A method for activating a fuel cell stack

Through membrane electrode pre-activation and valley current activation methods, the problems of long activation time and large hydrogen consumption of fuel cell stacks are solved, rapid activation and the formation of efficient electrical transmission channels are achieved, and stack performance and shipments are improved.

CN115863699BActive Publication Date: 2024-10-11HAIDRIVER (BEIJING) ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211620550.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-10-11
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The existing fuel cell stack activation method takes a long time, consumes a large amount of hydrogen, prolongs the production cycle, and there is little research on pre-activation of membrane electrodes, which affects the performance of the stack.

Method used

Membrane electrode pre-activation and stack valley-type activation methods are used. The membrane electrode is treated with hydrogen peroxide and dilute sulfuric acid in the pre-activation solution. Combined with the purging of humidified nitrogen and hydrogen, the valley-type current activation method is used to shorten the activation time and improve the utilization of the catalyst. rate and stability of electrical transmission channels.

Benefits of technology

It significantly shortens the activation time, reduces hydrogen consumption, improves membrane electrode performance and catalyst utilization, achieves rapid activation of the stack, and the current density reaches more than 1.5A/cm2, improving the shipment volume and stability of the stack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115863699B_ABST
    Figure CN115863699B_ABST
Patent Text Reader

Abstract

The present invention provides a method for activating a fuel cell stack, and belongs to the technical field of fuel cells. The present invention utilizes membrane electrode pre-activation and stack trough activation methods to achieve rapid activation of the fuel cell stack. The purpose of pre-activation is to wet the membrane electrode as a whole, to avoid excessive drying of the membrane electrode when stacking, which causes membrane wrinkles during operation, and to achieve cleaning of the proton exchange membrane, removal of catalyst impurities and reduction of oxides, thereby achieving maximum utilization of the catalyst. The trough current activation method alternately uses currents of different sizes to activate the membrane electrode, so that the catalyst activity in different gaps of the membrane electrode is stimulated, so that the catalyst in different gaps is exposed to activity, thereby achieving maximum utilization of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cells, and in particular to an activation method for a fuel cell stack. Background Art

[0002] The core component of the fuel cell stack is the membrane electrode (MEA), and the performance of the membrane electrode determines the performance of the entire fuel cell stack. Although the performance of the membrane electrode depends on the performance of the component catalyst, diffusion layer, and proton exchange membrane, in order to achieve the best performance during the operation of the stack, the MEA needs to be activated. In addition, the MEA also needs to be activated before it is operated again after being stored for a period of time.

[0003] The activation mechanism is quite complex and is generally considered to include the following processes: (1) humidification of the proton exchange membrane; (2) establishment of material (electron, gas, water) transmission channels; (3) optimization of the electrode structure; (4) improvement of the activity and utilization of the catalytic layer. Currently, there is relatively little research on activation methods. Common activation methods include water vapor activation and CO adsorption oxidation activation. Traditional activation methods take a long time, usually one day or even several days, which not only consumes a large amount of hydrogen, but also prolongs the production cycle of the fuel cell stack. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a method for activating a fuel cell stack. The present invention utilizes membrane electrode pre-activation and stack valley activation method to achieve rapid activation of the fuel cell stack.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for activating a fuel cell stack, comprising the following steps:

[0007] Pre-activating the membrane electrode in a pre-activation solution to obtain an activated membrane electrode; the pre-activation solution comprises the following components by volume: 5% to 40% hydrogen peroxide, 10% to 50% dilute sulfuric acid and 20% to 60% water, the mass concentration of the hydrogen peroxide is 3% to 5%, and the mass concentration of the dilute sulfuric acid is 3% to 5%;

[0008] The activated membrane electrode is stacked and activated in situ, and the stacked in situ activation comprises the following steps:

[0009] Switch both the cathode and cathode to humidified nitrogen to purge the stack;

[0010] Switch the anode to humidified hydrogen and the cathode to humidified air. First, increase the current to 30A and hold for 30-50s. Then increase the current to 570A and hold for 30-50s. Then reduce the current to 60A and hold for 30-50s. Then increase the current to 540A and hold for 30s-50s. And so on. When the current reaches 300A, activate at a constant current for 20-30min. Finally, reduce the current to 30A and hold for 20-30s to complete the first trough activation.

