A micro battery and its preparation method and application
The micro-battery with high energy density and power density is manufactured through micro-machining technology, which solves the problems of difficulty in safety monitoring of high-speed rotating equipment and insufficient energy supply capacity of traditional small button batteries, and achieves stable energy output and robustness in extreme environments. sexually powered.
Patent Information
- Application Number
- CN202211499281.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-28
AI Technical Summary
It is difficult to monitor the safety of existing high-speed rotating equipment. Traditional small button batteries have limited energy supply capabilities in extreme environments and cannot effectively provide high energy density and power density.
Micromachining technology is used to manufacture manganese dioxide/3,4-ethylenedioxythiophene polymer microelectrodes and zinc-coated carbon nanotube microelectrodes are assembled. The battery active materials are loaded through a three-dimensional porous structure, with manganese sulfate/zinc sulfate/xanthan. Gel electrolyte forms a micro battery with high energy density and power density.
It has realized a micro battery that provides high energy density and power density in extreme environments. It is suitable for high-speed rotation and vibration environments, has enhanced robustness, and is suitable for energy supply for equipment such as intelligent network nodes, micro-nano sensors, and micro robots.
Smart Images

Figure CN115863530B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the cross-technical field of nano energy storage materials, micro-machining technology and detection technology, and in particular to a micro-battery and a preparation method and application thereof. Background Art
[0002] Currently known high-speed rotating equipment has the problem of difficulty in monitoring its safety. For example, for a long time, the on-site monitoring technology of high-speed rotating equipment represented by ship propellers, EMU wheels, aircraft compressors, etc. has been difficult to achieve, and the only way to carry out maintenance is to adopt cumbersome maintenance methods such as multi-manual mechanical disassembly, which greatly increases the maintenance cost.
[0003] Micro batteries have the advantages of small size, light weight, simple structure, etc. They can provide high energy density and power density under the conditions of extremely small (less than 5mm), extremely thin (less than 200μm), and extremely light (less than 50mg). Therefore, micro batteries can be used in more scenarios compared to commercial small button batteries. Therefore, they can provide energy for smart network nodes, micro-nano sensors, micro robots and other equipment in extreme environments.
[0004] However, in order to increase the energy density, the current small button batteries mostly use dense active material loading methods, and the electron / ion conduction is extremely poor. Therefore, the voltage platform is low and the operating current is extremely small. They can only power electronic devices at the nanoampere to sub-microampere level, which greatly limits their use scenarios. Summary of the invention
[0005] In view of this, the present invention provides a micro battery and a preparation method and application thereof to solve the problem of difficulty in safety monitoring of existing high-speed rotating equipment.
[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0007] A method for preparing a micro battery, characterized in that it comprises the following steps:
[0008] S1. Fabrication of manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode
[0009] S11, mixing nickel sulfate and ammonium sulfate to obtain a mixed solution A; in the mixed solution A, using a metal micro-interdigitated electrode as a working electrode, and adopting a three-electrode deposition method under a constant voltage to obtain a porous metal microelectrode;
[0010] S12, mixing manganese acetate and 3,4-ethylenedioxythiophene to obtain a mixed solution B, and in the mixed solution B, using a porous metal microelectrode as a working electrode, and adopting an electrodeposition process under a constant voltage to obtain a manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode;
[0011] S2. Fabrication of zinc-coated carbon nanotube microelectrodes
[0012] S21, dispersing carbon nanotubes in an ethanol solution, adding magnesium nitrate, and mixing well to obtain a mixed solution C, in which a platinum sheet and a brass microelectrode are used as positive and negative electrodes, respectively, and an electrophoresis process is used under a constant voltage power supply to obtain an interdigitated microelectrode;
[0013] S22, mixing zinc sulfate and sodium sulfate to obtain a mixed solution D, in which an interdigitated microelectrode is used as a working electrode, and a constant voltage deposition method is used to deposit metal zinc nanosheets on the surface of the working electrode to obtain a zinc-coated carbon nanotube microelectrode;
[0014] S3. Assembly of micro batteries
[0015] S31, using the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode and the zinc-coated carbon nanotube microelectrode as a positive electrode and a negative electrode, respectively, and assembling them under an optical microscope;
[0016] S32. The assembled electrode surface is coated with manganese sulfate / zinc sulfate / xanthan gum gel electrolyte, and a micro battery is obtained after packaging.
