A high-voltage rectifier manufacturing process

By welding silicon wafers into a single unit and combining this with a high-voltage rectifier manufacturing process involving glass sintering, the adaptability of high-voltage silicon stacks to high-temperature and high-pressure environments has been solved, achieving higher reliability and temperature resistance.

CN115881550BActive Publication Date: 2026-11-17JINAN XINYUAN SEMICONDUCTOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211581554.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2026-11-17
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

Existing high-voltage silicon stack rectifier manufacturing processes cannot adapt to high-temperature and high-pressure environments, and product reliability is insufficient.

Method used

The process involves first welding silicon wafers together, then filling them with welding electrodes, solder pads, and molybdenum particles. This is combined with glass sintering and high-temperature welding. The linear thermal expansion coefficients of the molybdenum particles and the grains are similar to buffer thermal stress, and a high-thickness glass passivation layer is used to protect the PN junction.

Benefits of technology

The high-voltage rectifiers produced can adapt to high-temperature and high-pressure environments, have higher reliability and resistance to high and low temperature cycles, and improve product structural stability and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115881550B_ABST
    Figure CN115881550B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of semiconductor manufacturing technology, specifically relating to a high-voltage rectifier manufacturing process; it includes the following steps: Step 1: Prepare materials and load ten large silicon wafers into a welding mold; Step 2: Enter the furnace and weld at high temperature under nitrogen protection; Step 3: Wire cut, followed by cleaning of the die; Step 4: Load raw materials; Step 5: Press with a weight, enter the welding furnace, and weld at high temperature under nitrogen protection; Step 6: Out of the furnace and changeover; Step 7: Acid washing and ultrasonic cleaning with water; Step 8: After applying glass slurry, enter the sintering furnace under nitrogen protection for glass sintering; Step 9: Reliability testing; Step 10: Prepare for adhesive application; Step 11: Apply adhesive and cure after application; Step 12: Surface tin treatment; Step 13: Second reliability test; Step 14: Electrical testing; Step 15: Printing and visual inspection; Step 16: Packaging and warehousing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor processing, and specifically relates to a high-voltage rectifier manufacturing process. Background Technology

[0002] A rectifier is a device that converts alternating current (AC) into direct current (DC). It has two main functions: first, to convert AC into DC, which is then filtered and supplied to the load or to the inverter; second, to provide charging voltage to the battery.

[0003] The document with publication number CN114551250 B discloses a mass production process for high-voltage silicon stacks, including the following steps: Step 1. Apply solder: Place multiple DBC boards in a fixture and use a screen printing machine to print a layer of solder with a thickness of 0.1mm-0.2mm on each DBC board; Step 2. Assemble the chips: Use an automatic assembly machine equipped with a chip pick-up head to pick up multiple chips at once and lay them flat on the predetermined positions on each DBC board. Then, use solder to fix the chips to each DBC board. Step 3. Apply solder: Use a dispensing machine to apply solder to multiple chips and their pin bonding points; Step 4. Assemble jumpers: Use an automatic assembly machine equipped with a jumper pick-up head to pick up multiple jumpers at once and place them in the predetermined positions on each DBC board. Then, solder the jumpers with solder to obtain a whole chip with multiple chips connected in series on the DBC board. Step 5. Pin Assembly: Pre-fabricate a pin frame containing multiple pins, and then use solder to fix each pin in the pin frame to both ends of each overall chip. Step 6. Sintering: Sintering is carried out in a vacuum furnace at a temperature of 360℃±20℃. After sintering, the product is removed and placed in a transfer fixture. Step 7. Cleaning: Remove any residue from the welding surface using rosin cleaning solution; Step 8. Encapsulation: Using an injection molding machine and mold, epoxy resin is used to encapsulate each integral chip under high temperature (175±20℃) and high injection pressure (50N±20N) to form high-voltage silicon stacks with different encapsulation forms. Step 9. Pin plating: Apply tin plating with a thickness of not less than 3µm to the pins of the high-voltage silicon stack using a rack plating process; Step 10. Lead cutting: Use a lead cutting machine to cut the lead frame and cut the finished high-voltage silicon stack with the leads connected together into individual units; Step 11. Test printing: Use a combination machine and a digital machine to test the parameters of the high-voltage silicon stack, and print markings on the qualified products; Step 12. Packaging: Pack the completed high-voltage silicon stacks in packaging bags and cartons; The high-voltage silicon stack products produced by the above methods are mass-produced as individual units and cannot adapt to high-temperature and high-pressure environments. Summary of the Invention

[0004] The present invention addresses the problems mentioned above by designing a high-voltage rectifier manufacturing process.