[0011] Then the current is increased to 570A, stayed for 10s to 20s, then the current is reduced to 60A, stayed for 10 to 20s, then the current is increased to 540A, stayed for 10 to 20s, then the current is reduced to 90A, stayed for 10 to 20s, and so on. When the current reaches 300A, constant current activation is performed for 5 to 10min, and finally the current is reduced to 30A, stayed for 10 to 20s, to complete the second stage of valley activation. The first valley activation cycle includes the first stage of valley activation and the second stage of valley activation.

[0012] Cycle 3 to 5 times of trough activation.

[0013] Preferably, the pre-activation solution comprises the following components in volume fractions: 30% to 35% hydrogen peroxide, 20% to 25% dilute sulfuric acid and 40% to 50% water, the mass fraction of the hydrogen peroxide is 3%, and the mass fraction of the dilute sulfuric acid is 5%.

[0014] Preferably, the purging time is 30 to 40 minutes.

[0015] Preferably, the purging process includes: heating from 30° C. to 78° C., and the heating rate is 2° C. / min.

[0016] Preferably, the stoichiometric ratio of the anode is 1.6 to 2.5, and the stoichiometric ratio of the cathode is 2.8 to 3.5.

[0017] Preferably, the humidity of the anode is 40% to 60%, and the humidity of the cathode is 60% to 80%.

[0018] Preferably, the back pressure of the anode is 13-110 kPa, and the back pressure of the cathode is 33-130 kPa.

[0019] Preferably, during the in-situ activation of the stack, the current ramping rate is independently 5 to 20 A / s.

[0020] Preferably, the pre-activation time is 0.5 to 1 h.

[0021] Preferably, the number of membrane electrodes in the stacked in-situ activation is 90 to 120, and the power is independently 30 to 50 kW.

[0022] The present invention utilizes membrane electrode pre-activation and stack valley activation method to realize rapid activation of fuel cell stack. The purpose of pre-activation is to wet the membrane electrode as a whole to avoid excessive drying of the membrane electrode when stacking, which causes membrane wrinkles during operation. It also realizes the cleaning of the proton exchange membrane, the removal of catalyst impurities and the reduction of oxides, thereby realizing the maximum utilization of the catalyst. The valley current activation method activates the membrane electrode by alternating currents of different sizes, so that the catalyst activity in different gaps of the membrane electrode is stimulated, the catalyst activity in different gaps is exposed, and the maximum utilization of the catalyst is realized.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] (1) The activation time is greatly shortened. Compared with the activation time of one day or even several days, the present invention reduces the activation time, reduces the consumption of hydrogen, and increases the shipment volume of the fuel cell stack;

[0025] (2) Pre-activated membrane electrode can improve the overall performance of membrane electrode and increase the utilization rate of catalyst. The valley current activation method uses different currents to form a stable electrical transmission channel and mass transmission channel for the battery stack. After several valley activations, the activation effect can make the current density at 0.65V reach 1.5A / cm 2 above. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of voltage change during in-situ activation of the stack in the present invention;

[0027] Figure 2 1 is the polarization curve before and after activation of Example 1;

[0028] Figure 3 2 is the polarization curve before and after activation of Example 2;

[0029] Figure 4 The polarization curves of comparative example 1 before and after activation;

[0030] Figure 5 The graphs are the uniformity curves of the battery stack after activation of Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0031] The present invention provides a method for activating a fuel cell stack, comprising the following steps:

[0032] Pre-activating the membrane electrode in a pre-activation solution to obtain an activated membrane electrode; the pre-activation solution comprises the following components by volume: 5% to 40% hydrogen peroxide, 10% to 50% dilute sulfuric acid and 20% to 60% water, the mass concentration of the hydrogen peroxide is 3% to 5%, and the mass concentration of the dilute sulfuric acid is 3% to 5%;

[0033] The activated membrane electrode is stacked and activated in situ, and the stacked in situ activation comprises the following steps:

[0034] Switch both the cathode and cathode to humidified nitrogen to purge the stack;

[0035] Switch the anode to humidified hydrogen and the cathode to humidified air. First, increase the current to 30A and hold for 30-50s. Then increase the current to 570A and hold for 30-50s. Then reduce the current to 60A and hold for 30-50s. Then increase the current to 540A and hold for 30s-50s. And so on. When the current reaches 300A, activate at a constant current for 20-30min. Finally, reduce the current to 30A and hold for 20-30s to complete the first trough activation.