[0017] According to the above scheme, in the mixed solution A, the mass ratio of the nickel sulfate to the ammonium sulfate is 1:(1-10), and in the mixed solution B, the mass ratio of the manganese acetate to the 3,4-ethylenedioxythiophene is 0.5-(10:1).
[0018] According to the above scheme, the three-electrode deposition method under constant voltage described in step S11 includes: using a metal micro-interdigitated electrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode, and depositing for 10 to 200 seconds under a constant voltage of -3 to -5V.
[0019] According to the above scheme, in step S12, the electrodeposition process includes: using a metal micro-interdigitated electrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode, at a voltage range of 0 to 0.9 V, using a voltage of 1 to 50 mV s -1 Scanning speed, 10 to 200 cycles of deposition.
[0020] According to the above scheme, in the mixed solution C, the mass ratio of the carbon nanotubes to the magnesium nitrate is 0.5 to (10:1), and in the mixed solution D, the mass ratio of the zinc sulfate to the sodium sulfate is 1 to (5:1).
[0021] According to the above scheme, the electrophoresis process in step S21 includes: a platinum sheet as a positive electrode, and a brass, copper, nickel, stainless steel or titanium microelectrode as a negative electrode.
[0022] According to the above scheme, the constant voltage deposition method in step S22 includes: constant voltage of 10 to 60 V, and deposition time of 1 to 30 min.
[0023] According to the above scheme, the method for preparing the manganese sulfate / zinc sulfate / xanthan gum gel electrolyte in step S32 includes: adding manganese sulfate and zinc sulfate into water, stirring evenly by ultrasonication, adding xanthan gum, and mixing evenly.
[0024] On the basis of the above scheme, the second object of the present invention is to provide a micro battery prepared by the above-mentioned micro battery preparation method.
[0025] Based on the above scheme, the third purpose of the present invention is to provide the application of micro batteries in sensor systems for monitoring high-speed rotation and closed components.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] (1) The present invention uses micro-interdigitated electrodes manufactured based on micro-machining technology to perform electrodeposition to construct a three-dimensional porous structure. After the battery active material is loaded on the surface of the three-dimensional porous structure, it is matched with the negative electrode of the interdigitated microelectrode, coated with electrolyte and packaged to obtain a micro-battery. The structure is simple, the positive and negative electrodes are physically separated, and the robustness is stronger, which can cope with stronger vibration, acceleration and other conditions.
[0028] (2) The micro-battery produced by the present invention has the advantages of small size, thin thickness, light weight, extremely high power density / energy density, simple production, and easy integration. After being integrated with a small commercial sensor system, it can provide stable energy output on the one hand, and can adapt to high-speed rotation and vibration environments on the other hand, showing the potential for commercial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a schematic diagram of the main process flow of the micro battery according to an embodiment of the present invention;
[0031] Figure 2 The scanning electron microscope image and energy spectrum characterization image of the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode described in Example 1 of the present invention;
[0032] Figure 3This is a graph showing the electrochemical performance characterization results of the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode described in Example 1 of the present invention;
[0033] Figure 4 This is a diagram showing the electrochemical performance characterization and application demonstration of the microbattery described in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0035] It should be noted that in the description of the embodiments of the present application, the description of the term "some specific embodiments" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0036] The “in the range of” described in this embodiment includes both end values, such as “in the range of 1 to 100” includes both end values of 1 and 100.
