A method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode

By electrodepositing a Zn-(Ni/FeOOH film on the surface of nickel foam, the problem of poor stability of FeOOH-based materials under high current density is solved, an efficient and robust redox catalyst is achieved, and the demand for industrial hydrogen production by electrolysis of water is achieved.

CN115896845BActive Publication Date: 2024-10-11SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210662044.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-13
Publication Date
2024-10-11
Estimated Expiration
2042-06-13

AI Technical Summary

Technical Problem

Existing FeOOH-based materials are difficult to maintain long-term stability at high current densities, resulting in a decline in catalytic performance and unable to meet the needs of industrial water electrolysis for hydrogen production.

Method used

A self-supporting zinc-doped nickel/iron oxyhydroxide catalytic electrode is used to prepare a Zn-(Ni/FeOOH film on the surface of nickel foam through electrodeposition method to improve the conductivity of the electrode and exposure of catalytic active sites, and reduce excessive Potential.

Benefits of technology

We have achieved a low-cost and large-area synthesis of an efficient and robust redox catalyst that can maintain long-term stability at high current densities, which is better than most precious metal-free electrocatalysts and shows the great potential of iron-based cheap resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115896845B_ABST
    Figure CN115896845B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode, which comprises the following raw materials and components: foamed nickel (NF), FeSO4·7H2O, ZnCl2, and the preparation thereof involves cutting the foamed nickel (0.5×0.5 cm 2 ) was used as the working electrode, and a platinum sheet (1×1cm 2 ) and Ag / AgCl (3.5M KCl) were used as the counter electrode and reference electrode respectively; FeSO4·7H2O (1.39 g) and ZnCl2 (0.03 g) were dissolved in 50 mL of aqueous solution to prepare an electrolyte, and the three electrodes in step 2 were placed in the electrolyte. At room temperature of 25°C, after electroplating at a voltage of 1.3 V for 500 s, the target sample (zinc-doped nickel / iron oxyhydroxide film, Zn‑(Ni / FeOOH)) was electroplated on the surface of the original nickel foam. 2+ The modification of Ni / FeOOH and the superhydrophilic / superaerophobic properties of the electrode surface enable the catalytic electrode obtained by the present invention to exhibit ultrahigh OER activity and excellent long-term stability at high current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field related to electrochemical catalytic materials, and in particular to a method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode. Background Art

[0002] The use of water electrolysis technology to produce green hydrogen can effectively address the energy and environmental crisis caused by the massive consumption of fossil fuels. However, the large-scale application of water electrolysis technology is still limited by high energy consumption and high cost. In particular, the oxygen evolution reaction (OER), as one of the half-reactions of water electrolysis technology, has slow kinetics, which seriously hinders the efficiency of hydrogen production and is considered to be a key bottleneck in the development of water electrolysis technology. Although a large number of researchers are committed to developing efficient and inexpensive non-precious metal-based catalysts for efficient oxygen evolution, it is still difficult to meet the requirements of industrial water electrolysis. At 1000mA cm -2 It can work stably for at least 100 hours at high current density; therefore, the development of non-precious metal catalysts with excellent activity and ultra-high stability at high current density is of great significance for promoting the large-scale electrolysis of water to produce hydrogen.

[0003] Iron (Fe)-based materials, especially FeOOH, have attracted great attention as promising OER catalysts due to their abundant reserves, low price and environmental friendliness. In addition, the intrinsic activity of FeOOH in OER is higher than that of NiOOH and CoOOH. However, the poor electrical conductivity of FeOOH makes its OER performance far from satisfactory. Therefore, it is still a severe challenge to improve the catalytic performance and long-term stability of FeOOH-based materials to meet industrial needs. The following strategies have been developed to regulate FeOOH into advanced electrocatalysts: (1) by combining with conductive materials (e.g., Co, CeO 2 ) or conductive substrates (e.g. nickel foam) to improve the charge transport capacity of FeOOH-based nanomaterials; (2) regulating the electronic structure of FeOOH by doping to improve its OER activity; (3) designing a hierarchical structure based on FeOOH to increase the number of active sites and fully expose the active sites, thereby improving its catalytic performance.

