Separator for lithium secondary batteries, method for manufacturing the same, and separator manufactured by the same method.

By using a combination of fluorinated adhesive polymers and olefin copolymers in the separator of lithium secondary batteries, the problems of reduced adhesion and increased thermal shrinkage between the porous polymer substrate and the porous coating are solved, achieving higher adhesion and lower thermal shrinkage, thus improving the safety and performance of lithium secondary batteries.

CN115769430BActive Publication Date: 2026-11-17LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180042408.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2021-06-30
Publication Date
2026-11-17
Estimated Expiration
2041-06-30

AI Technical Summary

Technical Problem

Existing lithium secondary battery separators suffer from reduced adhesion (peel strength) and increased thermal shrinkage when using dispersants, resulting in reduced adhesion between the porous polymer substrate and the porous coating.

Method used

A porous coating is formed by using a fluoropolymer and an olefin copolymer of repeating units derived from ethylene monomers and repeating units derived from vinyl acetate monomers, combined with an appropriate dispersant. The weight average molecular weight of the olefin copolymer is controlled to be 400,000 or less, and the weight average molecular weight of the fluoropolymer is between 100,000 and 1,500,000, thereby optimizing the adhesion of the porous coating and the porous polymer substrate.

Benefits of technology

This improves the adhesion (peel strength) between the porous polymer substrate and the porous coating, while reducing the thermal shrinkage rate and enhancing the adhesion (laminar strength) between the separator and the electrode, thus ensuring the safety and performance of the lithium secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115769430B_ABST
    Figure CN115769430B_ABST
Patent Text Reader

Abstract

This disclosure relates to a separator for a lithium-ion secondary battery and a method of manufacturing the same. The separator for the lithium-ion secondary battery comprises: a porous polymer substrate; and a porous coating formed on at least one surface of the porous polymer substrate, comprising inorganic particles, a fluoropolymer (A), and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers. A separator having improved adhesion (peel strength) between the porous coating and the porous polymer substrate and improved adhesion (laminar strength) to the counter electrode can be provided by using an olefin copolymer having predetermined properties, and a method of manufacturing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a method for manufacturing a separator applicable to electrochemical devices such as lithium secondary batteries, and the separator obtained therefrom.

[0002] This application claims priority to Korean Patent Application No. 10-2020-0080604, filed in Korea on June 30, 2020, the disclosure of which is incorporated herein by reference. Background Technology

[0003] Energy storage technology has recently received increasing attention. Efforts to develop electrochemical devices are increasingly being realized, as applications of energy storage technology have expanded to power mobile phones, cameras, and laptops, and even electric vehicles. In this context, electrochemical devices have garnered the most attention. Among these electrochemical devices, the development of rechargeable secondary batteries has been a focus. Recently, active research has been conducted on designing novel electrodes and batteries to improve capacity density and specific energy in the development of these batteries.

[0004] Among commercially available rechargeable batteries, lithium-ion batteries, developed in the early 1990s, have attracted considerable attention due to their higher operating voltage and significantly higher energy density compared to conventional batteries such as Ni-MH, Ni-Cd, and lead-sulfuric acid batteries that utilize aqueous electrolytes.

[0005] Although electrochemical devices such as lithium-ion batteries have been manufactured by many companies, their safety characteristics have shown varying degrees of variation. Evaluating and ensuring the safety of these electrochemical devices is crucial. For example, separators prevent short circuits between the positive and negative electrodes and provide pathways for lithium-ion transport. Therefore, separators are a significant factor affecting battery safety and output characteristics.

[0006] Such separators frequently utilize porous polymer substrates. In addition, separators with a porous coating comprising inorganic particles and a binder polymer disposed on at least one surface of the porous polymer substrate are frequently used to prevent thermal shrinkage of the porous polymer substrate and increase adhesion to the electrodes.

[0007] Here, when preparing the slurry for forming the porous coating, a dispersant is introduced to disperse the inorganic particles. However, the problem with this dispersant is that it leads to a decrease in adhesion (peel strength) and an increase in thermal shrinkage between the porous polymer substrate and the porous coating.

[0008] In these cases, this disclosure relates to providing a separator that, despite the use of a dispersant, exhibits improved adhesion (peel strength) between a porous polymer substrate and a porous coating, and demonstrates reduced thermal shrinkage. Summary of the Invention

[0009] Technical issues

[0010] This disclosure is designed to address problems in the related art, and therefore this disclosure relates to providing a separator having improved adhesion (peel strength) between a porous polymer substrate and a porous coating, and a method of manufacturing the separator.

[0011] This disclosure also relates to providing a partition with a reduced thermal shrinkage rate and a method of manufacturing the partition.

[0012] In addition, this disclosure relates to providing a separator with improved adhesion to electrodes (laminar strength) and a method of manufacturing the same.

[0013] Technical solution

[0014] In one aspect of this disclosure, a partition is provided according to any of the following embodiments.

[0015] According to a first embodiment, a separator for a lithium secondary battery is provided, comprising:

[0016] Porous polymer substrates; and

[0017] A porous coating formed on at least one surface of the porous polymer substrate, comprising inorganic particles, a fluoropolymer (A), and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers.

[0018] The content of the olefin copolymer is 5 parts by weight or less based on 100 parts by weight of the porous coating, and

[0019] The olefin copolymer has a weight-average molecular weight of 400,000 or less.

[0020] According to the second embodiment, a separator for a lithium secondary battery as defined in the first embodiment is provided.

[0021] The content of the repeating unit (a) derived from the ethylene monomer is 20 parts by weight or less based on the total weight of 100 parts by weight of the olefin copolymer.

[0022] According to the third embodiment, a separator for a lithium secondary battery as defined in the first or second embodiment is provided.

[0023] The olefin copolymers described herein have a weight-average molecular weight of 100,000 to 400,000.

[0024] According to the fourth embodiment, a separator for a lithium secondary battery as defined in any of the first to third embodiments is provided.

[0025] The olefin copolymer further comprises repeating units (c) derived from comonomers.

[0026] The repeating units derived from the comonomer include repeating units derived from acrylate monomers, carboxyl-containing C1-C10 monomers, or two or more of these monomers.

[0027] Furthermore, the content of the repeating unit (a) derived from the ethylene monomer is 13 parts by weight or less based on 100 parts by weight of the olefin copolymer.

[0028] According to the fifth embodiment, a separator for a lithium secondary battery as defined in the fourth embodiment is provided.

[0029] The olefin copolymers described herein have a weight-average molecular weight of 350,000 or less.