[0037] An embodiment of the present invention provides a method for preparing a micro battery, comprising the following steps:
[0038] S1. Fabrication of manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode
[0039] S11. Mix nickel sulfate and ammonium sulfate, ultrasonicate at room temperature for 15 minutes, and stir for 15 minutes to obtain a light green mixed solution A. In the mixed solution A, use a micro-machined metal micro-interdigitated electrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode, and deposit for 10 to 200 seconds at a constant voltage of -3 to -5 V to obtain a porous metal microelectrode.
[0040] Among them, the metal micro-interdigitated electrodes made by micro-machining refer to metal four-finger micro-electrodes prepared by laser engraving, machine tool processing, and wet etching. The width of a single interdigitated finger is 360μm, the specifications of the entire electrode are 3900μm×3600μm, and the thickness is 10 to 200μm.
[0041] S12. Mix manganese acetate and 3,4-ethylenedioxythiophene (EDOT), and ultrasonically stir to obtain a mixed solution B. In the mixed solution B, a porous metal microelectrode is used as a working electrode, a platinum sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode. At a voltage range of 0 to 0.9 V, a scan rate of 1 to 50 mV s-1 is used, and cyclic deposition is performed for 10 to 200 cycles to obtain a manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode.
[0042] Among them, in the mixed solution A, the mass ratio of nickel sulfate to ammonium sulfate is 1:(1-10), and in the mixed solution B, the mass ratio of manganese acetate to 3,4-ethylenedioxythiophene is 0.5-(10:1).
[0043] S2. Fabrication of zinc-coated carbon nanotube microelectrodes
[0044] S21. Disperse carbon nanotubes (CNT) in ethanol solution, add magnesium nitrate, and ultrasonicate for 50-70 minutes. Mix well to obtain a black mixed solution C. In the mixed solution C, use a platinum sheet and a brass microelectrode as the positive and negative electrodes, respectively. Under a constant voltage, electrophoresing the carbon nanotubes on the surface of the microelectrode, and drying to obtain a uniform black interdigitated microelectrode.
[0045] S22. Mix zinc sulfate and sodium sulfate to obtain a mixed solution D. In the mixed solution D, a three-electrode system is composed of an interdigitated microelectrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode. A constant voltage deposition method is used to deposit metal zinc nanosheets on the surface of the working electrode to obtain a zinc-coated carbon nanotube microelectrode.
[0046] In the mixed solution C, the mass ratio of carbon nanotubes to magnesium nitrate is 0.5 to (10:1), and in the mixed solution D, the mass ratio of zinc sulfate to sodium sulfate is 1 to (5:1).
[0047] S3. Assembly of micro batteries
[0048] S31, using a manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode and a zinc-coated carbon nanotube microelectrode as the positive electrode and the negative electrode, respectively, and assembling them under an optical microscope;
[0049] S32. The assembled electrode surface is coated with manganese sulfate / zinc sulfate / xanthan gum gel electrolyte, and then covered with a PE square film. The PE square film is then sealed around with a sealant to obtain a micro battery.
[0050] The preparation method of manganese sulfate / zinc sulfate / xanthan gum gel electrolyte comprises: adding manganese sulfate and zinc sulfate into water, stirring ultrasonically until clarified, adding xanthan gum with a mass ratio of 0.1 to 2 g / ml, stirring at 40° C. for 50 to 70 minutes, and mixing evenly to obtain a gel electrolyte.
[0051] The present invention places a micro-machined interdigitated metal thin electrode in a nickel sulfate and ammonium sulfate solution of a certain concentration, adopts an electrodeposition bubble template method, and quickly constructs a vertical three-dimensional porous structure composed of micron nickel particle clusters on the surface of the interdigitated microelectrode. Then, 3,4-ethylenedioxythiophene is mixed with a certain concentration of manganese acetate, and a cyclic voltammetry deposition method is adopted on the surface of the three-dimensional porous nickel structure to obtain an active material film mixed with manganese dioxide / 3,4-ethylenedioxythiophene polymer in one step. The active material film has a vertical three-dimensional porous structure similar to that of three-dimensional porous nickel, and has a large electrolyte / active material contact area while obtaining a high active material loading amount. The obtained interdigitated microelectrode is a positive electrode, which is combined with a zinc interdigitated negative electrode, coated with a manganese sulfate / zinc sulfate / xanthan gum gel electrolyte, and encapsulated to obtain a zinc-manganese microbattery with manganese dioxide as the main active material.