[0004] However, although the existing technology improves the catalytic activity and stability of FeOOH-based materials, it is difficult to work stably in an environment with high current density. This is because at high current density (e.g. ≥1000mA cm-2), a large number of bubbles will quickly form on the electrode surface, which will hinder the exposure of active sites and charge / mass transfer, resulting in an increase in overpotential. In addition, the strong interaction between the bubbles and the catalyst surface produces mechanical stress and violent vibration on the electrode, causing the active material to detach from the conductive substrate and the active catalyst to dissolve. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode to solve the problem that the prior art proposed in the above background technology improves the catalytic performance of FeOOH-based materials but is difficult to maintain long-term stability in a high current density environment.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode, comprising the following raw materials and components: nickel foam (NF), FeSO 4 7H 2 O, ZnCl 2 , characterized in that: cutting nickel foam (0.5×0.5cm 2 ) was used as the working electrode, and a platinum sheet (1×1cm 2 ) and Ag / AgCl (3.5 M KCl) were used as the counter electrode and reference electrode, respectively; the electrolyte was FeSO 4 7H 2 O (1.39 g) and ZnCl 2 (0.02g, 0.03g, 0.05g) were dissolved in 50mL of aqueous solution.

[0007] As a further technical solution, the working electrode NF (0.5×0.5 cm 2 ) Before use, it needs to be ultrasonically cleaned with HCl solution (2 mol / L), ethanol and water for 10 min respectively.

[0008] As a further technical solution, the three electrodes are placed in an electrolyte, and after electroplating for 500 seconds at a voltage of 1.3 V at a room temperature of 25° C., the target sample is electroplated on the surface of the original nickel foam.

[0009] A method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode comprises the following steps:

[0010] Step 1: The nickel foam (NF) was ultrasonically cleaned with HCl solution (2 mol / L), ethanol and water for 10 min respectively;

[0011] Step 2: Cut NF (0.5×0.5cm 2 ) was used as the working electrode, and a platinum sheet (1×1cm 2 ) and Ag / AgCl (3.5MKCl) were used as counter electrode and reference electrode, respectively;

[0012] Step 3: Add FeSO 4 7H 2 O (1.39 g) and ZnCl 2(0.02g, 0.03g, 0.05g) were dissolved in 50mL aqueous solution to prepare electrolyte, and the three electrodes in step 2 were placed in the electrolyte. After electroplating at a voltage of 1.3V for 500s at room temperature of 25°C, the target sample was electroplated on the surface of the original nickel foam.

[0013] Step 4: Wash the electrode surface with ultrapure water and dry it in an oven at 60°C for testing.

[0014] As a further technical solution, in step 3, 1.39 g FeSO 4 7H 2 O (1.39 g) and ZnCl 2 (0.03 g) was dissolved in 50 mL of aqueous solution to prepare the electrolyte. The Zn-(Ni / FeOOH) film was successfully coated on the NF (0.5×0.5 cm 2 ) surface to obtain Zn-(Ni / FeOOH)@NF electrode.

[0015] As a further technical solution, in step 2, when the preparation area is 40 cm 2 The large-size electrode, NF was cut into 4×10 cm 2 As the working electrode; the counter electrode is 3×3cm 2 Platinum electrode, reference electrode uses Ag / AgCl (3.5MKCl) electrode, FeSO 4 7H 2 O (11.12 g) and ZnCl 2 (0.24 g) was dissolved in 400 mL of water to prepare the electrolyte, and then electrodeposited at 1.3 V and 25 °C for 500 s to obtain a 40 cm 2 Zn-(Ni / FeOOH)@NF.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. Low-cost and large-scale synthesis methods can transform commercial nickel foam and cheap iron-based resources into efficient and robust OER catalysts; thanks to Zn 2+ Simultaneous modification on Ni / FeOOH, Zn-(Ni / FeOOH)@NF has hydrophilic / aerophobic surface, high conductivity, and abundant catalytic active sites;

[0018] 2. The Zn-(Ni / FeOOH)@NF electrode only needs low overpotentials of 302, 330, and 347 mV to drive 400, 1000, and 1500 mA cm -2The current density of Zn-(Ni / FeOOH)@NF was 400 mA cm -2 It shows the smallest overpotential and the longest stability under the condition;