[0030] According to the sixth embodiment, a separator for a lithium secondary battery as defined in any of the first to fifth embodiments is provided.

[0031] The porous coating further includes a dispersant.

[0032] According to the seventh embodiment, a separator for a lithium secondary battery as defined in any of the first to sixth embodiments is provided.

[0033] The dispersant includes fatty acid compounds, alkylammonium compounds, titanate-based compounds, silane-based compounds, phenolic compounds, or two or more of these.

[0034] According to the eighth embodiment, a separator for a lithium secondary battery as defined in any of the first to seventh embodiments is provided.

[0035] The fluoropolymers mentioned therein include polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trifluoroethylene, polyvinylidene fluoride-co-trifluorochloroethylene, polyvinylidene fluoride-co-tetrafluoroethylene, or two or more thereof.

[0036] According to the ninth embodiment, a separator for a lithium secondary battery as defined in any of the first to eighth embodiments is provided.

[0037] The fluoropolymer adhesive has a weight-average molecular weight of 100,000 to 1,500,000.

[0038] According to the tenth embodiment, a separator for a lithium secondary battery as defined in any of the first to ninth embodiments is provided.

[0039] The separator exhibits adhesion (peel strength) between the porous polymer substrate and the porous coating at 70 gf / 15 mm or greater, and adhesion (laminar strength) between the separator and the electrode at 50 gf / 25 mm or greater.

[0040] In another aspect of this disclosure, a method for manufacturing a separator for a lithium secondary battery is provided according to any of the following embodiments.

[0041] According to the eleventh embodiment, a method for manufacturing a separator for a lithium secondary battery is provided, comprising the following steps:

[0042] Inorganic particles are introduced into a fluoropolymer (A) dissolved in an organic solvent and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers, and the inorganic particles are dispersed therein to prepare a slurry for forming a porous coating; and

[0043] The slurry for forming a porous coating is applied to at least one surface of a porous polymer substrate having multiple pores, and then dried to form a porous coating on at least one surface of the porous polymer substrate.

[0044] The content of the olefin copolymer is 5 parts by weight or less based on 100 parts by weight of the porous coating, and

[0045] The olefin copolymer has a weight-average molecular weight of 400,000 or less.

[0046] According to the twelfth embodiment, a method for manufacturing a separator for a lithium secondary battery as defined in the eleventh embodiment is provided.

[0047] The content of the repeating unit (a) derived from the ethylene monomer is 20 parts by weight or less based on the total weight of 100 parts by weight of the olefin copolymer.

[0048] According to the thirteenth embodiment, a method for manufacturing a separator for a lithium secondary battery, as defined in the eleventh or twelfth embodiment, is provided.

[0049] The organic solvents mentioned therein include ketone solvents.

[0050] According to the fourteenth embodiment, a method for manufacturing a separator for a lithium secondary battery as defined in the thirteenth embodiment is provided.

[0051] The ketone solvent mentioned above includes acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, ethyl propyl ketone, ethyl isobutyl ketone, or two or more of them.

[0052] According to the fifteenth embodiment, a method for manufacturing a separator for a lithium secondary battery as defined in any of the eleventh to fourteenth embodiments is provided.

[0053] The drying step is carried out at a relative humidity of 30% to 80%.

[0054] According to the sixteenth embodiment, a method for manufacturing a separator for a lithium secondary battery as defined in any of the eleventh to fifteenth embodiments is provided.

[0055] The weight ratio of the inorganic particles to the total weight of the fluoropolymer (A) and the olefin copolymer (B) is 50:50 to 90:10.

[0056] In another aspect of this disclosure, a lithium secondary battery according to the following embodiments is provided.

[0057] According to the seventeenth embodiment, a lithium secondary battery is provided, including a positive electrode, a negative electrode, and a separator inserted between the positive electrode and the negative electrode, wherein the separator is the same as that defined in any of the first to tenth embodiments.

[0058] Beneficial effects

[0059] According to embodiments of the present disclosure, a separator having improved adhesion (peel strength) between the porous coating and the porous polymer substrate and improved adhesion (laminar strength) to the counter electrode can be provided by using an olefin copolymer having predetermined properties, and a method for manufacturing the separator.

[0060] According to embodiments of this disclosure, a partition with improved thermal shrinkage rate and a method of manufacturing the partition can also be provided. Attached Figure Description

[0061] The accompanying drawings illustrate preferred embodiments of the present disclosure and, together with the following disclosure, are used to provide a further understanding of the technical features of the present disclosure. Therefore, the present disclosure should not be construed as limited to the drawings. Furthermore, the shape, size, scale, or proportion of some components in the drawings may be exaggerated for the purpose of clearer description.

[0062] Figure 1 Based on the scanning electron microscope (SEM) image of the septum of Comparative Example 4.

[0063] Figure 2 Based on the scanning electron microscope (SEM) image of the septum of Comparative Example 5. Detailed Implementation

[0064] In the following description, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terminology used in the specification and appended claims should not be construed as limited to its common or dictionary meaning, but rather should be interpreted based on its meaning and concept in relation to the technical aspects of the present disclosure, on the principle that the inventors are allowed to appropriately define the terminology for the best interpretation. Therefore, the descriptions presented herein are merely preferred examples for illustrative purposes and are not intended to limit the scope of the present disclosure; thus, it should be understood that other equivalents and modifications may be made thereto without departing from the scope of the present disclosure.

[0065] Throughout the specification, the statement "a portion includes an element" does not exclude the presence of any other elements, but rather implies that the portion may further include other elements.

[0066] As used herein, the terms “approximately,” “substantially,” or similar, when implying an acceptable degree of preparation and material error unique to the claimed meaning, are used to mean from or to the claimed value and to prevent unintentional infringers from improperly using the claimed disclosure, including accurate or absolute values ​​provided to aid in understanding the disclosure.

[0067] In electrochemical devices such as lithium-ion batteries, separators typically use porous polymer substrates, which thus present the problem of exhibiting shrinkage behavior. Therefore, porous coatings have been introduced to reduce the thermal shrinkage rate of the separators.

[0068] Porous coatings are formed by dispersing inorganic particles in a solvent, applying the resulting dispersion to a porous polymer substrate, and then drying. Here, a dispersant is introduced to increase the dispersibility of the inorganic particles. The inventors of this disclosure have discovered that dispersants conventionally used in the dispersant introduction step have a low weight-average molecular weight (Mw) of about 5,000 or less and promote the dispersion of inorganic particles, but lead to problems such as reduced adhesion (peel strength) or increased thermal shrinkage between the porous polymer substrate and the porous coating.