[0052] It is understandable that the microbattery with a double-finger structure divides the positive and negative electrodes by a very small interdigital gap, and there is a narrow positive and negative electrode ion transmission channel between the two electrodes. As the thickness of the positive and negative electrode materials increases, the positive and negative electrode ion transmission distance remains unchanged, so it is considered to be the microbattery configuration with the highest power density. Therefore, the microbattery prepared by the present invention has the advantages of small size, thin thickness, light weight, extremely high power density / energy density, simple production, and easy integration. After integration with a small commercial sensor system, on the one hand, it can provide stable energy output, and on the other hand, due to the simple structure, the positive and negative electrodes are physically separated, and the robustness is stronger, and it can cope with stronger vibration, acceleration and other conditions, and can adapt to high-speed rotation and vibration environments.
[0053] Energy storage devices used for high-speed rotation need to have thin thickness and light weight in order to resist high centrifugal forces. Limited by its geometric characteristics, it is more difficult for energy storage devices to obtain high energy density and power density. Although traditional thin-film batteries can have high energy density, the electrodes are too dense and the ion transmission rate is slow under high load of active materials. The micro-battery prepared by the present invention has greatly expanded the contact area between the electrolyte and the electrode through the construction of a vertical porous structure, which is an important strategy to improve power density.
[0054] In addition, with the advancement of micro-processing, new energy and electronic technology, micro-batteries, as the core units of micro- and portable electronic devices, will have broader application prospects.
[0055] Based on the above solution, another embodiment of the present invention provides a micro battery, which is prepared using the above-mentioned method for preparing the micro battery.
[0056] Based on the above solution, another embodiment of the present invention provides the use of micro batteries in sensor systems for monitoring high-speed rotation and closed components.
[0057] On the basis of the above-mentioned embodiments, the present invention provides the following specific examples to further illustrate the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The experimental methods without specifying specific conditions in the following examples are usually based on the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by mass.
[0058] Example 1
[0059] This embodiment provides a method for preparing a micro battery, comprising the following steps:
[0060] 1. Manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode production:
[0061] 1) Add 0.1 M nickel sulfate and 0.5 M ammonium sulfate to 20 mL of water, sonicate for 15 minutes at room temperature, and stir for 15 minutes to obtain a light green solution;
[0062] 2) in the solution obtained in step 1), a three-electrode deposition method is used, with a micro-machined interdigitated micro-thin metal electrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode, and deposition is performed for 100 seconds under a constant voltage of -4.5 V to obtain a porous metal microelectrode;
[0063] 3) 0.245 g of manganese acetate tetrahydrate and 100 μL of EDOT were added to 20 mL of water and ultrasonically stirred for 1 minute to obtain a milky white dispersion.
