C, with a heating rate of 6°C / min; the second stage: heating from 250°C to 750°C, with a heating rate of 3.5°C / min; the third stage: heating from 750°C to 1300°C, with a heating rate of 2°C / min; after the gradient heating reaches the highest temperature, the temperature is kept for 10 hours; the gradient cooling process includes the first stage: cooling from 1300°C to 1000°C, with a cooling rate of 4°C / min; the second stage: cooling from 1000°C to room temperature, with a cooling rate of 7°C / min;
[0059] The carbonized material is graphitized at high temperature, and the finished product is screened and demagnetized to obtain the coal-based raw material lithium-ion battery negative electrode material, and the graphitization temperature is 2800°C.
[0060] Comparative Example 1
[0061] The preparation steps and parameters in this comparative example are consistent with those in Example 3, except that no gradient heating process is used for heating. The specific adjustment is: heating from room temperature to 1250° C., V=4° C. / min.
[0062] Comparative Example 2
[0063] The preparation steps and parameters in this comparative example are consistent with those in Example 3, except that no gradient cooling process is used during heating. The specific adjustment is: from 1250°C to room temperature, V = 5°C / min.
[0064] Comparative Example 3
[0065] The preparation steps and parameters in this comparative example are consistent with those in Example 3, with the only difference being that the gradient heating and cooling processes are not adopted during the heating. The specific adjustments are: heating from room temperature to 1250°C, V=4°C / min; cooling from 1250°C to room temperature, V=5°C / min.
[0066] Comparative Example 4
[0067] The preparation steps and parameters in this comparative example are consistent with those in Example 3, with the only difference being that the insulation time is shorter, specifically adjusted to: insulation at 1250° C. for 3 h.
[0068] The performance of the coal-based raw material lithium-ion battery negative electrode materials prepared in the above Examples 1-4 and Comparative Examples 1-4 was tested, and the test results are shown in the following table:
[0069]
[0070] From the test results of Examples 1-4 in the above table, it can be seen that the preparation method of the negative electrode material in this scheme does not adopt high temperature and high pressure mixing reaction conditions when mixing the coal raw material and the organic coating material, but directly mixes them. The process is simple and the cost is low. However, the first discharge capacity of the obtained negative electrode material reaches more than 325mAh / g, the first efficiency is more than 92%, and the number of cycles to maintain 90% capacity is ≥550 times. The product quality of the negative electrode material is better. When preparing the negative electrode material in this scheme, the material can be fully graphitized when the graphitization temperature exceeds 3000℃. The optimal graphitization temperature is about 3050℃. If the temperature is too high, the graphitization process is difficult to produce and the energy consumption is high.
[0071] However, the performance of Comparative Examples 1-4 decreased after the gradient heating, gradient cooling and insulation time in this scheme were not adopted, especially the initial efficiency of the negative electrode material and the number of cycles to maintain 90% capacity. When the insulation time of the highest carbonization temperature was too short, the cycle performance was greatly affected.
[0072] Example 5
[0073] All preparation steps and parameters in this embodiment are the same as those in Embodiment 1, except that the organic coating material in this embodiment is adjusted to carbon fiber spinnable asphalt.
[0074] The performance of the coal-based raw material lithium-ion battery negative electrode material prepared in Example 5 was tested, and the test results are shown in the following table:
[0075]
[0076] From the test results in the above table, it can be seen that when a better organic coating material - carbon fiber spinnable asphalt is used to coat the coal raw material, the first discharge capacity and cycle performance of the obtained negative electrode material become better.
[0077] Example 6
[0078] The preparation steps and parameters in this embodiment are the same as those in Embodiment 2, except that the mass ratio of the coal raw material to the organic coating material in this embodiment is adjusted to 100:12.
[0079] Example 7
[0080] The preparation steps and parameters in this embodiment are the same as those in Embodiment 3, except that the anthracite particle size D50 finally obtained in this embodiment is 8-15 μm, and the polyvinyl alcohol particle size D50 is 3-6 μm.
[0081] The performance of the coal-based raw material lithium-ion battery negative electrode material prepared in the above Examples 6-7 was tested, and the test results are shown in the following table:
[0082]
[0083] It can be seen from the test results in the above table that compared with Example 2, Example 6 has the same other conditions, only the mass ratio of coal raw material and organic coating material is changed to 100:12, wherein the discharge capacity is slightly reduced, mainly because the capacity of the organic coating material that acts as a coating is lower than that of anthracite after graphitization. Therefore, when the amount of coating agent added increases, the capacity will be slightly reduced, but it does not affect the normal use of the negative electrode material. The performance of the obtained negative electrode material is higher than the use standard, and as the amount of coating agent added increases, the cycle performance can be significantly improved. Compared with Example 3, Example 7 has the same other conditions, the anthracite raw material is placed in a pulverizer and crushed to D50 of 8 to 15 μm, and the particle size D50 of the organic coating material is 3 to 6 μm, and the first discharge capacity and cycle performance of the obtained negative electrode material are improved.
[0084] In this scheme, after the coal raw material and the organic coating material are coated, the final product particle size obtained after carbonization and graphitization is preferably D50 13~18μm. Since the added organic coating material has adhesive properties, the particle size will become larger during the coating process. Therefore, the particle size of the coal raw material is preferably D50 8~15μm, and the particle size of the organic coating material is preferably D50 3~6μm.