[0069] To address the aforementioned problems, this disclosure relates to providing a separator that, despite the use of a dispersant, exhibits improved adhesion (peel strength) between a porous polymer substrate and a porous coating, and reduced thermal shrinkage.

[0070] In one aspect of this disclosure, a method for manufacturing a separator for a lithium secondary battery is provided, comprising the following steps:

[0071] Porous polymer substrates; and

[0072] A porous coating formed on at least one surface of the porous polymer substrate, comprising inorganic particles, a fluoropolymer (A), and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers.

[0073] The content of the olefin copolymer is 5 parts by weight or less based on 100 parts by weight of the porous coating, and

[0074] The olefin copolymer has a weight-average molecular weight of 400,000 or less.

[0075] The separator for lithium secondary batteries according to embodiments of the present disclosure will be explained in more detail below.

[0076] The separator for a lithium secondary battery according to embodiments of the present disclosure comprises a fluorine-based adhesive polymer (A) and an olefin copolymer (B) in a porous coating.

[0077] According to related technologies, porous coatings are formed using fluoropolymer binders. This type of porous coating is formed by applying a slurry to a porous polymer substrate and drying the solvent under humidified conditions to create pores in the porous coating, while simultaneously forming an adhesive layer on the surface portion of the porous coating. This appears to be because the fluoropolymer binder is dissolved in the solvent. However, when the porous coating is formed using only the fluoropolymer binder, the fluoropolymer binder is only located on the surface portion of the porous coating, such as... Figure 1As shown in the figure, there is a problem of relatively reduced adhesion (peel strength) between the porous coating and the porous polymer substrate.

[0078] Simultaneously, the inventors of this disclosure intend to increase the adhesion (peel strength) between the porous coating and the porous polymer substrate by adding an olefin copolymer (B). The inventors of this disclosure have discovered that when the porous coating is formed using only the olefin copolymer (B), the olefin copolymer does not undergo humidification phase separation but is instead coated onto the surface of the porous polymer substrate in the form of a film. This can be seen from... Figure 2 This can be seen from the text.

[0079] In these cases, according to this disclosure, the simultaneous use of a fluoropolymer and an olefin copolymer allows the porous coating to have a larger fluoropolymer / olefin copolymer weight ratio (A / B) toward the surface portion of the porous coating. In this way, the inventors of this disclosure intend to simultaneously improve the adhesion (peel strength) between the porous coating and the porous polymer substrate and the adhesion (laminar strength) between the separator and the electrode.

[0080] The fluoropolymer (A) is a semi-crystalline polymer that undergoes phase separation under humidification conditions to form a porous structure. For this reason, when the fluoropolymer is combined with inorganic particles and applied to a porous polymer substrate, it is primarily located on the surface of the porous coating, rather than between the substrate and the inorganic particles. In this way, adhesion between the electrodes and separators is improved.

[0081] Fluoropolymer adhesives possess adhesive properties and provide bonding strength between porous polymer substrates and porous coatings, or between porous coatings and electrodes. Furthermore, fluoropolymer adhesives are used to immobilize inorganic particles, preventing them from detaching from the porous coating.

[0082] According to embodiments of this disclosure, fluoropolymer adhesives may include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-hexafluoropropylene (PVDF-CHAPY), polyvinylidene fluoride-co-trifluoroethylene (PVDF-CHAPY), polyvinylidene fluoride-co-tetrafluoroethylene (PVDF-CHAPY), or two or more thereof. For example, fluoropolymer adhesives may include PVDF-CHAPY and PVDF-CHAPY.

[0083] According to embodiments of this disclosure, fluoropolymer adhesive polymers may have a weight-average molecular weight of 100,000 or greater, 200,000 or greater, or 300,000 or greater, and 1,500,000 or less, 1,000,000 or less, or 800,000 or less. For example, fluoropolymer adhesive polymers may have a weight-average molecular weight of 300,000 to 800,000 to ensure processability while ensuring heat resistance and adhesive properties.

[0084] Here, the weight-average molecular weight of the fluoropolymer adhesive can be determined using gel permeation chromatography (GPC, PL GPC220, Agilent Technologies).

[0085] Specifically, the weight-average molecular weight can be determined under the following analytical conditions:

[0086] - Column: PL MiniMixed B x 2

[0087] Solvent: DMF

[0088] - Flow rate: 0.3 mL / min

[0089] - Sample concentration: 2.0 mg / mL

[0090] Injection volume: 10μL

[0091] - Column temperature: 40℃

[0092] - Detector: Agilent RI detector

[0093] - Standard: Polystyrene (corrected using a third-order function)

[0094] -Data Processing: ChemStation

[0095] The olefin copolymer (B) comprises an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers.

[0096] Here, olefin copolymers are used as dispersants to disperse inorganic particles. According to this disclosure, olefin copolymers are also used as adhesive polymers to increase the adhesion (peel strength) between porous polymer substrates and porous coatings.

[0097] Here, the content of the ethylene monomer-derived repeating unit (a) is preferably 20 parts by weight or less based on the total weight of 100 parts by weight of the olefin copolymer. For example, the content of the ethylene monomer-derived repeating unit may be 20 parts by weight or less, 18 parts by weight or less, 16 parts by weight or less, 14 parts by weight or less, 12 parts by weight or less, or 10 parts by weight or less, or 1 to 20 parts by weight, or 4 to 20 parts by weight. The separator according to the embodiments of this disclosure uses the olefin copolymer after it has been dissolved in an organic solvent. When the content of the ethylene monomer-derived repeating unit is 20 parts by weight or less, the olefin copolymer is readily soluble in the organic solvent used according to the embodiments of this disclosure, which is beneficial for forming a porous coating.

[0098] According to embodiments of this disclosure, the content of the olefin copolymer is 5 parts by weight or less per 100 parts by weight of the porous coating. Specifically, the content of the olefin copolymer is 4 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, or 1 to 5 parts by weight, or 1 to 3 parts by weight per 100 parts by weight of the porous coating. When the content of the olefin copolymer is greater than 5 parts by weight, adhesion to the electrode (laminar strength) may not be guaranteed.

[0099] According to embodiments of this disclosure, the olefin copolymer has a weight-average molecular weight of 400,000 or less. When the weight-average molecular weight of the olefin copolymer is greater than 400,000, the dispersibility of the slurry applied to the substrate for forming a porous coating is low, and therefore the slurry cannot be applied at all. In particular, when the inorganic particles in the slurry have large particle sizes and exhibit high settling rates, coating may not be feasible. According to embodiments of this disclosure, the olefin copolymer may have a weight-average molecular weight of 400,000 or less, 350,000 or less, or 300,000 or less, and 50,000 or more, 100,000 or more, or 150,000 or more. For example, the weight-average molecular weight may be from 100,000 to 400,000, particularly from 280,000 to 380,000, to ensure processability while ensuring heat resistance and adhesion properties.