[0064] 4) In the solution obtained in step 3), a porous nickel interdigital microelectrode was used as a working electrode, a platinum sheet was used as a counter electrode, and a silver / silver chloride electrode was used as a reference electrode to form a three-electrode system, and cyclic voltammetry was performed at a voltage range of 0-1.2 V and a speed of 50 mV s -1 Electrodeposition was performed for 70 cycles at the same scanning rate to obtain a manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode;
[0065] 2. Preparation of zinc negative microelectrode:
[0066] 5) Disperse 20 mg of carbon nanotubes (CNT) in 20 mL of ethanol solution, add 10 mg of magnesium nitrate particles, and sonicate for 1 hour to obtain a black uniform dispersion;
[0067] 6) In the dispersion obtained in 5), an interdigitated brass microelectrode is used as a negative electrode and a platinum electrode is used as a positive electrode. A constant voltage of 10 V is used for 600 seconds to electrophoresed the carbon nanotubes on the surface of the microelectrode, and after drying, a uniform black interdigitated microelectrode is obtained;
[0068] 7) The black interdigitated microelectrode obtained in step 6) is used as a working electrode, a platinum sheet is used as a counter electrode, and a silver / silver chloride electrode is used as a reference electrode to form a three-electrode system, and a metal zinc nanosheet is deposited on the surface of the working electrode in a mixed solution of 0.5 M zinc sulfate and 0.5 M sodium sulfate by a -1.1 V constant voltage deposition method for 600 s to obtain a zinc-coated carbon nanotube (Zn@CNT) microelectrode;
[0069] 3. Manganese sulfate / zinc sulfate / xanthan gum gel electrolyte preparation:
[0070] 8) Add 0.4 M manganese sulfate and 2 M zinc sulfate to 20 mL of water, stir thoroughly and ultrasonicate to obtain a clear solution;
[0071] 9) adding 0.7 g of xanthan gum to the solution obtained in step 8), and stirring to obtain a gel electrolyte;
[0072] 3. Assembly of manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode and zinc negative electrode microelectrode:
[0073] 9) Assembling the prepared manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode and Zn@CNT microelectrode as the negative electrode under an optical microscope;
[0074] 10) Coating the manganese sulfate / zinc sulfate / xanthan gum gel electrolyte on the surface of the electrode assembled in step 9), covering it with a PE square film, and then sealing the PE square film with a sealant to obtain a micro battery.
[0075] 11) The micro battery is attached to the surface of the rotating device and connected in series with the sensor system integrated on the surface to provide energy for it.
[0076] like Figure 1 The main process flow diagram of the microbattery is shown in the figure. The specific steps are: (a) preparing three-dimensional porous nickel interdigital electrodes by bubble template method; (b) using porous nickel interdigital electrodes as substrates, obtaining manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrodes by cyclic voltammetry electrodeposition solution; (c) demonstrating the strategy for achieving high mass loading and constructing effective ion transport channels; (d) combining manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrodes with interdigital zinc microelectrodes, coating with gel electrolyte and then encapsulating with PE to obtain a microbattery.
[0077] Taking the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode prepared in step 4) of Example 1 as an example, the morphology was analyzed by scanning electron microscopy and the surface analysis was performed by X-ray photoelectron spectroscopy. The results are shown in Figure 2 shown.
[0078] Figure 2(a)-(b) are magnified images of porous nickel interdigitated microelectrodes. It can be seen that a large number of porous structures are distributed on the surface of the microelectrode, providing a large specific surface area for the electrode. The scanning electron microscope image shows that the macroporous structure appears vertically inward on the surface of the electrode, which is different from the existing technology, the spatial network porous structure constructed by interweaving nanowires. Figure 2 (c) is the microstructure of manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode. The porous nickel framework provides sufficient space and surface for the growth of active materials. Compared with the porous nickel microelectrode, the pore size has not changed significantly, which will provide rich ion transport paths for electrolyte ions. Figure 2 (d) is the energy spectrum (EDS) mapping of the edge of the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode, which confirms the uniform distribution of Mn, S, and Ni elements, and the surface manganese dioxide and 3,4-ethylenedioxythiophene polymer are uniformly coated on the surface of the microelectrode. Figure 2 (e)-(f) are X-ray photoelectron spectroscopy (XPS) images of manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrodes, showing that the microelectrodes contain S, C, O, and Mn elements, and the self-selective energy separation of 11.7 eV corresponds to Mn 4+ 2p electrons.
[0079] The electrochemical performance of the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode prepared in step 4) of this Example 1 was characterized. Figure 3 shown.