[0019] 3. Zn-(Ni / FeOOH)@NF at 1000mA cm -2 The catalytic performance at high current density is also better than most noble metal-free electrocatalysts, second only to Ni 0.8 Fe 0.2 -AHNAs, Ni-Fe-W LDH / NF and Fe,Co,Ni-based ternary metal MOFs ( Figure 6 ). And Zn-(Ni / FeOOH)@NF at 1000mA cm -2 It exhibits the best stability for 1000 h, outperforming all NF self-supported non-precious metal electrocatalysts;

[0020] 4. The invented Zn-(Ni / FeOOH)@NF electrode can be prepared on a large area and directly applied to OER, with an area of ​​40 cm 2 The constructed electrodes only require 285 and 405 mV to drive 1000 and 3000 mA oxygen evolution currents, respectively; demonstrating the great potential of using iron-based, cheap and abundant natural resources as industrial oxygen evolution catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the synthesis and characterization of the Zn-(Ni / FeOOH)@NF catalyst of the present invention;

[0022] Figure 2 The scanning electron microscope image, X-ray energy dispersion spectrum and transmission electron microscope characterization schematic diagram of the Ni / FeOOH@NF structure of the present invention are shown;

[0023] Figure 3 The scanning electron microscope image, X-ray energy dispersion spectrum and transmission electron microscope characterization schematic diagram of the NiZn@NF structure of the present invention are shown;

[0024] Figure 4 Schematic diagram of the polarization curve of the Zn-(Ni / FeOOH)@NF electrode of the present invention and the working photos before and during the LSV test;

[0025] Figure 5 All FeOOH-based electrocatalysts with the structure of the present invention can be used at high current density (≥400 mA cm -2 ) under OER performance comparison diagram;

[0026] Figure 6 Schematic diagram of the comparison of OER performance of non-precious metal electrocatalysts of the structure of the present invention under alkaline conditions. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Specific implementation method 1, see Figure 1-6 The present invention provides a technical solution: a method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode, comprising the following raw materials and components: nickel foam (NF), FeSO 4 7H 2 O, ZnCl 2 The preparation characteristics are as follows: the electrode is prepared by an electrodeposition method, involving three electrodes and an electrolyte, and the three electrodes are a working electrode, a counter electrode and a reference electrode, wherein the working electrode is NF (0.5×0.5cm 2 ), the counter electrode is a platinum sheet (1×1cm 2 ), the reference comparison uses Ag / AgCl (3.5M KCl), and the electrolyte is FeSO 4 7H 2 O (1.39 g) and ZnCl 2 (0.02g, 0.03g, 0.05g) were dissolved in 50mL of aqueous solution.

[0029] A method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode comprises the following steps: Step 1: ultrasonically clean nickel foam (NF) with HCl solution (2 mol / L), ethanol and water for 10 min respectively; Step 2: cut NF (0.5×0.5 cm 2 ) was used as the working electrode, and a platinum sheet (1×1cm 2 ) and Ag / AgCl (3.5M KCl) as the counter electrode and reference electrode respectively; Step 3: FeSO 4 7H 2 O (1.39 g) and ZnCl 2 (0.02g, 0.03g, 0.05g) are dissolved in 50mL aqueous solution to prepare an electrolyte, and the three electrodes in step 2 are placed in the electrolyte. At room temperature of 25°C, after electroplating at a voltage of 1.3V for 500s, the target sample will be electroplated on the surface of the original nickel foam; Step 4: Wash the electrode surface with ultrapure water and place it in an oven at 60°C to dry it for testing.

[0030] In this example, 1.39 g FeSO4 7H 2 O (1.39 g) and ZnCl 2 (0.03 g) was dissolved in 50 mL of aqueous solution to prepare the electrolyte. The Zn-(Ni / FeOOH) film was successfully coated on the NF (0.5×0.5 cm 2 ) surface to obtain Zn-(Ni / FeOOH)@NF electrode.