[0100] Here, the weight-average molecular weight of the olefin copolymer can be determined using gel permeation chromatography (GPC: gel permeation chromatography, PL GPC220, Agilent Technologies).

[0101] Specifically, the weight-average molecular weight can be determined under the following analytical conditions:

[0102] - Column: PL MiniMixed B x 2

[0103] Solvent: DMF

[0104] - Flow rate: 0.3 mL / min

[0105] - Sample concentration: 2.0 mg / mL

[0106] Injection volume: 10μL

[0107] - Column temperature: 40℃

[0108] - Detector: Agilent RI detector

[0109] - Standard: Polystyrene (corrected using a third-order function)

[0110] -Data Processing: ChemStation

[0111] According to embodiments of this disclosure, the olefin copolymer further comprises repeating units (c) derived from a comonomer, and said repeating units may include acrylate monomers, carboxyl-containing C1-C10 monomers, or two or more of these monomers. Here, the content of the repeating units (a) derived from the ethylene monomer is preferably 13 parts by weight or less based on 100 parts by weight of the olefin copolymer. Furthermore, the olefin copolymer preferably has a weight-average molecular weight of 350,000 or less. Within the above-defined range, the olefin copolymer is soluble in solvents used according to this disclosure, particularly organic ketone solvents.

[0112] According to embodiments of this disclosure, the acrylate monomer may include, selected from, vinyl acrylate, 2-butoxyethyl acrylate, 2-butoxyethyl methacrylate, 2-ethoxyethyl acrylate, 2-ethoxyethyl methacrylate, 2-ethyl-2-adamantyl acrylate, 2-ethyl-2-adamantyl methacrylate, 2-hydroxyethyl acrylate, 2-methyl-2-adamantyl acrylate, 2-methyl-2-adamantyl methacrylate, benzyl acrylate, cyclohexyl acrylate, di(ethylene glycol) ethyl ether acrylate, di(ethylene glycol) ethyl ether methacrylate, di(ethylene glycol) methyl ether acrylate, dicyclopentyl acrylate, epoxy acrylate, ethylene glycol methyl ether acrylate, ethylene glycol phenyl ether acrylate, hydroxypropyl acrylate, isobornyl acrylate, methyladamantyl acrylate, neopentyl glycol benzoate. The ester, 2-hydroxyethyl methacrylate, adamantyl methacrylate, allyl methacrylate, benzyl methacrylate, cyclohexyl methacrylate, dicyclopentyl methacrylate, epoxycyclohexyl methyl methacrylate, ethylene glycol phenyl ether methacrylate, hydroxybutyl methacrylate, hydroxypropyl methacrylate, isobornyl methacrylate, glycidyl methacrylate, methyl adamantyl methacrylate, methyl methacrylate, methyl glycidyl methacrylate, isobutyl acrylate, tert-butyl acrylate, lauryl acrylate, alkyl acrylate, 2-hydroxyacrylate, trimethoxybutyl acrylate, ethyl carbitol acrylate, 4-hydroxybutyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 3-fluoroethyl acrylate, 4-fluoropropyl acrylate, and triethylsiloxyethyl acrylate.

[0113] According to embodiments of this disclosure, the C1-C10 monomer containing a carboxyl group can be a vinyl acid monomer.

[0114] According to embodiments of this disclosure, carboxyl-containing C1-C10 monomers may include vinyl acid, acrylic acid, methacrylic acid, itaconic acid, or two or more of these.

[0115] Meanwhile, in the partition according to the embodiments of the present disclosure, the porous coating may have a larger weight ratio (A / B) of fluorinated adhesive polymer / olefin copolymer toward the surface portion of the porous coating.

[0116] This is because the fluoropolymer is a crystalline polymer compared to the olefin copolymer. The olefin copolymer used according to this disclosure is an amorphous polymer. Therefore, when the olefin copolymer is applied to a porous polymer substrate under humidified conditions, no phase separation occurs, causing it to remain on one side of the porous polymer substrate compared to the fluoropolymer.

[0117] According to embodiments of this disclosure, the porous coating may further include a dispersant. The dispersant is introduced to prevent the aggregation of solid components during the formation of the porous coating by dispersing inorganic particles.

[0118] For example, the dispersant may be a fatty acid compound, an alkylammonium compound, a titanate-based compound, a silane-based compound, a phenolic compound, or two or more of these.

[0119] For example, fatty acid compounds can be selected from any of the group consisting of C10 or higher acids such as palmitic acid, stearic acid, and oleic acid, or a mixture of two or more of them.

[0120] For example, alkylammonium compounds may include compounds represented by the following chemical formula 1:

[0121] [Chemical Formula 1]

[0122]

[0123] (Where n is an integer from 0 to 15.)

[0124] For example, a titanate-based compound may be any one of the group consisting of monoalkoxy titanates, neoalkoxy titanates, isopropyltris(dioctyl)phosphate titanates, isopropyltris(dioctyl)pyrophosphate titanates, oleyl titanates, isopropyltrioleyl titanates, isopropyltristearate titanates, and isopropyltriisostearate titanates, or a mixture of two or more of them.

[0125] For example, a silane-based compound can be a silane-based compound that includes two or more functional groups selected from the group consisting of vinyl, epoxy, amino, acryloyloxy, methacryloyloxy, methoxy, ethoxy, styryl, isocyanurate, and isocyanate groups.

[0126] In this way, the partition according to the embodiments of this disclosure shows adhesion (peel strength) between the porous polymer substrate and the porous coating at 70 gf / 15 mm or greater, and adhesion (laminar strength) to the counter electrode at 50 gf / 25 mm or greater.

[0127] In another aspect of this disclosure, a method for manufacturing a separator for a lithium secondary battery is provided.

[0128] In particular, the method for manufacturing a separator for lithium secondary batteries includes the following steps:

[0129] Inorganic particles are introduced into a fluoropolymer (A) dissolved in an organic solvent and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers, and the inorganic particles are dispersed therein to prepare a slurry for forming a porous coating; and

[0130] The slurry for forming a porous coating is applied to at least one surface of a porous polymer substrate having multiple pores, and then dried to form a porous coating on at least one surface of the porous polymer substrate.