[0005] To achieve the above objectives, the present invention provides a high-voltage rectifier manufacturing process, comprising the following steps: Step 1: Prepare the materials and load the large silicon wafer into the welding mold; Step two involves entering the furnace and welding at high temperature under nitrogen protection; Step 3: Wire cutting; the large silicon wafers welded together are wire cut into a circle, and the grains are cleaned; Step 4: Raw material loading; Step 5: Press down the heavy hammer, put it into the welding furnace, and weld at high temperature under nitrogen protection; Step six: Out of the oven and transfer; Step 7: Pickling and ultrasonic cleaning with water; use a pickling machine to acidically etch the PN junction surface of the grains in the welded product to remove possible contaminants. During the pickling process, perform ultrasonic cleaning with high-purity water according to the procedure. Step 8: Coat the cleaned workpiece with glass slurry and place it in a sintering furnace under nitrogen protection for glass sintering. Step Nine: Reliability Testing; Before and after the reliability testing, the laboratory shall conduct semi-automatic electrical testing. Step 10: Prepare for glue injection; Step 11: Applying adhesive and curing after application; Step 12: Surface tin treatment; Step Thirteen: Second Reliability Test; Before and after the reliability test, the laboratory shall conduct semi-automatic electrical tests. Step Fourteen: Electrical Testing; Fully automated electrical testing is performed on the production line. Step 15: Printing and visual inspection; Step sixteen: Pack and store.

[0006] Furthermore, the raw material loading sequence in step four is as follows: loading two copper electrodes in the first stage, loading four welding pieces in the first stage, loading four molybdenum particles in the first stage, loading four cleaned crystals, loading four molybdenum particles in the second stage, loading four welding pieces in the second stage, and loading two copper electrodes in the second stage, all uniformly and orderly loaded into the cut welding mold.

[0007] Furthermore, in step five, the maximum temperature inside the welding furnace is 715℃~760℃, the time spent in the constant temperature zone above 660℃ is 11~17min, the time spent in the constant temperature zone above 580℃ is 17~21min, and the furnace outlet temperature is ≤130℃; the pressure of the nitrogen gas is 2.5±0.5kg / cm². 2 .

[0008] Furthermore, the pickling machine mentioned in step seven includes an acid tank #1 and an acid tank #2. The acid tank #1 is filled with mixed acid #1, and the acid tank #2 is filled with mixed acid #2. The ratio of mixed acid #1 is nitric acid: sulfuric acid: hydrofluoric acid: phosphoric acid = 1:2:1:2; the ratio of mixed acid #2 is phosphoric acid: hydrogen peroxide: deionized water = 1:2:3.

[0009] Preferably, the actual acid temperature of the No. 1 mixed acid is 25℃~28℃, and the actual acid temperature of the No. 2 mixed acid is 62℃±3℃.

[0010] Preferably, the maximum temperature of the sintering furnace in step eight is 670℃±10℃, and the time for passing through the area above 630℃ is 6min~12min, with a chain speed of 12.5cm / 60±2s.

[0011] Furthermore, step ten, the preparation of the adhesive for injection, includes the following steps: S1 Electrical pre-classification; S2 Hi-rel; The product undergoes high-temperature and high-pressure working environment testing. The working environment is in insulating oil at an ambient temperature of 175℃, and the applied voltage is not less than 10... 4 V.

[0012] Preferably, the glass slurry in step eight is prepared as follows: glass powder / high-purity deionized water = (450 ± 1 g) / (175 ± 5 ml).

[0013] Furthermore, the surface tin treatment described in step twelve includes the following steps: P1 Copper electrode pretreatment; P2 checks the tinning parameters; P3 Loading; P4 Soldering tray installation; P5 Tin Dipping; P6 Cooling; P7 is the other end that is immersed in tin; P8 Material feeding; P9 cleaning machine preparation; Clean with P10 cleaning agent; P11 Drying; P12 Sorting of products with defective appearance; P13 Packing.

[0014] In summary, the high-voltage rectifier manufacturing process of the present invention has the following advantages and beneficial technical effects: 1. The high-voltage rectifier manufacturing process of the present invention adopts the method of first welding silicon wafers into a connected whole, and then filling in welding electrodes, welding sheets and molybdenum particles. The process is simple and applicable to various production modes.