[0036] Then the current is increased to 570A, stayed for 10s to 20s, then the current is reduced to 60A, stayed for 10 to 20s, then the current is increased to 540A, stayed for 10 to 20s, then the current is reduced to 90A, stayed for 10 to 20s, and so on. When the current reaches 300A, constant current activation is performed for 5 to 10min, and finally the current is reduced to 30A, stayed for 10 to 20s, to complete the second stage of valley activation. The first valley activation cycle includes the first stage of valley activation and the second stage of valley activation.

[0037] Cycle 3 to 5 times of trough activation.

[0038] The present invention pre-activates a membrane electrode in a pre-activation solution to obtain an activated membrane electrode; the pre-activation solution comprises the following components in volume fractions: 5% to 40% hydrogen peroxide, 10% to 50% dilute sulfuric acid and 20% to 60% water, the mass concentration of the hydrogen peroxide is 3% to 5%, and the mass concentration of the dilute sulfuric acid is 3% to 5%.

[0039] In the present invention, the pre-activation solution preferably comprises the following components in volume fractions: 30% to 35% hydrogen peroxide, 20% to 25% dilute sulfuric acid and 40% to 50% water, the mass concentration of the hydrogen peroxide is preferably 3%, and the mass concentration of the dilute sulfuric acid is preferably 5%.

[0040] The present invention has no particular limitation on the preparation method of the pre-activation solution, and the method may be well known to those skilled in the art, such as stirring.

[0041] In the present invention, the water is preferably deionized water.

[0042] In the present invention, the pre-activation time is preferably 0.5 to 1 h.

[0043] In the present invention, the frame of the membrane electrode is preferably clamped with a flat clamp, vertically inserted into the pre-activation solution, and the membrane electrode is laid flat to be fully soaked for the pre-activation.

[0044] In the present invention, the flat clamp is preferably made of rubber.

[0045] After the preactivation is completed, the present invention preferably uses dust-free paper or dust-free cloth to absorb excess preactivation liquid.

[0046] After obtaining the activated membrane electrode, the present invention performs in-situ activation on the activated membrane electrode by stacking, and the in-situ activation comprises the following steps:

[0047] Switch both the cathode and cathode to humidified nitrogen to purge the stack;

[0048] Switch the anode to humidified hydrogen and the cathode to humidified air. First, increase the current to 30A and hold for 30-50s. Then increase the current to 570A and hold for 30-50s. Then reduce the current to 60A and hold for 30-50s. Then increase the current to 540A and hold for 30s-50s. And so on. When the current reaches 300A, activate at a constant current for 20-30min. Finally, reduce the current to 30A and hold for 20-30s to complete the first trough activation.

[0049] Then the current is increased to 570A, stayed for 10s to 20s, then the current is reduced to 60A, stayed for 10 to 20s, then the current is increased to 540A, stayed for 10 to 20s, then the current is reduced to 90A, stayed for 10 to 20s, and so on. When the current reaches 300A, constant current activation is performed for 5 to 10min, and finally the current is reduced to 30A, stayed for 10 to 20s, to complete the second stage of valley activation. The first valley activation cycle includes the first stage of valley activation and the second stage of valley activation.

[0050] Cycle 3 to 5 times of trough activation.

[0051] In the present invention, the purging time is preferably 30 to 40 minutes.

[0052] In the present invention, the purging process preferably includes: heating from 30°C to 78°C, and the heating rate is 2°C / min. The purpose of the purging is to moisten the activated membrane electrode, establish a transmission channel, and make the stack structure more stable.

[0053] In the present invention, the stoichiometric ratio of the anode is preferably 1.6 to 2.5, and the stoichiometric ratio of the cathode is preferably 2.8 to 3.5.