[0085] Example 8
[0086] The preparation steps and parameters in this embodiment are consistent with those in Example 2, the only difference being that the preferred carbonization system is adopted, which is specifically adjusted as follows: the gradient heating process includes the first stage: heating from room temperature to 300°C, with a heating rate of 6°C / min; the second stage: heating from 300°C to 900°C, with a heating rate of 4°C / min; the third stage: heating from 900°C to 1400°C, with a heating rate of 2°C / min; when the gradient heating reaches the highest temperature, the temperature is kept for 9 hours; the gradient cooling process includes the first stage: cooling from 1400°C to 1050°C, with a cooling rate of 3.5°C / min; the second stage: cooling from 1050°C to room temperature, with a cooling rate of 6°C / min.
[0087] The performance of the coal-based raw material lithium-ion battery negative electrode material prepared in Example 8 was tested, and the test results are shown in the following table:
[0088]
[0089] From the test results in the above table, it can be seen that compared with Example 2, Example 8 has the same other conditions, only the carbonization temperature rise curve and the maximum insulation temperature of carbonization are changed. The optimal maximum temperature of carbonization is 1150°C, and the insulation time is 9h. The performance of the obtained negative electrode material is further improved.
[0090] Example 9
[0091] The preparation steps in Example 9 are consistent with those in Example 1, but better parameters and conditions are selected, that is, the coating agent is carbon fiber spinnable asphalt; the mass ratio of anthracite to carbon fiber spinnable asphalt is 100:12; the graphitization temperature is 3050°C; the particle size D50 of the anthracite after crushing is 8-15μm, and the particle size D50 of the carbon fiber spinnable asphalt is 3-6μm; the gradient heating process of carbonization includes the first stage: heating from room temperature to 300°C, and the heating rate is 6°C / min; the second stage: heating from 300°C to 900°C, and the heating rate is 4°C / min; the third stage: heating from 900°C to 1400°C, and the heating rate is 2°C / min; when the gradient heating reaches the highest temperature, keep warm for 9h; the gradient cooling process includes the first stage: cooling from 1400°C to 1050°C, and the cooling rate is 3.5°C / min; the second stage: cooling from 1050°C to room temperature, and the cooling rate is 6°C / min.
[0092] The performance of the coal-based raw material lithium-ion battery negative electrode material prepared in Example 9 was tested, and the test results are shown in the following table:
[0093]
[0094] It can be seen from the test results in the above table that, after further restriction of the above parameters, the coal-based raw material lithium-ion battery negative electrode material prepared in Example 9 has the best first discharge capacity, first efficiency and cycle performance.
[0095] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a negative electrode material for a lithium-ion battery made of coal, characterized in that: The steps include: The coal raw material and the organic coating material are uniformly mixed to obtain a mixed material; The mixed material is subjected to gradual temperature increase and gradual temperature decrease in an inert or reducing atmosphere to complete carbonization; Graphitizing the carbonized material to obtain the coal-based raw material lithium-ion battery negative electrode material; The gradient heating process comprises: The first stage: heating from room temperature to 200-300℃, with a heating rate of 4-6℃ / min; The second stage: heating from 200-300℃ to 300-1000℃, with a heating rate of 3-4℃ / min; The third stage: heating from 300-1000℃ to 1000-1400℃, with a heating rate of 1-2℃ / min; The gradient cooling process comprises: The first stage: cooling from 1000-1400℃ to 950-1100℃, with a cooling rate of 2-4℃ / min; The second stage: cooling from 950-1100℃ to room temperature, with a cooling rate of 4-7℃ / min.
2. The method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials according to claim 1, characterized in that: After the temperature is gradually increased to the highest temperature, keep it warm for 4-10 hours.
3. The method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials according to claim 1, characterized in that: The graphitization temperature is 2800-3200°C.
4. The method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials according to claim 1, characterized in that: When mixed, the mass ratio of the coal raw material to the organic coating material is 100:(5-20).
5. The method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials according to claim 1, characterized in that: The organic coating material is at least one of asphalt, resin or high molecular polymer; The coal raw material is at least one of anthracite, bituminous coal and lignite.
6. The method for preparing a negative electrode material for a lithium-ion battery made of coal as a raw material according to claim 5, characterized in that: The asphalt includes at least one of coal asphalt, petroleum asphalt, carbon fiber spinnable asphalt, bonding asphalt or road asphalt; The resin includes at least one of epoxy resin or phenolic resin; The high molecular polymer includes at least one of polyvinyl alcohol, polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile or polyamide.
7. The method for preparing a negative electrode material for a lithium-ion battery made of coal raw materials according to claim 1, characterized in that: The particle size D50 of the coal raw material is 5-30 μm, and the particle size D50 of the organic coating material is 1-10 μm.
8. A coal-based lithium-ion battery negative electrode material, characterized in that: The negative electrode material for a lithium-ion battery made from coal raw materials is prepared by the preparation method of the negative electrode material for a lithium-ion battery made from coal raw materials as described in any one of claims 1 to 7. The negative electrode material for a lithium-ion battery made from coal raw materials is a core-shell structure, comprising a core body and a shell coated on the core body, and the graphitization degree of the core body is greater than the graphitization degree of the shell.