[0131] The content of the olefin copolymer is 5 parts by weight or less based on 100 parts by weight of the porous coating, and

[0132] The olefin copolymer has a weight-average molecular weight of 400,000 or less.

[0133] First, inorganic particles are introduced into and dispersed in a fluorinated adhesive polymer (A) dissolved in an organic solvent and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers, to prepare a slurry (S1) for forming a porous coating.

[0134] The fluoropolymer (A) and the olefin copolymer (B) are dissolved in an organic solvent. Refer to the above description of the fluoropolymer (A) and the olefin copolymer (B).

[0135] Organic solvents can be ketone solvents. For example, solvents may include acetone, methyl ethylketone, methyl propyl ketone, methyl isobutyl ketone, ethyl propyl ketone, ethyl isobutyl ketone, or two or more of these.

[0136] According to this disclosure, there are no particular limitations on the inorganic particles, provided they are electrochemically stable. That is, there are no particular limitations on the inorganic particles that can be used herein, provided they are within the operating voltage range of the applicable electrochemical device (e.g., based on Li / Li). + It should not cause oxidation and / or reduction in the 0-5V range. In particular, when using inorganic particles with high dielectric constants, the ionic conductivity of the electrolyte can be improved by increasing the degree of dissociation of electrolyte salts such as lithium salts in the liquid electrolyte.

[0137] For the reasons mentioned above, inorganic particles can be inorganic particles with a dielectric constant of 5 or greater, inorganic particles with lithium-ion transport capability, or a combination thereof.

[0138] Inorganic particles with a dielectric constant of 5 or greater may include those selected from Al₂O₃, SiO₂, ZrO₂, AlO(OH), TiO₂, BaTiO₃, and Pb(ZrO₂) x Ti 1-x O3(PZT, where 0 < x < 1), Pb 1-x La x Zr 1-y Ti y O3(PLZT, where 0 < x < 1, 0 < y < 1), (1-x)Pb(Mg) 1 / 3 Nb 2 / 3 Any one of the following groups: O3-xPbTiO3 (PMN-PT, where 0 < x < 1), hafnium oxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZO3, and SiC, or a mixture of two or more of them.

[0139] Inorganic particles with lithium-ion transport capabilities can be selected from lithium phosphate (Li3PO4) and lithium titanium phosphate (Li... x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0<x<2, 0<y<1, 0<z<3), (LiAlTiP) x O y Base glass (1 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2), SiS2-based glass (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), and P2S5-based glass (Li x P y S zAny one of the groups consisting of 0 < x < 3, 0 < y < 3, 0 < z < 7, or a mixture of two or more of them.

[0140] In addition, there are no particular limitations on the average particle diameter of the inorganic particles. However, the inorganic particles preferably have an average particle diameter of 0.001 μm to 10 μm in order to form a porous coating with uniform thickness and provide suitable porosity. The average particle diameter of the inorganic particles is preferably 100 nm to 2 μm, more preferably 150 nm to 1 μm.

[0141] Inorganic particles can be added after they have been pre-crushed to a predetermined average particle diameter. Alternatively, the inorganic particles can be added to the binder polymer solution, then crushed and dispersed, while controlling them to have a predetermined diameter using a ball milling process or similar method.

[0142] The weight ratio of inorganic particles to the total content of the binder polymer can be from 90:10 to 50:50. When the weight ratio of inorganic particles to the total content of the binder polymer meets the above-defined range, the problem of reduced pore size and porosity of the resulting porous coating due to increased binder polymer content can be prevented. It also solves the problem of reduced peel resistance of the resulting porous coating due to decreased binder polymer content.

[0143] Inorganic particles can be dispersed using methods commonly known to those skilled in the art. For example, ultrasonic dispersers, ball mills, bead mills, dispersers, mixers, or the like can be used; in particular, ball mills or bead mills are preferred. The dispersion time can vary depending on the volume to be processed, but can suitably be from 1 hour to 20 hours. The particle size of the pulverized particles can be controlled depending on the size of the beads used in the ball mill or bead mill, or the ball milling (or bead milling) time.

[0144] Then, a slurry for forming a porous coating is applied to a porous polymer substrate having multiple pores and then dried to obtain a separator with a porous coating on the porous polymer substrate (S2).

[0145] According to this disclosure, the porous polymer substrate is a porous membrane that provides channels for lithium-ion transport while electrically insulating the anode and cathode from each other to prevent short circuits. No particular material can be used, as long as it is a material conventionally used as a separator in electrochemical devices.

[0146] In particular, the porous polymer substrate can be a porous polymer film substrate or a porous polymer nonwoven mesh substrate.

[0147] The porous polymer membrane substrate can be a porous polymer membrane comprising polyolefins such as polyethylene or polypropylene. This polyolefin porous polymer membrane substrate can achieve a shut-off function at temperatures ranging from 80°C to 150°C.

[0148] In this document, polyolefin-based porous polymer membranes may be formed from polymers, either alone or in combination of two or more of them, including polyolefin polymers such as polyethylene, polypropylene, polybutene, or polypentene, which contain high-density polyethylene, linear low-density polyethylene, low-density polyethylene, or ultra-high molecular weight polyethylene.

[0149] In addition, porous polymer membrane substrates can be obtained by molding various polymers other than polyolefins, such as polyesters, into a membrane shape. Furthermore, porous polymer membrane substrates can have a stacked structure of two or more membrane layers, wherein each membrane layer can be formed by a polymer, including the polymers mentioned above such as polyolefins or polyesters, alone or in combination of two or more of them.

[0150] In addition to the polyolefins mentioned above, porous polymer membrane substrates and porous polymer nonwoven substrates can also be formed from polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, or polyethylene naphthalene, either alone or in combination.

[0151] While there is no particular limitation on the thickness of the porous polymer substrate, it can range from 1 μm to 100 μm, particularly from 5 μm to 50 μm. Since batteries have recently offered high output / high capacity, it is advantageous to use thin films as porous polymer substrates. The pores present in the porous polymer substrate can have diameters of 10 nm to 100 nm, 10 nm to 70 nm, 10 nm to 50 nm, or 10 nm to 35 nm, and porosity of 5% to 90%, preferably 20% to 80%. However, according to this disclosure, these numerical ranges can be easily changed depending on the specific embodiment or, if necessary.

[0152] The pores in a porous polymer substrate can include various types of pore structures. A pore falls within the scope of this disclosure when either the pore size measured using a porosimeter or the average pore size observed by field emission scanning electron microscopy (FE-SEM) meets the ranges defined above.