[0054] In the present invention, the humidity of the anode is preferably 40% to 60%, and the humidity of the cathode is preferably 60% to 80%.

[0055] In the present invention, the back pressure of the anode is preferably 13 to 110 kPa, and the back pressure of the cathode is preferably 33 to 130 kPa.

[0056] In the present invention, the current ramping rate during the in-situ activation of the stack is independently preferably 5 to 20 A / s.

[0057] In the present invention, the number of membrane electrodes in the stacked in-situ activation is preferably 90 to 120, and the power is preferably independently 30 to 50 kW.

[0058] In the present invention, the minimum voltage setting in the stack in-situ activation is preferably ≥0.3V, and the system will automatically stop if it is lower than 0.3V.

[0059] Figure 1 It is a schematic diagram of voltage change during in-situ activation of the stack in the present invention.

[0060] In the present invention, the process of the first stage trough activation is shown in Table 1.

[0061] Table 1 The process of the first trough activation

[0062]

[0063]

[0064] In the present invention, the process of the second trough activation is shown in Table 2.

[0065] Table 2 The process of the second trough activation

[0066]

[0067] In order to further illustrate the present invention, the activation method of the fuel cell stack provided by the present invention is described in detail below in combination with examples, but they should not be understood as limiting the scope of protection of the present invention.

[0068] Example 1

[0069] Prepare 35 parts of 3% mass concentration H2O2, 25 parts of 5% mass concentration H2SO4, and 40 parts of deionized water by volume, stir for 0.5 hours, and mix evenly. Clamp the membrane electrode with a flat clamp, put it vertically into the prepared solution, slowly lay it flat, let it stand for 0.5 hours, and absorb the excess water with a dust-free cloth. Prepare 90 membrane electrodes according to this operation, stack the pretreated membrane electrodes, and prepare for activation test.

[0070] Start the temperature control program and cooling water program for the assembled stack, control the cathode back pressure at 33kPa, and the anode back pressure at 13kPa. The anode stoichiometric ratio is 2.5, the cathode stoichiometric ratio is 3.5, the anode humidity is always controlled at 40%RH, and the cathode humidity is always controlled at 60%RH. Manual temperature control, the stack temperature starts at 30℃, 2℃ / min adjustment, gradually heats up to 78℃, and purges steadily for 10 minutes to complete the nitrogen purge.

[0071] The anode was switched to humidified hydrogen, the cathode was switched to humidified air, the cathode stoichiometric ratio was gradually increased from 2.5 to 3.5, the anode stoichiometric ratio was gradually increased from 1.6 to 2.5, the anode back pressure was gradually increased from 13 to 100 kPa, the cathode back pressure was gradually increased from 33 to 120 kPa, the operating temperature was 75 ° C for the anode, 75 ° C for the cathode, and the stack temperature was 78 ° C. Start the load, increase the current to 30 A first, run for 30 seconds, then increase the current to 570 A, run for 30 seconds, then reduce the current to 60 A, run for 30 seconds, then increase the current to 540 A, run for 30 seconds... (current load rate 15 A / s) and so on, until the current reaches 300 A, run at a constant current of 300 A for 20 minutes, then reduce the current to 30 A, run for 20 seconds, and complete the first section of valley activation. The parameters of the first section of valley activation are shown in Table 1.

[0072] After the first stage of valley activation, the current is raised from 30A to 570A after staying for 10s, running for 10s, then reduced to 60A, running for 10s, then raised to 540A, running for 10s, reduced to 90A, running for 10, and so on. When the current reaches 300A, constant current is loaded for 10min, and then the current is reduced to 30A, running for 20s to complete the second stage of valley activation. The parameters of the second stage of valley activation are shown in Table 2. In summary, the first valley activation is completed, and three cycles are performed to complete the stack activation (polarization test is required before and after stack activation).

[0073] The conditions of polarization test are as follows: 30-570A as scanning current density, 30s at each current, current ramp rate of 15A / s, anode stoichiometry of 2.2, cathode stoichiometry of 3.5. Anode humidity 40%RH, cathode humidity 60%RH, hydrogen back pressure 120kPa, air back pressure 100kPa, anode 75℃, cathode 75℃, stack temperature 78℃.