[0015] 2. The high-voltage rectifier manufacturing process of the present invention adopts a glass sintering product structure. The structure has a grain in the middle, and molybdenum grains, solder sheets, and oxygen-free copper electrodes on both sides. The grain and molybdenum grain are protected by glass. Molybdenum grains are selected as the diode die substrate. The molybdenum grain and the grain will generate a certain linear thermal expansion when heated. Because the linear thermal expansion coefficients of molybdenum grain and the grain are similar, the thermal expansion coefficients of molybdenum grain and the grain are close. When the temperature changes abruptly, the internal stress caused by thermal expansion and contraction can be buffered, and the grain will not fail.

[0016] 3. The high-voltage rectifier produced by this invention can not only be used in high-temperature and low-temperature environments, but also adapt to environments with cyclical changes in high and low temperatures.

[0017] 4. The high-voltage rectifier manufacturing process of the present invention uses a high-thickness glass passivation layer to protect the PN junction, resulting in higher product reliability. Conventional diodes use white glue (which has a poorer protective effect than glass) to protect the PN junction, or GPP products use a thinner (about 0.06mm thick) glass passivation layer to protect the PN junction. However, the glass thickness of this product is 0.5mm, which is much greater than that of GPP products, thus giving it high reliability. Attached Figure Description

[0018] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a flowchart of a high-voltage rectifier manufacturing process according to the present invention; Figure 2 This is a schematic diagram of the structure of the large silicon wafer being loaded into the welding mold of the present invention; Figure 3 This is a schematic diagram of the raw materials after loading in step four of this invention.

[0019] Explanation of reference numerals in the attached figures: 1. Mold cover, 2. Mold body, 3. Ten large silicon wafers, 4. Copper electrode, 5. Solder sheet, 6. Molybdenum particle, 7. Grain. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of the embodiments of this invention will be described in more detail below with reference to the accompanying drawings. In the drawings, the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout; the described embodiments are some embodiments of this invention, but not all embodiments; the embodiments and directional terms described below with reference to the accompanying drawings are exemplary and intended to explain this invention, and should not be construed as limiting this invention; all other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention. The embodiments of this invention will be described in detail below with reference to the accompanying drawings:

Example 1

[0021] Specifically: Step 1: Prepare the materials and load the large silicon wafer into the welding mold; for example... Figure 2 As shown, ten large silicon wafers are loaded at a time; Step 2: Place the wafers into the furnace and weld them together at high temperature under nitrogen protection; Step 3: Wire cutting; Take out the ten soldered silicon wafers and use wire cutting to cut them into circles together; Step Four: As Figure 3 As shown, after cleaning the grains, the raw materials are loaded. The raw materials are loaded into the rectifier graphite mold in the following order: first, two copper electrodes; first, four solder pads; first, four molybdenum particles; four cleaned grains; second, four molybdenum particles; second, four solder pads; and second, two copper electrodes. The thin graphite plate on the mold separates the four groups of grains, solder pads, molybdenum particles, and copper electrodes.

[0022] Step 5: Place the heavy hammer on top and enter the welding furnace. Under nitrogen protection, perform high-temperature welding to weld the loaded raw materials and cut silicon wafers together. The maximum temperature inside the welding furnace is 715℃~760℃. The holding time in the temperature zone above 660℃ is 11~17 minutes, and the holding time in the temperature zone above 580℃ is 17~21 minutes. The outlet temperature is ≤130℃. The nitrogen pressure is 2.5±0.5kg / cm². 2; Step 6: Remove from the welding furnace and transfer to the pickling basket for the next pickling step. Step 7: Acid pickling and ultrasonic cleaning with water; Specifically: 7.1 Turn on the main power of the pickling machine, check whether the temperature of No. 1 acid / No. 2 acid / water tank meets the specifications (select cooling or heating according to the actual situation), turn on the running and booster pumps, and turn on the ultrasonic machine switch.

[0023] 7.2 Place the pickling basket containing the welded finished products into the inlet of the pickling machine. The pickling machine will automatically pickle the products according to the prescribed procedure. Five empty pickling baskets must be placed in front of the pickling basket to prevent water from entering the water tank when rinsing from above, which would cause uneven water temperature.

[0024] 7.3 Pickling Machine Setting Program 7.3.1 Connect the programmer to the pickling machine program control unit.

[0025] 7.3.2 Press the "DEV" key to select the menu "HPP" → "ENT" → "SET" key 7.3.3 Press the “SET” key to set the time, press the “EST” key, and press the “ESC” key to exit programming after all settings are completed.