[0080] Figure 3 (a) shows the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode product at a current density of 1 mA cm -2 From the discharge curve below, it can be seen that the microelectrode has an ultra-stable discharge platform at 1.2-1.4V, showing its high capacity. Figure 3 (b) is between 1 and 10 mA cm -2 The area capacitance curves of the microelectrodes with different thicknesses of manganese dioxide / 3,4-ethylenedioxythiophene polymer layer at different current densities show that the area capacitance retention rate is good as the thickness increases, indicating that it can provide high mass load and achieve efficient ion transport at 70 cycles. Figure 3 (c) MnO2 / 3,4-EDT polymer microelectrode at 1-10 mA cm -2 The charge and discharge curves under current density show high symmetry, a stable discharge curve and a high voltage platform. Figure 3 (d) 1 to 5 mV s -1 The cyclic voltammetry curve of the microelectrode below shows that at 1 mV s -1 The two Mn reduction peaks at 1.4 and 1.2 V in the curve reveal that Mn4+ and Mn 2+ The mutual conversion of the two materials corresponds to the charge and discharge curves, which fully demonstrates the excellent electrochemical performance of the microbattery.
[0081] The electrochemical performance of the microbattery prepared in Example 1 was characterized and its application demonstrated. Figure 4 shown.
[0082] Figure 4 (a) The microbattery assembled from a manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode and a zinc negative electrode microelectrode has a high conductivity at 1-5 mV s -1 The cyclic voltammetry curves at different scan rates under the same shape can be seen, which fully demonstrates the excellent rate performance and highly reversible redox reaction. Figure 4 (b) shows the range from 0.5 to 10 mA cm -2 The charge and discharge curves at different current densities all show a stable discharge platform at 1.2-1.4V. Figure 4 (c) is the Lagung diagram of the microbattery with high energy density while maintaining high power density, which still shows great advantages compared with many reported works. Figure 4 (d) shows the exponential increase in voltage and capacitance of microbatteries after series connection, demonstrating the high integration and scalability of microbatteries. Figure 4 (e)-(g) are application demonstrations of microbatteries assembled from manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrodes and zinc negative electrode microelectrodes. Figure 4 (e) shows the high flexibility of the microbattery after integration with the PET substrate. By connecting in series, it can stably achieve an ultra-high voltage output of over 10 V, laying the foundation for the realization of commercial microbatteries. Figure 4 (f) A micro-battery is installed on the surface of an axial flow fan blade that is subject to high-speed rotation, high vibration, and high wind pressure, and provides stable power to the LED to ensure safe operation in a high-speed environment for a long time, as a demonstration of in-situ monitoring of high-speed rotating components. Figure 4 (g) Powering an electronic timer with a single micro battery, achieving a long service life of over 400 minutes,
[0083] Compared with the existing top-down strategy micro-batteries, this example product meets the plug-in compatibility requirements and is closer to actual needs. This also fully reveals the huge potential of this example product after combining it with the existing chip integration process.
[0084] Example 2
[0085] This embodiment provides a method for preparing a micro battery, which is different from Embodiment 1 in that:
[0086] Step 1) depositing for 120 seconds at a constant voltage of -4.5 V to obtain a porous metal microelectrode;
[0087] The remaining steps and procedures are the same as those in Example 1.
[0088] Example 3
[0089] This embodiment provides a method for preparing a micro battery, which is different from Embodiment 1 in that:
[0090] Step 11), integrating the micro battery with the pressure sensor in the tire pressure monitoring device to construct an on-site tire pressure micro monitoring system.
[0091] In summary, the present invention provides a micro-battery for use in a sensor system for monitoring high-speed rotation and closed components. Compared with conventional button-type micro-batteries, the micro-battery produced by the present invention has the advantages of small size (area: 0.14cm2), thin thickness (0.2mm), light weight (100mg), extremely high power density / energy density, simple production, and easy integration.