[0153] In this paper, in the case of dry separators with a commonly known uniaxial orientation, the median pore size, measured by FE-SEM in the transverse (TD) direction rather than the longitudinal (MD) direction, is taken as the standard pore size. In the case of other porous polymer substrates with a network structure (e.g., wet polyethylene (PE) separators), the pore size measured by a porosimeter is taken as the standard pore size.

[0154] While there are no particular limitations on the thickness of the porous coating, it can range from 1 μm to 10 μm, particularly from 1.5 μm to 8 μm. Furthermore, there are no particular limitations on the porosity of the porous coating, but it is preferably between 35% and 65%.

[0155] The partition according to the embodiments of this disclosure may further include other additives as components of the porous coating, in addition to the inorganic particles and adhesive polymers described above.

[0156] While there are no particular limitations on the process of applying a slurry for forming a porous coating onto a porous polymer substrate, slot coating or dip coating processes are preferred. Slot coating involves applying a slurry supplied via a slot die to the entire surface of the substrate, and the coating thickness can be controlled depending on the flow rate supplied from a metering pump. Dip coating, on the other hand, involves immersing the substrate in a tank containing the composition to perform the coating, and the coating thickness can be controlled depending on the concentration of the composition and the rate at which the substrate is removed from the tank. Furthermore, for more precise control of the coating thickness, post-metering can be performed after immersion using a Mayer bar or similar method.

[0157] The porous polymer substrate coated with a slurry for forming a porous coating can then be dried in a dryer such as an oven to form a porous coating on at least one surface of the porous polymer substrate.

[0158] In porous coatings, inorganic particles are bonded together by a binder polymer, and they stack up and come into contact with each other, thereby forming an interstitial volume between the inorganic particles, and the interstitial volume between the inorganic particles becomes an empty space to form pores.

[0159] In other words, the adhesive polymer binds inorganic particles together, thus maintaining their bonded state. For example, the adhesive polymer connects and fixes inorganic particles together. Furthermore, the pores in the porous coating are formed by interstitial volumes between the inorganic particles, which become vacant spaces. These spaces can be defined by inorganic particles that are substantially facing each other in a closely packed or densely packed structure.

[0160] Drying can be carried out in a drying chamber, where the conditions are not particularly limited due to the use of non-solvents.

[0161] However, since the partition is dried under humidified conditions according to embodiments of this disclosure, the fluoropolymer adhesive can be primarily distributed on the surface of the porous coating. The drying step can be carried out at a relative humidity of 30% or greater, 35% or greater, or 40% or greater, and 80% or less, 75% or less, or 70% or less. For example, the drying step can be carried out at a relative humidity of 40% to 80%. Furthermore, the drying step can be carried out at a temperature of 20°C to 70°C for 0.1 minutes to 2 minutes.

[0162] In another aspect of this disclosure, an electrochemical device is provided, including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator described above according to the embodiments of this disclosure.

[0163] Electrochemical devices include any device that performs an electrochemical reaction, and specific examples include all types of primary cells, secondary cells, fuel cells, solar cells, or capacitors such as supercapacitors. In particular, lithium secondary cells, including lithium metal secondary cells, lithium-ion secondary cells, lithium polymer secondary cells, or lithium-ion polymer batteries, are preferred among secondary cells.

[0164] There are no particular limitations on the positive and negative electrodes used in conjunction with the separator according to this disclosure, and they can be obtained by incorporating electrode active materials into the electrode current collector using methods generally known in the art. Non-limiting examples of positive electrode active materials include conventional positive electrode active materials that can be used as positive electrodes in conventional electrochemical devices. In particular, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or lithium composite oxides containing combinations thereof are preferred. Non-limiting examples of negative electrode active materials include conventional negative electrode active materials that can be used as negative electrodes in conventional electrochemical devices. In particular, materials such as lithium metal or lithium alloys (which intercalate lithium), carbon, petroleum coke, activated carbon, graphite, or other carbonaceous materials are preferred. Non-limiting examples of positive electrode current collectors include foils made of aluminum, nickel, or combinations thereof. Non-limiting examples of negative electrode current collectors include foils made of copper, gold, nickel, copper alloys, or combinations thereof.

[0165] The electrolyte that can be used in the electrochemical device according to this disclosure is having A + B - Salts of structure, in which A + Including, for example, Li + Na + K + alkali metal cations such as B, or combinations thereof, - Including PF6 - BF4 - Cl - ,Br - I - ClO4 - AsF6 - CH3CO2 - CF3SO3 - N(CF3SO2)2 - C(CF2SO2)3 - Anions such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma-butyrolactone (γ-butyrolactone), or combinations thereof, are present in organic solvents, including but not limited to these.

[0166] Depending on the manufacturing process of the final product and the desired properties of the final product, electrolyte injection can be performed at an appropriate step during the process used to manufacture the battery. That is, electrolyte injection can be performed before battery assembly or as a final step in battery assembly.

[0167] The embodiments will then be described in more detail so that this disclosure can be readily understood. However, the following embodiments may be embodied in many different forms and should not be construed as limited to the exemplary implementations set forth herein. Rather, these exemplary implementations are provided so that this disclosure will be thorough and complete, and will fully convey the scope of this disclosure to those skilled in the art.

[0168] Comparative Example 1

[0169] First, polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride-co-trifluorochloroethylene (PVDF-CTFE), with a weight average molecular weight of approximately 400,000, were introduced into acetone as a solvent and dissolved therein at 50°C for approximately 4 hours to prepare an adhesive polymer solution. Next, aluminum hydroxide (Al(OH)3) (particle size: 900 nm) as inorganic particles was introduced into the adhesive polymer solution. Then, a liquid fatty acid (BYK Co., P104) as a dispersant was introduced therein. Here, the weight ratio of inorganic particles: fluorinated polymer: dispersant was controlled at 75:23:2 to prepare a slurry for forming a porous coating. Specifically, the weight ratio of inorganic particles: polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP): polyvinylidene fluoride-co-trifluorochloroethylene (PVDF-CTFE): dispersant is controlled at 75:18:5:2. Here, the solids content (solvent-free slurry) is 15 parts by weight based on 100 parts by weight of slurry.

[0170] The slurry used to form the porous coating was applied to both surfaces of a 9 μm thick polyethylene porous membrane (porosity: 45%) at 23°C and 45% relative humidity via a dip-coating process, followed by drying to obtain a separator with a porous coating of 6 μm thickness on each surface. The test results are shown in Table 1 below.

[0171] Comparative Example 2

[0172] The separator was obtained in the same manner as in Comparative Example 1, except that a silane-based compound (BYK Co., C8002) was introduced as a dispersant instead of a liquid fatty acid (BYK Co., P104). The test results are shown in Table 1 below.