[0026] 7.3.4 The program is as follows: Address instruction operand (SET) C 0 300 (Acid etching time #1: 85″±5″) C 1 250 (Acid etching time #1: 95″±5″) C 2 220 (Acid etching time 105″±5″) T 3 30 (Acid injection time #1) T 4 18 (Acid injection time #2) Note: The etching time for #2 acid is based on the pickling machine's cycle. 7.4 Instrument Settings 7.4.1 Set temperature for #1 acid heater: 30~35℃. The set temperature must ensure that the actual acid temperature of #1 acid is within the range of 25~28℃. 7.4.2 Water heater set temperature: 25~30℃. The set temperature must ensure that the actual measured water temperature in the water tank matches: 25~28℃. 7.4.3 Set temperature for #2 acid heater: 63±2℃. The set temperature must ensure that the actual acid temperature of #2 acid matches: 62±3℃. 7.5 Pickling Requirements The ratio of the mixed acids #1 is nitric acid: sulfuric acid: hydrofluoric acid: phosphoric acid = 1:2:1:2.

[0027] The ratio of the mixed acid #2 is phosphoric acid: hydrogen peroxide: deionized water = 1:2:3.

[0028] Pickling is performed according to the following process: 1# mixed acid 85″±5″ → rinse with water 57″±5″ → 2# mixed acid 57″±5″ → rinse with water → ultrasonic cleaning with high-purity water → high-pressure rinsing → ready to apply glass slurry.

[0029] Step 8: Under nitrogen protection, the glass enters the sintering furnace for glass sintering. Specifically: 8.1 First, remove a certain number of welded parts from the pickling basket after pickling and etching; 8.2 Place the welded parts on a specific fixture; 8.3 Align the needle of the glass slurry bottle with the grains (molybdenum grains) of the weldment, squeeze out a glass slurry of appropriate size, so that the glass slurry balls coated on each grain of the weldment are of uniform size, and then rotate it evenly; the glass slurry ratio is: glass powder / high-purity deionized water = (450±1 g) / (175±5 ml).

[0030] 8.4 After the glass slurry is evenly distributed on all the welded parts, cover it with a cover plate and heat it before placing it on the graphite strip.

[0031] 8.5 Then the welded parts with the glass slurry applied are put into the sintering furnace for sintering. During the process of entering the furnace, they are handled and placed steadily. The maximum temperature of the sintering furnace is 670℃±10℃. In the area above 630℃, the passage time is 6min~12min and the chain speed is 12.5cm / 60±2s.

[0032] Step Nine: Reliability Testing; Through reliability testing, products are screened. Before and after the reliability test, the laboratory conducts semi-automatic electrical tests, and qualified products are prepared for the next step of glue application.

[0033] Step 10: Prepare for glue injection; Specifically, it includes the following steps: S1 Electrical pre-classification; S2 Hi-rel; This step is used to test the product's operating environment under high temperature and high pressure conditions. The operating environment is in insulating oil at an ambient temperature of 175℃, and the voltage applied to the product is not less than 10. 4 V.

[0034] Specifically: The products prepared for adhesive injection were inspected. Nineteen pre-tested and qualified products were taken for testing, yielding 76 test data points (19*4). The tests included: first, TC high and low temperature cycling, with experimental conditions of VR@IR=5.0uA, IR@VR=11000V, and test environments of (175℃~190℃) / 15mins, 25℃ / 5mins, and (-65℃~-75℃) / 15mins. Next, high-temperature and high-pressure performance testing was performed, with experimental conditions of pressurizing the product in insulating oil at 175℃ for 10 minutes. 4 V, the pressurization time is 168 hours. After that, the experimental product is cooled for 2 hours before the product results are tested.

[0035] Test data is detailed in Table 1: Table 1 Step 11: Applying adhesive and curing after application; Specifically: 1. Place the sintered glass workpiece into the mold and inject adhesive. During the adhesive injection process, ensure that the copper electrode is exposed outside the adhesive injection area. 2. The adhesive injection area includes solder pads, molybdenum particles, grains, molybdenum particles, and solder pads; Step 12: Surface tin treatment; including the following steps: P1 Copper electrode pretreatment; P2 checks the tinning parameters; P3 Loading; P4 Soldering tray installation; P5 Tin Dipping; P6 Cooling; P7 is the other end that is immersed in tin; P8 Material feeding; P9 cleaning machine preparation; Clean with P10 cleaning agent; P11 Drying; P12 Sorting of products with defective appearance; P13 Packing.

[0036] Step Thirteen: Second Reliability Test; Further testing of the finished rectifier. Before and after the second reliability test, the laboratory will also conduct semi-automatic electrical tests.