[0074] Example 2

[0075] Prepare 30 parts of 3% mass concentration H2O2, 20 parts of 5% mass concentration H2SO4, and 50 parts of deionized water by volume, stir for 0.5 hours, and mix evenly. Clamp the membrane electrode with a flat clamp, put it vertically into the prepared solution, slowly lay it flat, let it stand for 0.5 hours, and absorb the excess water with dust-free paper. Prepare 90 membrane electrodes according to this operation, stack the pretreated membrane electrodes, and prepare for activation test.

[0076] Start the temperature control program and cooling water program for the assembled battery stack, control the cathode back pressure at 40kPa, and the anode back pressure at 20kPa. The anode stoichiometric ratio is 2.2, the cathode stoichiometric ratio is 3, the anode humidity is always controlled at 50%RH, and the cathode humidity is always controlled at 50%RH. Manual temperature control, the battery stack temperature starts at 30℃, adjusts at 2℃ / min, and gradually heats up to 78℃. After steady purge for 10 minutes, complete the nitrogen purge.

[0077] The anode was switched to humidified hydrogen, the cathode was switched to humidified air, the cathode stoichiometric ratio was gradually increased from 2.2 to 3, the anode stoichiometric ratio was gradually increased from 1.2 to 2, the anode back pressure was gradually increased from 20kPa to 110kPa, the cathode back pressure was gradually increased from 40kPa to 130kPa, the operating temperature was 75℃ for the anode, 75℃ for the cathode, and the stack temperature was 78℃. Start the load, increase the current to 30A first, run for 40s, then increase the current to 570A, run for 40s, then reduce the current to 60A, run for 40s, then increase the current to 540A, run for 40s (current load rate 20A / s), and so on, until the current reaches 300A, run at a constant current of 300A for 30min, then reduce the current to 30A, run for 20s, and complete the first stage of valley activation. The parameters of the first stage of valley activation are shown in Table 1.

[0078] After the first stage of valley activation, the current is raised from 30A to 570A after staying for 10s, running for 15s, then reduced to 60A, running for 15s, then raised to 540A, running for 15s, reduced to 90A, running for 15s, and so on. When the current reaches 300A, constant current is loaded for 10min, and then the current is reduced to 30A, running for 20s to complete the second stage of valley activation. The parameters of the second stage of valley activation are shown in Table 2. In summary, the first valley activation is completed, and three cycles are performed to complete the stack activation (polarization test is required before and after stack activation).

[0079] Comparative Example 1

[0080] Prepare 35 parts of 3% mass concentration H2O2, 25 parts of 5% mass concentration H2SO4, and 40 parts of deionized water by volume, stir for 0.5 hours, and mix evenly. Clamp the membrane electrode with a flat clamp, put it vertically into the prepared solution, slowly lay it flat, let it stand for 0.5 hours, and absorb the excess water with a dust-free cloth. Prepare 90 membrane electrodes according to this operation, stack the pretreated membrane electrodes, and prepare for activation test.

[0081] Start the temperature control program and cooling water program for the assembled battery stack, control the cathode back pressure at 33kPa, and the anode back pressure at 13kPa. The anode stoichiometric ratio is 2.5, the cathode stoichiometric ratio is 3.5, the anode humidity is always controlled at 40%RH, and the cathode humidity is always controlled at 60%RH. Manual temperature control, the battery stack temperature starts at 30℃, adjusts at 2℃ / min, and gradually heats up to 78℃. After steady purge for 10 minutes, complete the nitrogen purge.

[0082] The anode was switched to humidified hydrogen, and the cathode was switched to humidified air. The cathode stoichiometric ratio gradually increased from 2.5 to 3.5, the anode stoichiometric ratio gradually increased from 1.6 to 2.5, the anode back pressure gradually increased from 13 to 100 kPa, and the cathode back pressure gradually increased from 33 to 120 kPa. The operating temperatures were 75°C for the anode, 75°C for the cathode, and 78°C for the stack.

[0083] Start the load, run at 30A for 5 minutes, slowly increase the current to 300A, run at 300A constant current for 3 hours, then reduce the current to 30A and run for 10 minutes to complete constant current stack activation. The stack constant current activation procedure is shown in Table 3.