[0092] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a micro battery, characterized in that: The steps include: S1. Fabrication of manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode S11, mixing nickel sulfate and ammonium sulfate to obtain a mixed solution A; in the mixed solution A, using a metal micro-interdigitated electrode as a working electrode, and adopting a three-electrode deposition method under a constant voltage to obtain a porous metal microelectrode; S12, mixing manganese acetate and 3,4-ethylenedioxythiophene to obtain a mixed solution B, and in the mixed solution B, using a porous metal microelectrode as a working electrode, and adopting an electrodeposition process under a constant voltage to obtain a manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode; S2. Fabrication of zinc-coated carbon nanotube microelectrodes S21, dispersing carbon nanotubes in an ethanol solution, adding magnesium nitrate, and mixing well to obtain a mixed solution C, in which a platinum sheet and a brass microelectrode are used as positive and negative electrodes, respectively, and an electrophoresis process is used under a constant voltage power supply to obtain an interdigitated microelectrode; S22, mixing zinc sulfate and sodium sulfate to obtain a mixed solution D, in which an interdigitated microelectrode is used as a working electrode, and a constant voltage deposition method is used to deposit metal zinc nanosheets on the surface of the working electrode to obtain a zinc-coated carbon nanotube microelectrode; S3. Assembly of micro batteries S31, using the manganese dioxide / 3,4-ethylenedioxythiophene polymer microelectrode and the zinc-coated carbon nanotube microelectrode as a positive electrode and a negative electrode, respectively, and assembling them under an optical microscope; S32. The assembled electrode surface is coated with manganese sulfate / zinc sulfate / xanthan gum gel electrolyte, and a micro battery is obtained after packaging.
2. The preparation method according to claim 1, characterized in that: In the mixed solution A, the mass ratio of the nickel sulfate to the ammonium sulfate is 1:(1-10), and in the mixed solution B, the mass ratio of the manganese acetate to the 3,4-ethylenedioxythiophene is 0.5-(10:1).
3. The preparation method according to claim 2, characterized in that: The three-electrode deposition method under constant voltage described in step S11 includes: using a metal micro-interdigitated electrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode, and depositing for 10 to 200 seconds under a constant voltage of -3 to -5 V.
4. The preparation method according to claim 3, characterized in that: In step S12, the electrodeposition process includes: using a metal micro-interdigitated electrode as a working electrode, a platinum sheet as a counter electrode, and a silver / silver chloride electrode as a reference electrode, at a voltage range of 0 to 0.9 V, using a voltage of 1 to 50 mV s -1 Scanning speed, 10 to 200 cycles of deposition.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In the mixed solution C, the mass ratio of the carbon nanotubes to the magnesium nitrate is 0.5 to (10:1), and in the mixed solution D, the mass ratio of the zinc sulfate to the sodium sulfate is 1 to (5:1).
6. The preparation method according to claim 5, characterized in that: The electrophoresis process in step S21 includes: a platinum sheet as the positive electrode and a brass, copper, nickel, stainless steel or titanium microelectrode as the negative electrode.
7. The preparation method according to claim 6, characterized in that: The constant voltage deposition method in step S22 includes: a constant voltage of 10 to 60 V and a deposition time of 1 to 30 min.
8. The preparation method according to claim 1, characterized in that: The preparation method of the manganese sulfate / zinc sulfate / xanthan gum gel electrolyte in step S32 includes: adding manganese sulfate and zinc sulfate into water, stirring evenly by ultrasonication, adding xanthan gum, and mixing evenly.
9. A micro battery, characterized in that: The micro battery is prepared by the preparation method of any one of claims 1 to 8.
10. Use of the microbattery according to claim 9 or the microbattery prepared by the preparation method according to any one of claims 1 to 8 in a sensor system for monitoring high-speed rotation and closed components.
Citation Information
Patent Citations
Aqueous zinc-manganese battery fiber with dual-function protective layer and of fiber
CN113036096A
Method for controlling concentration of electrophoresis solution of carbon nano tube
US20070240988A1