[0037] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high-voltage rectifier manufacturing process, characterized in that, Includes the following steps: Step 1: Prepare the materials and load the large silicon wafer into the welding mold; Step two involves entering the furnace and welding at high temperature under nitrogen protection; Step 3: Wire cutting; the large silicon wafers welded together are wire cut into a circle, and the grains are cleaned; Step 4: Raw material loading, in the following order: loading the first two copper electrodes, loading the first four welding pieces, loading the first four molybdenum granules, loading the four cleaned grains, loading the second four molybdenum granules, loading the second four welding pieces, and loading the second two copper electrodes, all evenly and orderly loaded into the cut welding mold; the first two copper electrodes and the second two copper electrodes are arranged perpendicularly. Step 5: Press down the heavy hammer, put it into the welding furnace, and weld at high temperature under nitrogen protection; Step six: Out of the oven and transfer; Step 7: Pickling and ultrasonic cleaning with water; use a pickling machine to acidically etch the PN junction surface of the grains in the welded product to remove possible contaminants. During the pickling process, perform ultrasonic cleaning with high-purity water according to the procedure. Step 8: Coat the cleaned workpiece with glass slurry and place it in a sintering furnace under nitrogen protection for glass sintering. Step Nine: Reliability Testing; Before and after the reliability testing, the laboratory shall conduct semi-automatic electrical testing. Step 10: Prepare for glue injection; Step 11: Applying adhesive and curing after application; Step 12: Surface tin treatment; Step Thirteen: Second Reliability Test; Before and after reliability testing, the laboratory must conduct semi-automatic electrical tests; Step Fourteen: Electrical Testing; Fully automated electrical testing is performed on the production line. Step 15: Printing and visual inspection; Step sixteen: Pack and store.

2. The high-voltage rectifier manufacturing process according to claim 1, characterized in that: The maximum temperature inside the welding furnace in step five is 715℃~760℃. The time spent in the constant temperature zone above 660℃ is 11~17 minutes, and the time spent in the constant temperature zone above 580℃ is 17~21 minutes. The furnace outlet temperature is ≤130℃. The pressure of the nitrogen gas is 2.5±0.5kg / cm³. 2 .

3. The high-voltage rectifier manufacturing process according to claim 2, characterized in that: The pickling machine mentioned in step seven includes an acid tank #1 and an acid tank #2. The acid tank #1 is filled with mixed acid #1, and the acid tank #2 is filled with mixed acid #2. The ratio of mixed acid #1 is nitric acid: sulfuric acid: hydrofluoric acid: phosphoric acid = 1:2:1:2; the ratio of mixed acid #2 is phosphoric acid: hydrogen peroxide: deionized water = 1:2:

3.

4. The high-voltage rectifier manufacturing process according to claim 3, characterized in that: The actual acid temperature of the No. 1 mixed acid is 25℃~28℃, and the actual acid temperature of the No. 2 mixed acid is 62℃±3℃.

5. The high-voltage rectifier manufacturing process according to claim 4, characterized in that: In step eight, the maximum temperature of the sintering furnace is 670℃±10℃. In the area above 630℃, the transit time is 6min~12min, the chain speed is 12.5cm / 60±2s, and the sintering temperature is 300℃-360℃.

6. The high-voltage rectifier manufacturing process according to claim 5, characterized in that: Step 10, the preparation for glue injection, includes the following steps: S1 Electrical pre-classification; S2 Hi-rel; The product undergoes high-temperature and high-pressure working environment testing. The working environment is in insulating oil at an ambient temperature of 175℃, and the applied voltage is not less than 10... 4 V.

7. The high-voltage rectifier manufacturing process according to claim 6, characterized in that: The glass slurry preparation ratio in step eight is: glass powder / high-purity deionized water = (450±1 g) / (175±5 ml).

8. The high-voltage rectifier manufacturing process according to claim 7, characterized in that: The surface tin treatment described in step twelve includes the following steps: P1 Copper electrode pretreatment; P2 checks the tinning parameters; P3 Loading; P4 Soldering tray installation; P5 Tin Dipping; P6 Cooling; P7 is the other end that is immersed in tin; P8 Material feeding; P9 cleaning machine preparation; Clean with P10 cleaning agent; P11 Drying; P12 Sorting of products with defective appearance; P13 Packing.

Citation Information

Patent Citations

  • A single-unit production process and a batch production process for a high-voltage silicon stack

    CN114551250B

  • Method for manufacturing fast-recovery glass package diode with ultra-high voltage above 13,000 V

    CN104377129A