[0084] Table 3 Comparative Example 1 Stack Constant Current Activation Procedure

[0085]

[0086] Figure 2 is the polarization curve before and after activation of Example 1, Figure 2 It can be seen that the current density of Example 1 at 0.65V before activation is 1.52A / cm 2 , after activation, it can reach 1.68A / cm 2 .

[0087] Figure 3 The polarization curves before and after activation of Example 2 are shown in FIG. Figure 3 It can be seen that the current density of Example 2 at 0.65V before activation is 1.57A / cm 2 After activation, the current density can reach 1.72A / cm 2 All of the above indicate that the valley current activation method improves the oxygen transmission channel, maximizes the utilization of Pt, and improves the overall performance of the membrane electrode.

[0088] Figure 4 The polarization curves before and after activation of Comparative Example 1 are shown in FIG. Figure 4 It can be seen that the current density of Comparative Example 1 at 0.65V before activation is 1.48A / cm 2 After activation, the current density at 0.65V is 1.51A / cm 2 , indicating that constant current activation did not improve the performance of the membrane electrode in the short term.

[0089] Figure 5 The uniformity curves of the activated stacks of Example 1 and Comparative Example 1 show that after the valley activation procedure, the voltage of each piece is more consistent, while after the constant current activation, the voltage still fluctuates. This shows that the activation method of the present invention can be applied not only to new membrane electrodes, but also to long-standing stacks.

[0090] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for activating a fuel cell stack, characterized in that: The following steps are involved: Pre-activating the membrane electrode in a pre-activation solution to obtain an activated membrane electrode; the pre-activation solution comprises the following components by volume: 30% to 35% hydrogen peroxide, 20% to 25% dilute sulfuric acid and 40% to 50% water, the mass fraction of the hydrogen peroxide is 3%, and the mass fraction of the dilute sulfuric acid is 5%; The activated membrane electrode is stacked and activated in situ, and the stacked in situ activation comprises the following steps: Switch both the cathode and cathode to humidified nitrogen to purge the stack; Switch the anode to humidified hydrogen and the cathode to humidified air. First, increase the current to 30A and hold for 30-50s. Then increase the current to 570A and hold for 30-50s. Then reduce the current to 60A and hold for 30-50s. Then increase the current to 540A and hold for 30s-50s. And so on. When the current reaches 300A, activate at a constant current for 20-30min. Finally, reduce the current to 30A and hold for 20-30s to complete the first trough activation. Then the current is increased to 570A, stayed for 10s to 20s, then the current is reduced to 60A, stayed for 10 to 20s, then the current is increased to 540A, stayed for 10 to 20s, then the current is reduced to 90A, stayed for 10 to 20s, and so on. When the current reaches 300A, constant current activation is performed for 5 to 10 minutes, and finally the current is reduced to 30A, stayed for 10 to 20s, completing the second valley activation. The first valley activation cycle includes the first valley activation and the second valley activation. Cycle 3 to 5 times of trough activation.

2. The activation method according to claim 1, characterized in that The purging time is 30 to 40 minutes.

3. The activation method according to claim 1 or 2, characterized in that The purging process includes: heating from 30° C. to 78° C., and the heating rate is 2° C. / min.

4. The activation method according to claim 1, characterized in that The stoichiometric ratio of the anode is 1.6 to 2.5, and the stoichiometric ratio of the cathode is 2.8 to 3.

5.

5. The activation method according to claim 1 or 4, characterized in that: The humidity of the anode is 40% to 60%, and the humidity of the cathode is 60% to 80%.

6. The activation method according to claim 1, characterized in that: The back pressure of the anode is 13-110 kPa, and the back pressure of the cathode is 33-130 kPa.

7. The activation method according to claim 1, characterized in that: During the in-situ activation of the stack, the current ramp rates are independently 5 to 20 A / s.

8. The activation method according to claim 1, characterized in that: The pre-activation time is 0.5 to 1 h.

9. The activation method according to claim 1, characterized in that: The number of membrane electrodes in the stacked in-situ activation is 90 to 120, and the power is independently 30 to 50 kW.