[0173] Example 1

[0174] First, polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP) and polyvinylidene fluoride-co-trifluorochloroethylene (PVDF-CTFE) with a weight average molecular weight of about 400,000, serving as fluoropolymers (A), were introduced into acetone as a solvent and dissolved therein at 50°C for about 4 hours to prepare a polymer solution. Next, aluminum hydroxide (Al(OH)3) (particle size: 900 nm) as inorganic particles was introduced into the polymer solution. Then, an olefin copolymer (B) (content of repeating units derived from ethylene monomer: 6 parts by weight based on 100 parts by weight of the olefin copolymer, weight average molecular weight: 280,000) and a liquid fatty acid compound (BYK Co., P104) as a dispersant were introduced therein. Here, the weight ratio of inorganic particles: fluorinated polymer: olefin copolymer: dispersant is controlled at 75:23:1:1 to prepare a slurry for forming a porous coating. Specifically, the weight ratio of inorganic particles: polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP): polyvinylidene fluoride-co-trifluorochloroethylene (PVDF-CTFE): olefin copolymer: dispersant is controlled at 75:18:5:1:1. Here, the solids content (solvent-free slurry) is 15 parts by weight based on 100 parts by weight of slurry.

[0175] The slurry used to form the porous coating was applied to both surfaces of a 9 μm thick polyethylene porous membrane (porosity: 45%) at 23°C and 45% relative humidity via a dip-coating process, followed by drying to obtain a separator with a porous coating of 6 μm thickness on each surface. The test results are shown in Table 1 below.

[0176] Example 2

[0177] The separator was obtained in the same manner as in Example 1, except that a silane-based compound (BYK Co., C8002) was introduced as a dispersant instead of a liquid fatty acid (BYK Co., P104). The test results are shown in Table 1.

[0178] Example 3

[0179] The separator was obtained in the same manner as in Example 1, except that only the olefin copolymer (B) was used, instead of the olefin copolymer (B) and liquid fatty acid (BYK Co., P104). The test results are shown in Table 1.

[0180] [Table 1]

[0181]

[0182] Examples 4 and 5

[0183] The separator was obtained in the same manner as in Example 3, except that the content of the olefin copolymer (B) was controlled as shown in Table 2 below. The test results are shown in Table 2.

[0184] Comparative Example 3

[0185] The separator was obtained in the same manner as in Example 3, except that the content of the olefin copolymer (B) was controlled as shown in Table 2 below. The test results are shown in Table 2.

[0186] [Table 2]

[0187]

[0188]

[0189] Comparative Example 4

[0190] First, polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP), with a weight-average molecular weight of approximately 400,000, was introduced into acetone as a solvent and dissolved therein at 50°C for approximately 4 hours to prepare an adhesive polymer solution with a solids content of 5 parts by weight. Here, the solids content in the adhesive polymer solution was calculated according to the formula [(fluorinated adhesive polymer) / (fluorinated adhesive polymer + solvent)] × 100.

[0191] An adhesive polymer solution was applied to both surfaces of a 9 μm thick porous polyethylene membrane (porosity: 45%) at 23°C and 45% relative humidity via a dip-coating process, followed by drying to obtain a separator with a porous coating of 2 μm thickness on each surface. Test results are shown in... Figure 1 middle.

[0192] Comparative Example 5

[0193] First, the olefin copolymer (B) is introduced into acetone as a solvent and dissolved therein at 50°C for about 4 hours to prepare an adhesive polymer solution with a solids content of 5 parts by weight. Here, the solids content in the adhesive polymer solution is calculated according to the formula [(olefin copolymer) / (olefin copolymer + solvent)]×100.

[0194] An adhesive polymer solution was applied to both surfaces of a 9 μm thick porous polyethylene membrane (porosity: 45%) at 23°C and 45% relative humidity via a dip-coating process, followed by drying to obtain a separator with a porous coating of 2 μm thickness on each surface. Test results are shown in... Figure 2 middle.

[0195] Examples 6 and 7

[0196] The separator was obtained in the same manner as in Example 3, except that the content of the olefin copolymer (B) was controlled as shown in Table 3 below. The test results are shown in Table 3 below.

[0197] Comparative Example 6

[0198] The separator was obtained in the same manner as in Example 3, except that the content of the olefin copolymer (B) was controlled as shown in Table 3 below. The test results are shown in Table 3.

[0199] [Table 3]

[0200]

[0201] Test methods

[0202] 1) Methods for measuring thickness

[0203] The thickness of each partition was measured using a thickness gauge (Mitutoyo Co., VL-50S-B).

[0204] 2) Methods for determining thermal shrinkage rate

[0205] The heat shrinkage rate of each partition is calculated by measuring the change in length in the longitudinal (MD) and transverse (TD) directions and using the formula [(initial length - length after heat shrinkage at 150°C for 30 minutes) / (initial length)] × 100.

[0206] 3) Determination of adhesion (peel strength) between the porous polymer substrate and the porous coating.

[0207] Each separator according to the embodiments and comparative examples was cut to a size of 15mm × 100mm. Double-sided tape was attached to the glass plate, and the porous coated surface of the separator was attached to the tape. Then, the ends of the separators were mounted to a UTM instrument (LLOYD Instrument LF Plus), and forces were applied at 180° and 300mm / min. The force required to separate the porous coating from the porous polymer substrate was measured.

[0208] 4) Determination of adhesion (laminar strength) between electrodes and separators

[0209] To determine the adhesion (laminar strength) between the electrode and each separator, the anode was prepared as described.

[0210] First, artificial graphite, carbon black, carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed with water in a weight ratio of 96:1:1:2 to obtain an anode slurry. The anode slurry was prepared at a concentration of 3.5 mAh / cm³. 2 The capacity is coated onto copper foil to form a thin electrode plate, which is then dried at 135°C for 3 hours or longer, and then pressed to obtain the anode.

[0211] The obtained anodes were cut to a size of 25 mm × 100 mm. Each separator according to the examples and comparative examples was cut to a size of 15 mm × 100 mm. The separators were stacked with the anodes, the stack was inserted between 100 μm thick PET films and adhered using a flat press. Here, the flat press was heated and pressurized at 60°C for 1 second at a pressure of 6.5 MPa. The adhered separators and anodes were attached to a glass slide using double-sided tape. The ends of the separators (10 mm or less from the end of the adhered surface) were peeled off and attached to the 25 mm × 100 mm PET film using single-sided tape, so that they could be joined longitudinally. The glass slide was then mounted to the lower fixture of a UTM instrument (LLOYD Instrument LF Plus), and the PET film adhered to the separators was mounted to the upper fixture of the UTM instrument. Force was then applied at a rate of 180° and 300 mm / min. The force required to separate the anode from the porous coating facing the anode was measured.