[0031] Specifically, the present invention can adopt a low-cost and large-scale synthesis preparation method to convert commercial nickel foam and cheap iron-based resources into efficient and robust OER catalytic electrodes; the excellent catalytic performance is due to the Zn 2+ The modification of Ni / FeOOH, super hydrophilic / super aerophobic surface characteristics, high conductivity, abundant catalytic active sites and other factors. Specifically, the Zn-(Ni / FeOOH)@NF electrode of the present invention only needs a low overpotential of 302, 330, and 347 mV to drive 400, 1000, and 1500 mA cm -2 The current density of Zn-(Ni / FeOOH)@NF was 400 mA cm -2 It exhibits the smallest overpotential and the longest stability.

[0032] In the present invention, Zn-(Ni / FeOOH)@NF is 1000mA cm -2 The catalytic performance at high current density is also better than most noble metal-free electrocatalysts, second only to Ni 0.8 Fe 0.2 -AHNAs, Ni-Fe-W LDH / NF and Fe,Co,Ni-based ternary metal MOFs ( Figure 6 ). And Zn-(Ni / FeOOH)@NF at 1000mA cm -2 It exhibits the best stability for 1000 h, outperforming all NF self-supported non-precious metal electrocatalysts.

[0033] In this embodiment, when the preparation area is 40cm 2 The large-size electrode, NF was cut into 4×10 cm 2 As the working electrode; the counter electrode is 3×3cm 2 Platinum electrode, reference electrode Ag / AgCl (3.5M KCl) electrode, FeSO 4 7H 2 O (11.12 g) and ZnCl 2 (0.24 g) was dissolved in 400 mL of water to prepare the electrolyte, and then electrodeposited at 1.3 V and 25 °C for 500 s to obtain a 40 cm2 Zn-(Ni / FeOOH)@NF.

[0034] Specifically, the Zn-(Ni / FeOOH)@NF electrode created by the present invention can be prepared on a large scale and directly applied to OER, with an area of ​​40 cm 2 The constructed electrodes only require 285 and 405 mV to drive 1000 and 3000 mA oxygen evolution currents; showing the great potential of using iron-based cheap and abundant natural resources as electrochemical industrial catalysts

[0035] Example 1: 1.39 g FeSO 4 7H 2 O (1.39 g) and ZnCl 2 (0.03 g) was dissolved in 50 mL of aqueous solution to prepare the electrolyte. The Zn-(Ni / FeOOH) film was successfully coated on the NF (0.5×0.5 cm 2 ) surface, and the Zn-(Ni / FeOOH)@NF electrode was prepared as follows; Figure 1 shown.

[0036] Figure 1 Synthesis and characterization of Zn-(Ni / FeOOH)@NF catalyst; (a) Schematic diagram of the one-step synthesis process; (b, c) SEM images of Zn-(Ni / FeOOH)@NF at different magnifications; (d) SEM image used to reveal the thickness of Zn-(Ni / FeOOH) film; (e) TEM image of Zn-(Ni / FeOOH)@NF; (f, g) high-resolution TEM images and (h) X-ray energy dispersion spectrum.

[0037] Example 2: 1.39 g FeSO 4 7H 2 O was dissolved in 50 mL of aqueous solution to prepare the electrolyte; the FeOOH film modified by Ni nanoparticles was successfully coated on NF (0.5×0.5 cm) at room temperature of 25°C and a voltage of 1.3 V for 500 s. 2 ) surface, and the Ni / FeOOH@NF electrode was prepared as follows; Figure 2 shown.

[0038] Figure 2 (a, b) scanning electron microscope images, (c, e) X-ray energy dispersion spectra, and (d) transmission electron microscope characterization of Ni / FeOOH@NF.

[0039] Example 3: 0.03g ZnCl 2The electrolyte was prepared by dissolving in 50 mL of aqueous solution. The NiZn nanoparticles were successfully modified on NF (0.5×0.5 cm) by electroplating at 1.3 V for 500 s at room temperature of 25°C. 2 ) surface to obtain a NiZn / NF electrode; as follows Figure 3 shown.

[0040] Figure 3 (a, b) scanning electron microscope images, (c, e) X-ray energy dispersion spectra, and (d) transmission electron microscope characterization of NiZn@NF.