[0212] 5) Average particle diameter (D50) of the inorganic particles included in the slurry.

[0213] The average particle diameter of the inorganic particles in the slurry was determined using a particle size analyzer (product name: MASTERSIZER 3000, available from Malvern).

[0214] 6) Settling rate (μm / s) of the slurry used to form the porous coating

[0215] The settling rate of the slurry used to form the porous coating was determined by introducing the slurry into a dispersion analyzer (product name: Lumisizer, available from LUM), applying centrifugal force to it while rotating it at a rate of 1,000 rpm, and measuring the settling rate over time.

[0216] 7) Method for determining weight-average molecular weight

[0217] The weight-average molecular weights of the olefin copolymers and fluoropolymer binders used in each example and comparative example were determined by gel permeation chromatography (GPC, PL GPC220, Agilent Technologies) under the following conditions:

[0218] - Column: PL MiniMixed B x 2

[0219] Solvent: DMF

[0220] - Flow rate: 0.3 mL / min

[0221] - Sample concentration: 2.0 mg / mL

[0222] Injection volume: 10μL

[0223] - Column temperature: 40℃

[0224] - Detector: Agilent RI detector

[0225] - Standard: Polystyrene (corrected using a third-order function)

[0226] -Data Processing: ChemStation

[0227] As can be seen from Table 1, in Comparative Examples 1 and 2 without using olefin copolymers, the adhesion (peel strength) between the porous coating and the porous polymer substrate is significantly lower than in the Examples, and the thermal shrinkage is also poor.

[0228] As can be seen from Table 2, when the content of ethylene monomer-derived repeating units in the olefin copolymer is 7 parts by weight, the adhesion (laminar strength) between the separator and the anode is significantly lower than that in the example.

[0229] As can be seen from Table 3, when the weight-average molecular weight of the olefin copolymer is greater than 400,000, the slurry exhibits low dispersibility, making it difficult to form a porous coating.

[0230] In contrast, as can be seen from Examples 1 to 7 according to this disclosure, a separator and a method thereof can be provided that simultaneously have improved adhesion (peel strength) between the porous coating and the porous polymer substrate and improved adhesion (laminar strength) to the counter electrode by using an olefin copolymer having predetermined properties.

Claims

1. A separator for a lithium secondary battery, comprising: Porous polymer substrate; and A porous coating formed on at least one surface of the porous polymer substrate, comprising inorganic particles, a fluoropolymer (A), and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers. The content of the olefin copolymer is 5 parts by weight or less based on 100 parts by weight of the porous coating, and The olefin copolymer has a weight-average molecular weight of 100,000 to 400,000.

2. The separator for a lithium secondary battery according to claim 1, wherein the content of the repeating unit (a) derived from the ethylene monomer is 20 parts by weight or less based on the total weight of 100 parts by weight of the olefin copolymer.

3. The separator for a lithium secondary battery according to claim 1, wherein the olefin copolymer further comprises repeating units (c) derived from comonomers, the repeating units derived from comonomers comprising repeating units derived from acrylate monomers, carboxyl-containing C1-C10 monomers, or two or more of the monomers thereof, and the content of the repeating units (a) derived from ethylene monomers is 13 parts by weight or less based on 100 parts by weight of the olefin copolymer.

4. The separator for a lithium secondary battery according to claim 3, wherein the olefin copolymer has a weight-average molecular weight of 350,000 or less.

5. The separator for a lithium secondary battery according to claim 1, wherein the porous coating further comprises a dispersant.

6. The separator for a lithium secondary battery according to claim 5, wherein the dispersant comprises a fatty acid compound, an alkylammonium compound, a titanate compound, a silane compound, a phenolic compound, or two or more thereof.

7. The separator for a lithium secondary battery according to claim 1, wherein the fluorine-based adhesive polymer comprises polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trifluoroethylene, polyvinylidene fluoride-co-trifluorochloroethylene, polyvinylidene fluoride-co-tetrafluoroethylene, or two or more thereof.

8. The separator for a lithium secondary battery according to claim 1, wherein the fluorine-based adhesive polymer has a weight-average molecular weight of 100,000 to 1,500,000.

9. The separator for a lithium secondary battery according to claim 1, wherein the separator exhibits adhesion (peel strength) between the porous polymer substrate and the porous coating at a ratio of 70 gf / 15 mm or greater, and adhesion (laminar strength) between the separator and the electrode at a ratio of 50 gf / 25 mm or greater.

10. A method for manufacturing a separator for a lithium secondary battery, comprising the following steps: Inorganic particles are introduced into a fluorinated adhesive polymer (A) dissolved in an organic solvent and an olefin copolymer (B) having repeating units (a) derived from ethylene monomers and repeating units (b) derived from vinyl acetate monomers, and the inorganic particles are dispersed therein to prepare a slurry for forming a porous coating. and The slurry for forming a porous coating is applied to at least one surface of a porous polymer substrate having multiple pores, and then dried to form a porous coating on at least one surface of the porous polymer substrate. The content of the olefin copolymer is 5 parts by weight or less based on 100 parts by weight of the porous coating, and The olefin copolymer has a weight-average molecular weight of 100,000 to 400,000.

11. The method of manufacturing a separator for a lithium secondary battery according to claim 10, wherein the content of the repeating unit (a) derived from the ethylene monomer is 20 parts by weight or less based on the total weight of 100 parts by weight of the olefin copolymer.

12. The method of manufacturing a separator for a lithium secondary battery according to claim 10, wherein the organic solvent is a ketone solvent.

13. The method of manufacturing a separator for a lithium secondary battery according to claim 12, wherein the ketone solvent comprises acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, ethyl propyl ketone, ethyl isobutyl ketone, or two or more thereof.

14. The method of manufacturing a separator for a lithium secondary battery according to claim 10, wherein the drying step is carried out at a relative humidity of 30% to 80%.

15. The method of manufacturing a separator for a lithium secondary battery according to claim 10, wherein the weight ratio of the inorganic particles to the total weight of the fluorinated adhesive polymer (A) and the olefin copolymer (B) is from 50:50 to 90:

10.

16. A lithium secondary battery comprising a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the same as that defined in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Nitrogen supply nozzle

    KR1020200080604A

  • Separator fabrication method, separator fabricated thereby, and electrochemical element comprising separator

    CN110521021A