[0041] Example 4: Preparation of large-area Zn-(Ni / FeOOH)@NF; when the preparation area is 1×2, 1×3, 2×3 cm 2 The preparation conditions of the electrode are the same as those in Example 1. When the preparation area is 40 cm 2 The large-size electrode, NF was cut into 4×10 cm 2 As the working electrode, the counter electrode is 3×3 cm 2 Platinum electrode, reference electrode uses Ag / AgCl (3.5M KCl) electrode. FeSO 4 7H 2 O (11.12 g) and ZnCl 2 (0.24 g) was dissolved in 400 mL of water to prepare the electrolyte, and then electrodeposited at 1.3 V and 25 °C for 500 s to obtain a 40 cm 2 All electrodes were directly used for electrochemical performance tests after drying; Figure 4 shown.

[0042] Figure 4 The area of ​​(a) is 2, 3, 6 and 40 cm 2 (a) The polarization curves of Zn-(Ni / FeOOH)@NF electrodes; (b) The overpotentials of Zn-(Ni / FeOOH)@NF electrodes of different sizes at currents of 500, 1000, 1500, 2000, 2500, and 3000 mA; the areas are 2, 3, 6, and 40 cm, respectively. 2 (c) Nyquist plot and (d) R of Zn-(Ni / FeOOH)@NF recorded at 0.6 V (vs. Hg / HgO) s / R ct ; (e, f) area is 40cm 2 Working photos of the Zn-(Ni / FeOOH)@NF electrode before and during the LSV test in the current density range of 0-3000mA.

[0043] Figure 5The results show that the FeOOH-based electrocatalysts have good performance at high current density (≥400 mA cm -2 ) under OER performance comparison;

[0044] Figure 6 Comparison of the OER performance of non-precious metal electrocatalysts under alkaline conditions.

[0045] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode, characterized in that: It includes the following raw materials and components: nickel foam, FeSO4·7H2O and ZnCl 2, The preparation steps include: Step 1: Clean the nickel foam; Step 2: Cut 0.5×0.5cm 2 The nickel foam was used as the working electrode, and 1×1 cm 2 Pt sheet and 3.5 M KCl in Ag / AgCl were used as counter electrode and reference electrode, respectively; Step 3: 1.39 g of FeSO4·7H2O and 0.02 g, 0.03 g or 0.05 g of ZnCl2 are dissolved in 50 mL of aqueous solution to prepare an electrolyte, and the three electrodes in step 2 are placed in the electrolyte. After electrodeposition at a voltage of 1.3 V for 500 s at room temperature of 25°C, the target sample will be electrodeposited on the surface of the original nickel foam. Step 4: Wash the electrode surface with ultrapure water and dry it in an oven at 60°C for testing, thereby obtaining a Zn-(Ni / FeOOH)@NF electrode.

2. The method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode according to claim 1, characterized in that: In the step 1, the nickel foam needs to be ultrasonically cleaned with HCl solution, ethanol and water for 10 minutes respectively before use.

3. A method for preparing a self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode, characterized in that: This method is used to prepare a 40cm 2 A large-size self-supporting zinc-doped nickel / iron oxyhydroxide catalytic electrode is prepared, and the preparation method includes the following raw materials and components: nickel foam, FeSO4·7H2O and ZnCl 2, The preparation steps include: Step 1: Clean the nickel foam; Step 2: Cut 4×10cm 2 Nickel foam was used as the working electrode, and 3×3 cm 2 Pt sheet and 3.5 M KCl in Ag / AgCl were used as counter electrode and reference electrode, respectively; Step 3: 11.12 g of FeSO4·7H2O and 0.24 g of ZnCl2 were dissolved in 400 mL of aqueous solution to prepare an electrolyte, and the three electrodes in step 2 were placed in the electrolyte. After electroplating at a voltage of 1.3 V for 500 s at room temperature of 25°C, the target sample was electroplated on the surface of the original nickel foam. Step 4: Wash the electrode surface with ultrapure water and place it in an oven at 60°C to dry it for testing. 2 Zn-(Ni / FeOOH)@NF electrode.

Citation Information

Patent Citations

  • Ferronickle-based phosphide electro-catalytic material as well as preparation method and application thereof

    CN113684501A

  • Multi-metal hydroxide pre-catalyst as well as preparation method and application thereof

    CN113943950A

  • Self-source etching preparation method and application of nickel-doped iron oxyhydroxide self-supporting electrode material

    CN114277400A